Separator for electrochemical device and electrochemical device comprising the same
By using a porous coating of plate-shaped kaolin particles with a Mohs hardness of less than 3 and an ionic dispersant on the separator of a lithium secondary battery, the problems of separator shrinkage and pressure damage at high temperatures are solved, achieving thinner, lighter, and heat-resistant separators.
Patent Information
- Application Number
- CN202280025266.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-08-19
- Filing Date
- 2022-08-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-08-19
AI Technical Summary
The separators in existing lithium secondary batteries are prone to shrinkage or melting at high temperatures, leading to short circuit risks. They are also susceptible to pressure damage during assembly, affecting the safety and performance of the battery.
A porous substrate coating is used, which contains plate-shaped kaolin particles with a Mohs hardness of less than 3 and an ionic dispersant. The coating is bonded by an adhesive resin to form a porous coating with high packing density, which suppresses deformation caused by high temperature and pressure.
The thermal shrinkage characteristics and pressure resistance of the separator have been improved, which enhances the safety and stability of the battery and prevents damage caused by pressure.
Smart Images

Figure CN117157818B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2021-0109732, filed on August 19, 2021.
[0002] This disclosure relates to a separator for an electrochemical device and an electrochemical device comprising the separator. Background Technology
[0003] Recently, energy storage technology has received increasing attention. As its applications expand to power mobile phones, cameras, laptops, and even electric vehicles, research and development of electrochemical devices are becoming more concrete. While electrochemical devices are gaining attention at these levels, the development of rechargeable secondary batteries and high-energy-density lithium-ion batteries has become a focus. Recently, significant attention has been paid to ensuring safety in the development of these secondary batteries.
[0004] Currently, porous substrates made of polyolefin polymer resins are used as separator substrates in manufactured lithium-ion batteries to prevent short circuits between the anode and cathode. However, porous substrates have the problem of low heat resistance due to the shrinkage or melting of the polymer substrate at high temperatures. As a result, when the battery heats up to a high temperature due to internal or external stimuli, the shrinkage or melting of the separator increases the possibility of a short circuit and the rapid release of electrical energy, which can lead to battery explosion or ignition.
[0005] Therefore, in order to solve the above problems, a common approach is to improve heat resistance by forming a porous coating composed of inorganic particles and polymer binder on at least one side of a porous polymer substrate.
[0006] Although metal oxides or hydroxides such as alumina and boehmite are commonly used as inorganic particles, the pore structure of the porous substrate can be damaged when these particles are compressed under pressure during battery assembly. In particular, the higher the hardness of the inorganic particles, the greater the damage to the porous substrate due to localized pressure. Therefore, it is necessary to avoid damage to the separators caused by pressure.
[0007] Furthermore, due to the properties of the materials and the nature of the manufacturing processes, including stretching, polyolefin porous polymer substrates, which are commonly used as separators, exhibit severe thermal shrinkage at temperatures above 150°C, leading to short circuits between the anode and cathode. Therefore, it is necessary to prevent the shrinkage of the separators at high temperatures. Summary of the Invention
[0008] Technical issues
[0009] Therefore, the object of this disclosure is to provide a separator for an electrochemical device and an electrochemical device including the separator, wherein the separator of this disclosure can achieve thinning and lightweighting, improved thermal shrinkage characteristics, and prevