Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode

By introducing structures such as SiO₂ patterned layers and ScAlN buffer layers into AlGaN-based ultraviolet LED epitaxial wafers and optimizing growth conditions, the problem of poor crystal quality in AlGaN-based ultraviolet LED epitaxial wafers was solved, and the luminous efficiency was improved.

CN117153977BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311319185.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2026-11-24
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

The poor crystal quality of AlGaN-based ultraviolet LED epitaxial wafers results in low luminous efficiency, which is difficult to improve effectively with existing technologies.

Method used

A composite structure consisting of a SiO₂ patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer was adopted. The crystal was grown using methods such as PECVD and MOCVD, and the composition and thickness of each layer were controlled to optimize the growth conditions and improve the crystal quality.

Benefits of technology

It effectively reduces defect density, minimizes lattice mismatch, improves the luminous efficiency of light-emitting diodes, avoids thermal stress accumulation and thin film cracking, and enhances crystal quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117153977B_ABST
    Figure CN117153977B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode (LED) epitaxial wafer and its fabrication method, and the LED itself, relating to the field of semiconductor optoelectronic devices. The LED epitaxial wafer includes a substrate and a composite layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer sequentially disposed on the substrate. The composite layer includes a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially. The SiO2 patterned layer includes multiple SiO2 patterns arrayed on the substrate. Implementing this invention can improve the luminous efficiency of the LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology

[0002] Group III nitride semiconductor materials, such as GaN, InGaN, and AlGaN, can theoretically be used to fabricate light-emitting diodes (LEDs) and laser diodes (LDs) with a spectral range from infrared to ultraviolet light. Group III nitride-based ultraviolet and ultraviolet LEDs have broad application prospects in fields such as hygiene disinfection, UV curing, photolithography, anti-counterfeiting detection, medical diagnosis, and water purification due to their advantages including non-toxicity, ozone-free operation, fast switching speed, narrow spectral density, and long lifespan. Ultraviolet LEDs primarily use AlGaN as the growth material. Compared to GaN, AlGaN is much more difficult to grow because Al atoms have a higher adhesion coefficient and lower surface mobility, making it difficult for them to obtain sufficient energy to move to suitable lattice positions. This results in three-dimensional island-like growth, leading to the formation of different nucleation sites during AlGaN growth. These nucleation sites grow into islands and merge, resulting in a very high defect density (such as dislocations and interface defects) in the grown AlGaN material. This leads to poor crystal quality of AlGaN-based LED epitaxial wafers and low LED luminous efficiency. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode.

[0004] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.

[0005] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate and a composite layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer sequentially disposed on the substrate; the composite layer comprises a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially.

[0006] The SiO2 patterned layer comprises multiple SiO2 patterns arrayed on the substrate.

[0007] As an improvement to the above technical solution, the SiO2 patterned layer is obtained by ICP etching of a SiO2 thin film layer, wherein the thickness of the SiO2 thin film layer is 10nm-100nm, and the distribution density of the SiO2 pattern is 1×10⁻⁶. 6 pcs / cm 2 -1×108 pcs / cm 2 .

[0008] As an improvement to the above technical solution, the proportion of Sc component in the ScAlN buffer layer is 0.01-0.5.

[0009] The proportion of B component in the BGaN island nucleation layer is 0.01-0.4%;

[0010] The proportion of Al component in the three-dimensional BAlGaN layer is 0.01-0.7, and the proportion of B component is 0.1-0.7.

[0011] The proportion of Al component in the two-dimensional AlGaN merging layer is 0.2-0.7%.

[0012] As an improvement to the above technical solution, the thickness of the ScAlN buffer layer is 10nm-100nm;

[0013] The thickness of the BGaN island-shaped nucleation layer is 0.1 μm-1 μm;

[0014] The thickness of the three-dimensional BAlGaN layer is 0.5μm-5μm;

[0015] The thickness of the two-dimensional AlGaN merging layer is 0.5μm-5μm.

[0016] As an improvement to the above technical solution, along the epitaxial growth direction, the proportion of Sc component in the ScAlN buffer layer gradually increases from 0.01-0.1 to 0.2-0.5.

[0017] As an improvement to the above technical solution, along the epitaxial growth direction, the proportion of Al component in the three-dimensional BAlGaN layer gradually increases from 0.01-0.1 to 0.2-0.7, and the proportion of B component gradually decreases from 0.5-0.7 to 0.01-0.1.

[0018] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:

[0019] A substrate is provided on which a composite layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer are sequentially grown; the composite layer comprises a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially.

[0020] The SiO2 patterned layer comprises multiple SiO2 patterns arrayed on the substrate.

[0021] As an improvement to the above technical solution, a SiO2 thin film layer is deposited in the PECVD reaction chamber, wherein the deposition temperature of the SiO2 thin film is 250℃-300℃;

[0022] The SiO2 thin film layer is then etched by ICP to obtain the SiO2 patterned layer. The etching time is 10 min to 20 min. The etching gas is a mixture of Cl2 and BCl3, wherein the volume ratio of Cl2 to BCl3 is 10:1 to 10:2.

[0023] As an improvement to the above technical solution, the growth temperature of the ScAlN buffer layer is 700℃-1000℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2 and NH3, wherein the volume ratio of N2 to NH3 is 1:1-1:10.

[0024] The growth temperature of the BGaN island nucleation layer is 900℃-1100℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1 to 1:10:10.

[0025] The growth temperature of the three-dimensional BAlGaN layer is 1000℃-1200℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1-1:10:10.

[0026] The growth temperature of the two-dimensional AlGaN merging layer is 1100℃-1300℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1 to 1:10:10.

[0027] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.

[0028] Implementing this invention has the following beneficial effects:

[0029] 1. In the epitaxial wafer of the light-emitting diode of the present invention, the composite layer comprises a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially. First, the SiO2 patterned layer ensures that the subsequently grown three-dimensional BAlGaN layer and two-dimensional AlGaN merging layer can only grow within designated patterned regions, each patterned region being independent of the others, thereby avoiding the accumulation of thermal stress during growth and achieving stress separation and preventing film cracking. Second, the composite layer includes a ScAlN buffer layer. First, the ScAlN buffer layer prevents NH3 from reacting with the substrate and diffusing into the subsequently grown three-dimensional BAlGaN layer and two-dimensional AlGaN merging layer, thus preventing a decrease in crystal quality. Second, the ScAlN buffer layer provides a flat nucleation surface for the subsequently grown BGaN island nucleation layer, reducing the contact angle of the BGaN island nucleation layer growth and improving crystal quality. Third, the BGaN… The higher mobility of boron atoms in the island-like nucleation layer compared to al atoms avoids the problem of al atoms' low mobility failing to gain sufficient energy to move to suitable lattice positions on the surface, resulting in uniform nucleation sites in the BGaN island-like nucleation layer and reducing defect density. Fourth, the three-dimensional BAlGaN layer prevents nucleation sites from prematurely fusing to form penetrating dislocations, thus reducing crystal quality. Fifth, the two-dimensional AlGaN merging layer can fill the three-dimensional BAlGaN layer, forming a flat surface before depositing the N-type AlGaN layer, improving the crystal quality of the subsequently grown N-type AlGaN layer. Furthermore, the two-dimensional AlGaN merging layer allows compressive stress to be released through stacking faults, reducing line defects, improving crystal quality, and increasing diode luminous efficiency.

[0030] 2. In the epitaxial wafer of the light-emitting diode of the present invention, the proportion of Sc component in the ScAlN buffer layer gradually increases along the epitaxial growth direction. Since Sc atoms are comparable to Ga atoms, the gradual increase in the proportion of Sc component can reduce lattice mismatch with the BGaN island nucleation layer, improve crystal quality, and increase luminous efficiency.

[0031] 3. In the epitaxial wafer of the light-emitting diode of the present invention, along the epitaxial growth direction, the proportion of Al component in the three-dimensional BAlGaN layer gradually increases and the proportion of B component gradually decreases, which can reduce the lattice mismatch between BGaN island nucleation and two-dimensional AlGaN merging layer, improve crystal quality, and improve luminous efficiency. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;

[0033] Figure 2 This is a schematic diagram of the composite layer structure in one embodiment of the present invention;

[0034] Figure 3This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0036] refer to Figures 1-2 The present invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1 and a composite layer 2, an N-type AlGaN layer 3, a multiple quantum well layer 4, an electron blocking layer 5, a P-type AlGaN layer 6, and a P-type contact layer 7 sequentially disposed on the substrate 1; wherein, the composite layer 2 comprises a SiO2 patterned layer 21, a ScAlN buffer layer 22, a BGaN island nucleation layer 23, a three-dimensional BAlGaN layer 24, and a two-dimensional AlGaN merging layer 25 sequentially stacked. First, the SiO2 patterning layer 21 ensures that the subsequently grown three-dimensional BAlGaN layer 24 and two-dimensional AlGaN merging layer 25 can only grow within designated patterned regions, each region being independent of the others. This avoids the accumulation of thermal stress during growth, achieving stress separation and preventing film cracking. Second, the composite layer 2 includes a ScAlN buffer layer 22. Firstly, the ScAlN buffer layer 22 prevents NH3 from reacting with the substrate 1 and diffusing into the subsequently grown three-dimensional BAlGaN layer 24 and two-dimensional AlGaN merging layer 25, thus preventing a decrease in crystal quality. Secondly, the ScAlN buffer layer 22 provides a flat nucleation surface for the subsequently grown BGaN island nucleation layer 23, reducing the contact angle of the BGaN island nucleation layer 23 and improving crystal quality. Thirdly... The B atoms in the BGaN island nucleation layer 23 have a higher mobility than Al atoms, which avoids the problem that Al atoms cannot acquire enough energy to move to the appropriate lattice position on the surface due to their lower mobility. This allows the BGaN island nucleation layer 23 to form uniform nucleation sites and reduce defect density. Fourth, the three-dimensional BAlGaN layer 24 can prevent the nucleation sites from fusing prematurely and forming through dislocations, thus reducing crystal quality. Fifth, the two-dimensional AlGaN merging layer 25 can fill the three-dimensional BAlGaN layer 24, forming a flat surface before depositing the N-type AlGaN layer 3, improving the crystal quality of the subsequently grown N-type AlGaN layer 3. Furthermore, the two-dimensional AlGaN merging layer 25 can release compressive stress through stacking faults, reducing line defects, improving crystal quality, and increasing diode luminous efficiency.

[0037] Specifically, the SiO2 pattern layer 21 is obtained by ICP etching or RIE etching of a SiO2 thin film layer, preferably by ICP etching. The thickness of the SiO2 thin film layer is 10nm-100nm. If the thickness is greater than 100nm, the etching process becomes more difficult; if the thickness is less than 10nm, it is difficult to obtain a SiO2 pattern with good consistency. For example, the thickness of the SiO2 thin film layer can be 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, or 90nm, but is not limited to these.

[0038] Specifically, multiple arrays of SiO2 patterns are formed on substrate 1 by etching. The cross-sections of these patterns are rectangular, square, triangular, circular, or semi-circular, but not limited to these. Preferably, in one embodiment of the invention, the cross-section of the SiO2 islands is triangular. Specifically, the distribution density of the SiO2 patterns is 5 × 10⁻⁶. 5 pcs / cm 2 -5×10 8 pcs / cm 2 Within this range, the SiO2 pattern distribution density can effectively achieve stress separation and prevent film cracking. Preferably, the SiO2 pattern distribution density is 1×10⁻⁶. 6 pcs / cm 2 -1×10 8 pcs / cm 2 An example is 4×10 6 pcs / cm 2 8×10 6 pcs / cm 2 1×10 7 pcs / cm 2 4×10 7 pcs / cm 2 Or 8×10 7 pcs / cm 2 However, it is not limited to this.

[0039] Specifically, the proportion of Sc component in the ScAlN buffer layer 22 is 0.01-0.55. Within this range, the Sc component can achieve a better transition effect and reduce lattice mismatch with the BGaN island nucleation layer 23. Preferably, the proportion of Sc component is 0.01-0.5%, with exemplary values ​​being 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, or 0.45, but not limited to these. Preferably, in one embodiment of the present invention, the proportion of Sc component gradually increases from 0.01-0.1 to 0.2-0.5 along the epitaxial growth direction. Based on this setting, lattice mismatch with the BGaN island nucleation layer 23 can be reduced, improving crystal quality and luminous efficiency.

[0040] Specifically, the thickness of the ScAlN buffer layer 22 is 8nm-110nm. If its thickness is <8nm, it is difficult to form a smooth nucleation surface; if its thickness is >110nm, the fabrication efficiency is too low and the cost of the epitaxial wafer is high. Preferably, the thickness of the ScAlN buffer layer 22 is 10nm-100nm, with exemplary thicknesses of 20nm, 20nm, 40nm, 50nm, 55nm, 60nm, 70nm, 80nm, or 90nm, but not limited to these.

[0041] Specifically, the proportion of boron (B) in the BGaN island nucleation layer 23 is 0.005-0.45. If the proportion of B is less than 0.005, it is difficult to form uniform nucleation sites; if the proportion of B is greater than 0.45, the crystal quality will be reduced. Preferably, the proportion of B is 0.01-0.4%, such as 0.1, 0.15, 0.2, 0.25, 0.3, or 0.35, but is not limited thereto.

[0042] Specifically, the thickness of the BGaN island nucleation layer 23 is 0.1 μm-2 μm. Within this thickness range, uniform nucleation sites can be formed, reducing defects. Preferably, the thickness of the BGaN island nucleation layer 23 is 0.1 μm-1 μm, with exemplary values ​​of 0.2 μm, 0.4 μm, 0.5 μm, 0.6 μm, or 0.8 μm, but it is not limited to these values.

[0043] Specifically, the proportion of Al component in the three-dimensional BAlGaN layer 24 is 0.005-0.75, and the proportion of B component is 0.005-0.75. This range of Al and B component proportions reduces lattice mismatch between the BGaN island nucleation 23 and the two-dimensional AlGaN merging layer 25. Preferably, the proportion of Al component is 0.01-0.7, and the proportion of B component is 0.1-0.7, exemplarily 0.1, 0.2, 0.3, 0.4, 0.5, or 0.6, but not limited thereto. More preferably, in one embodiment of the present invention, along the epitaxial growth direction, the proportion of Al component in the three-dimensional BAlGaN layer 24 gradually increases from 0.01-0.1 to 0.2-0.7, and the proportion of B component gradually decreases from 0.5-0.7 to 0.01-0.1. Based on this setting, lattice mismatch can be further reduced, crystal quality improved, and luminous efficiency increased.

[0044] Specifically, the thickness of the three-dimensional BaAlGaN layer 24 is 0.4μm-6μm. If the thickness is <0.4μm, it is difficult to form a three-dimensional structure and cannot effectively avoid the fusion of nucleation points; if the thickness is >6μm, it will increase defects. Preferably, the thickness is 0.5μm-5μm, and exemplary thicknesses are 1μm, 1.5μm, 2μm, 2.5μm, 3μm or 4μm, but it is not limited to these.

[0045] Specifically, the proportion of Al component in the two-dimensional AlGaN merging layer 25 is 0.15-0.75. If the proportion of Al component is <0.15, the three-dimensional BAlGaN layer 24 cannot be effectively filled; if the proportion of Al component is >0.75, the lattice quality will be reduced. Preferably, the proportion of Al component is 0.2-0.7, exemplarily 0.3, 0.4, 0.5 or 0.6, but not limited thereto.

[0046] Specifically, the thickness of the two-dimensional AlGaN merging layer 25 is 0.4 μm-6 μm. If the thickness is <0.40 μm, it is difficult to fill the three-dimensional BAlGaN layer 24; if the thickness is >6 μm, it will reduce the lattice quality. Preferably, the thickness is 0.5 μm-5 μm, and exemplary thicknesses are 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, or 4 μm, but it is not limited thereto.

[0047] The substrate 1 can be a sapphire substrate, a silicon substrate, or a silicon carbide substrate, but is not limited to these. A silicon substrate is preferred.

[0048] The doping element of the N-type AlGaN layer 3 is Si, but it is not limited to Si. The doping concentration of the N-type AlGaN layer 3 is 1×10⁻⁶. 19 cm -3 -5×10 20 cm -3 The thickness is 1μm-5μm.

[0049] Among them, the multiple quantum well layer 4 is an alternating stack of Al x Ga 1-x N quantum well layer and Al y Ga 1-y N-quantum barrier layers, with a stacking period of 3-15. A single Al x Ga 1-x The thickness of the N-quantum well layer is 2nm-5nm, and x is 0.2-0.6. A single Al y Ga 1-y The thickness of the N quantum barrier layer is 5nm-15nm, and the y value is 0.4-0.8.

[0050] Among them, the electron blocking layer 5 can effectively limit electron overflow and reduce hole obstruction, thereby improving the hole-to-electron-well injection efficiency, reducing carrier Auger recombination, and improving the luminous efficiency of the light-emitting diode. Specifically, the electron blocking layer 5 is Al. z Ga 1-z The number of layers is N, but not limited to this. Specifically, the thickness of electron blocking layer 5 is 10nm-100nm, and the z-axis is 0.4-0.8.

[0051] The doping element in the p-type AlGaN layer 6 is Mg, but it is not limited to this. The doping concentration of Mg in the p-type AlGaN layer 6 is 1×10⁶. 19 cm -3 -5×10 20 cm -3 The thickness of the p-type AlGaN layer 6 is 20nm-200nm.

[0052] Among them, the P-type contact layer 7 is a P-type GaN layer, and the P-type doping element is Mg, but not limited to this. The Mg doping concentration is 5 × 10⁻⁶. 19 cm -3 -5×10 20 cm -3 The thickness of the P-type contact layer 7 is 5nm-100nm.

[0053] Accordingly, refer to Figure 3 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned light-emitting diode epitaxial wafer, and includes the following steps:

[0054] S100: Provides a substrate;

[0055] S200: A composite layer is grown on the substrate;

[0056] Specifically, in one embodiment of the present invention, S200 includes:

[0057] S210: Growing a patterned SiO2 layer on a substrate;

[0058] Specifically, a SiO2 thin film layer is deposited in the PECVD reaction chamber at a deposition temperature of 250℃-300℃. Then, the SiO2 thin film layer is etched by ICP to obtain a SiO2 patterned layer for 10-20 minutes. The etching gas used is a mixture of Cl2 and BCl3, with a volume ratio of Cl2 to BCl3 of 10:1-10:2.

[0059] S220: A ScAlN buffer layer is grown on a SiO2 patterned layer;

[0060] Specifically, the ScAlN buffer layer can be grown using magnetron sputtering (PVD), molecular beam epitaxy (MBE), and metal-organic chemical vapor deposition (MOCVD), but is not limited to these methods. Preferably, in one embodiment of the present invention, the ScAlN buffer layer is grown using MOCVD at a growth temperature of 700℃-1000℃ and a growth pressure of 50 torr-500 torr. The gas used during growth is a mixture of N2 and NH3, wherein the volume ratio of N2 to NH3 is 1:1-1:10. NH3 is introduced as the N source, TMAl is introduced as the Al source, and Sc(TMHD)3 is introduced as the Sc source.

[0061] S230: BGaN island nucleation layer is grown on ScAlN buffer layer;

[0062] Specifically, BGaN island nucleation layers are grown in MOCVD at a temperature of 900℃-1100℃ and a pressure of 50 torr-500 torr. The gas used during growth is a mixture of N2, H2, and NH3, with a volume ratio of N2, H2, and NH3 of 1:1:1 to 1:10:10. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, B2H6 as the B source, and TMGa as the Ga source.

[0063] S240: Growth of a three-dimensional BAlGaN layer on a BGaN island nucleation layer;

[0064] Specifically, a three-dimensional BAlGaN layer was grown in MOCVD at a growth temperature of 1000℃-1200℃ and a growth pressure of 50 torr-500 torr. The gas used during growth was a mixture of N2, H2, and NH3, with a volume ratio of N2, H2, and NH3 of 1:1:1 to 1:10:10. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, B2H6 as the B source, TMAl as the Al source, and TMGa as the Ga source.

[0065] S250: A two-dimensional AlGaN merging layer is grown on a three-dimensional BAlGaN layer;

[0066] Specifically, a two-dimensional AlGaN merging layer was grown in MOCVD at a growth temperature of 1100℃-1300℃ and a growth pressure of 50 torr-500 torr. The gas used during growth was a mixture of N2, H2, and NH3, with a volume ratio of N2, H2, and NH3 of 1:1:1 to 1:10:10. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, TMAl as the Al source, and TMGa as the Ga source.

[0067] S300: An N-type AlGaN layer is grown on the composite layer;

[0068] Specifically, N-type AlGaN layers are grown in MOCVD at a temperature of 1000℃-1300℃ and a pressure of 100 torr-500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and SiH4 is introduced as the N-type doping source; H2 and N2 are used as carrier gases, TMGa is introduced as the Ga source, and TMAl is introduced as the Al source.

[0069] S400: A multi-quantum-well layer is grown on an N-type AlGaN layer;

[0070] Among them, multiple Al atoms are periodically grown using MOCVD. x Ga 1-x N quantum well layer and Al y Ga 1-y An N-quantum barrier layer is obtained, which is equivalent to a multi-quantum well layer. Al x Ga 1-x The growth temperature of the N quantum well layer is 950℃-1150℃, and the growth pressure is 50 torr-300 torr. Al y Ga 1-y The growth temperature of the N quantum barrier layer is 1000℃-1300℃, and the growth pressure is 50 torr-300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga source, and TMAl is introduced as the Al source.

[0071] S500: An electron blocking layer is grown on a multi-quantum-well layer;

[0072] Specifically, the electron blocking layer is grown using MOCVD at a temperature of 1000℃-1100℃ and a pressure of 100 torr-300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source; H2 and N2 are used as carrier gases; TMGa is introduced as the Ga source; and TMAl is introduced as the Al source.

[0073] S600: A P-type AlGaN layer is grown on an electron blocking layer;

[0074] Specifically, a p-type AlGaN layer was grown in MOCVD at a temperature of 1000℃-1100℃ and a pressure of 100 torr-600 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and Cp2Mg was introduced as the p-type doping source; H2 and N2 were used as carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0075] S700: A P-type contact layer is grown on a P-type AlGaN layer;

[0076] Specifically, a P-type contact layer is grown in MOCVD at a temperature of 900℃-1100℃ and a pressure of 100 torr-600 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and Cp2Mg is introduced as the P-type doping source; H2 and N2 are used as carrier gases, and TMGa is introduced as the Ga source.

[0077] The present invention will be further described below with reference to specific embodiments:

[0078] Example 1

[0079] This embodiment provides a light-emitting diode epitaxial wafer, referenced... Figure 1 and Figure 2 It includes a substrate 1 and a composite layer 2, an N-type AlGaN layer 3, a multiple quantum well layer 4, an electron blocking layer 5, a P-type AlGaN layer 6, and a P-type contact layer 7 sequentially disposed on the substrate 1.

[0080] Substrate 1 is a silicon substrate.

[0081] The composite layer 2 comprises a SiO2 patterned layer 21, a ScAlN buffer layer 22, a BGaN island nucleation layer 23, a three-dimensional BAlGaN layer 24, and a two-dimensional AlGaN merging layer 25, stacked sequentially. Specifically, the SiO2 patterned layer 21 is obtained by ICP etching of a 100nm thick SiO2 thin film. Multiple arrayed SiO2 patterns are formed on the substrate 1 through etching, with triangular cross-sections and a SiO2 pattern distribution density of 5×10⁻⁶. 8 pcs / cm 2 The Sc component in the ScAlN buffer layer 22 is 0.55%, and its thickness is 110 nm; the B component in the BGaN island nucleation layer 23 is 0.45%, and its thickness is 2 μm; the Al component in the three-dimensional BAlGaN layer 24 is 0.75%, the B component is 0.005%, and its thickness is 6 μm; the Al component in the two-dimensional AlGaN merging layer 25 is 0.75%, and its thickness is 6 μm.

[0082] In the N-type AlGaN layer 3, the Si doping concentration is 2.5 × 10⁻⁶. 19 cm -3 Its thickness is 3μm.

[0083] Among them, the multiple quantum well layer 4 is an alternating stack of Al x Ga 1-x N quantum well layer (x = 0.55) and Al y Ga 1-y N (y = 0.7) quantum barrier layers, stacking period number 9, single Al x Ga1-x The thickness of the N quantum well layer is 3.5 nm, and a single Al y Ga 1-y The thickness of the N quantum barrier layer is 11 nm.

[0084] Among them, electron blocking layer 5 is Al z Ga 1-z The N-layer (z = 0.75) has a thickness of 30 nm. The p-type AlGaN layer 6 is doped with Mg at a concentration of 5 × 10⁶. 19 cm -3 The thickness is 100 nm. The P-type contact layer 7 is a P-type GaN layer, with Mg as the P-type dopant and a Mg doping concentration of 1 × 10⁻⁶. 20 cm -3 The thickness of the P-type contact layer 7 is 35 nm.

[0085] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0086] (1) Provide a substrate;

[0087] (2) Growing a composite layer on the substrate;

[0088] (I) Growing a SiO2 patterned layer on a substrate;

[0089] Specifically, a SiO2 thin film layer is deposited in the PECVD reaction chamber at a deposition temperature of 280°C. The SiO2 thin film layer is then etched by ICP to obtain a SiO2 patterned layer for 15 minutes. The etching gas used is a mixture of Cl2 and BCl3 with a volume ratio of 10:1.

[0090] (II) Growth of ScAlN buffer layer on SiO2 patterned layer;

[0091] Specifically, the ScAlN buffer layer was grown using MOCVD at a growth temperature of 850℃ and a growth pressure of 150 torr. The gas used during growth was a mixture of N2 and NH3, with a volume ratio of N2 to NH3 of 1:2. NH3 was introduced as the N source, TMAl as the Al source, and Sc(TMHD)3 as the Sc source.

[0092] (III) Growth of BGaN island-shaped nucleation layers on ScAlN buffer layers;

[0093] Specifically, BGaN island nucleation layers were grown in MOCVD at a growth temperature of 950℃ and a growth pressure of 150 torr. The gas used during growth was a mixture of N2, H2, and NH3, with a volume ratio of N2, H2, and NH3 of 1:3:2. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, B2H6 as the B source, and TMGa as the Ga source.

[0094] (Ⅳ) Growth of three-dimensional BAlGaN layers on BGaN island nucleation layers;

[0095] Specifically, a three-dimensional BAlGaN layer was grown in MOCVD at a growth temperature of 1050℃ and a growth pressure of 150 torr. The gas used during growth was a mixture of N2, H2, and NH3, with a volume ratio of N2, H2, and NH3 of 1:3:2. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, B2H6 as the B source, TMAl as the Al source, and TMGa as the Ga source.

[0096] (V) Growing a two-dimensional AlGaN merging layer on a three-dimensional BAlGaN layer;

[0097] Specifically, a two-dimensional AlGaN merging layer was grown in MOCVD at a growth temperature of 1200℃ and a growth pressure of 150 torr. The gas used during growth was a mixture of N2, H2, and NH3, with a volume ratio of 1:2:3. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, TMAl as the Al source, and TMGa as the Ga source.

[0098] (3) An N-type AlGaN layer is grown on the composite layer;

[0099] Specifically, an N-type AlGaN layer was grown using MOCVD at a growth temperature of 1200℃ and a growth pressure of 100 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source and SiH4 was introduced as an N-type doping source. H2 and N2 were used as carrier gases, TMGa was introduced as a Ga source, and TMAl was introduced as an Al source.

[0100] (4) Growth of multiple quantum well layers on N-type AlGaN layers;

[0101] Specifically, Al is periodically grown in MOCVD. x Ga 1-x N quantum well layer and Al y Ga 1-y N quantum barrier layers are used to obtain multiple quantum well layers; Al x Ga 1-xThe growth temperature of the N quantum well layer was 1050℃, and the growth pressure was 200 torr. Al y Ga 1-y The growth temperature of the N quantum barrier layer was 1150℃, and the growth pressure was 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, H2 and N2 were used as carrier gases, TEGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0102] (5) Grow an electron blocking layer on a multi-quantum-well layer;

[0103] Specifically, the electron blocking layer was grown using MOCVD at a growth temperature of 1050℃ and a growth pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; H2 and N2 were used as carrier gases; TMGa was introduced as the Ga source; and TMAl was introduced as the Al source.

[0104] (6) Grow a P-type AlGaN layer on an electron blocking layer;

[0105] Specifically, a p-type AlGaN layer was grown in MOCVD at a growth temperature of 1050℃ and a growth pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and Cp2Mg was introduced as the p-type doping source; H2 and N2 were used as carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0106] (7) Grow a P-type contact layer on a P-type AlGaN layer;

[0107] Specifically, a P-type contact layer was grown in MOCVD at a growth temperature of 1050℃ and a growth pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source, and Cp2Mg was introduced as a P-type dopant source; H2 and N2 were used as carrier gases, and TMGa was introduced as a Ga source.

[0108] Example 2

[0109] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the SiO2 thin film layer has a thickness of 50 nm and the SiO2 pattern distribution density is 1 × 10⁻⁶. 7 pcs / cm 2 The Sc component in the ScAlN buffer layer 22 accounts for 0.3% and has a thickness of 55 nm; the B component in the BGaN island nucleation layer 23 accounts for 0.4% and has a thickness of 0.5 μm; the Al component in the three-dimensional BAlGaN layer 24 accounts for 0.5% and the B component accounts for 0.2%, with a thickness of 2.5 μm; the Al component in the two-dimensional AlGaN merging layer 25 accounts for 0.6% and has a thickness of 1.5 μm. All other parameters are the same as in Example 1.

[0110] Example 3

[0111] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that the proportion of the Sc component gradually increases from 0.05 to 0.3 along the epitaxial growth direction. All other aspects are the same as in Embodiment 2.

[0112] Example 4

[0113] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that, along the epitaxial growth direction, the proportion of Al component in the three-dimensional BAlGaN layer 24 gradually increases from 0.05 to 0.5, while the proportion of B component gradually decreases from 0.5 to 0.01. All other aspects are the same as in Embodiment 3.

[0114] Comparative Example 1

[0115] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite layer 2 does not include the SiO2 patterned layer 21, the ScAlN buffer layer 22, the BGaN island nucleation layer 23, and the three-dimensional BAlGaN layer 24. Correspondingly, the preparation steps for the above-mentioned layers are not included in the preparation method, and the rest is the same as in Example 1.

[0116] Comparative Example 2

[0117] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite layer 2 does not include the SiO2 patterned layer 21, the BGaN island nucleation layer 23, and the three-dimensional BAlGaN layer 24. Correspondingly, the preparation steps for the above-mentioned layers are not included in the preparation method, and the rest is the same as in Example 1.

[0118] Comparative Example 3

[0119] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite layer 2 does not include the BGaN island nucleation layer 23 and the three-dimensional BaAlGaN layer 24. Correspondingly, the preparation method does not include the preparation steps of the above two layers, and the rest is the same as in Example 1.

[0120] Comparative Example 4

[0121] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite layer 2 does not include a three-dimensional BaAlGaN layer 24. Correspondingly, the fabrication method also omits the fabrication step of this layer, while the rest is the same as in Example 1.

[0122] The LED epitaxial wafers obtained in Examples 1-4 and Comparative Examples 1-4 were fabricated into 15mil*15mil chips using the same process conditions. 300 chips were fabricated for each example and comparative example, and tested at 120mA / 60mA currents. Using Comparative Example 1 as a benchmark, the improvement rate of luminous efficacy in each example was calculated. The specific calculation results are shown in the table below:

[0123]

[0124]

[0125] As can be seen from the table, the composite layer structure of this invention effectively improves the luminous efficacy. Furthermore, a comparison between Example 1 and Comparative Examples 1-4 shows that modifying the composite layer structure of this invention does not effectively improve the luminous efficacy.

[0126] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, characterized in that, It includes a substrate and a composite layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer sequentially disposed on the substrate; the composite layer includes a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially. The SiO2 patterned layer includes multiple SiO2 patterns distributed in an array on the substrate; The Sc component in the ScAlN buffer layer accounts for 0.01-0.5%, and its thickness is 10nm-100nm. The proportion of B component in the BGaN island nucleation layer is 0.01-0.4%, and its thickness is 0.1μm-1μm; The three-dimensional BAlGaN layer has an Al component ratio of 0.01-0.7 and a B component ratio of 0.1-0.7, and its thickness is 0.5μm-5μm. The proportion of Al component in the two-dimensional AlGaN merging layer is 0.2-0.7%, and its thickness is 0.5μm-5μm.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The SiO2 patterned layer is obtained by ICP etching of a SiO2 thin film layer, wherein the thickness of the SiO2 thin film layer is 10nm-100nm, and the distribution density of the SiO2 pattern is 1×10⁻⁶. 6 pcs / cm 2 -1×10 8 pcs / cm 2 .

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, Along the epitaxial growth direction, the proportion of Sc component in the ScAlN buffer layer gradually increases from 0.01-0.1 to 0.2-0.

5.

4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, Along the epitaxial growth direction, the proportion of Al component in the three-dimensional BAlGaN layer gradually increases from 0.01-0.1 to 0.2-0.7, while the proportion of B component gradually decreases from 0.5-0.7 to 0.01-0.

1.

5. A method for fabricating a light-emitting diode epitaxial wafer, used to fabricate a light-emitting diode epitaxial wafer as described in any one of claims 1-4, characterized in that, include: A substrate is provided on which a composite layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer are sequentially grown; the composite layer comprises a SiO2 patterned layer, a ScAlN buffer layer, a BGaN island nucleation layer, a three-dimensional BAlGaN layer, and a two-dimensional AlGaN merging layer stacked sequentially. The SiO2 patterned layer includes multiple SiO2 patterns distributed in an array on the substrate; The Sc component in the ScAlN buffer layer accounts for 0.01-0.5%, and its thickness is 10nm-100nm. The proportion of B component in the BGaN island nucleation layer is 0.01-0.4%, and its thickness is 0.1μm-1μm; The three-dimensional BAlGaN layer has an Al component ratio of 0.01-0.7 and a B component ratio of 0.1-0.7, and its thickness is 0.5μm-5μm. The proportion of Al component in the two-dimensional AlGaN merging layer is 0.2-0.7%, and its thickness is 0.5μm-5μm.

6. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, A SiO2 thin film layer is deposited in a PECVD reaction chamber, wherein the deposition temperature of the SiO2 thin film is 250℃-300℃; The SiO2 thin film layer is then etched by ICP to obtain the SiO2 patterned layer. The etching time is 10 min to 20 min. The etching gas is a mixture of Cl2 and BCl3, wherein the volume ratio of Cl2 to BCl3 is 10:1 to 10:

2.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth temperature of the ScAlN buffer layer is 700℃-1000℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2 and NH3, wherein the volume ratio of N2 to NH3 is 1:1-1:

10. The growth temperature of the BGaN island nucleation layer is 900℃-1100℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1 to 1:10:

10. The growth temperature of the three-dimensional BAlGaN layer is 1000℃-1200℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1-1:10:

10. The growth temperature of the two-dimensional AlGaN merging layer is 1100℃-1300℃, the growth pressure is 50 torr-500 torr, and the gas used during growth is a mixture of N2, H2 and NH3, wherein the volume ratio of N2, H2 and NH3 is 1:1:1 to 1:10:

10.

8. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1-4.

Citation Information

Patent Citations

  • Preparation method for semiconductor light-emitting device

    CN104795472A

  • Fine structure for mounting and optical transmitter

    JP2002083953A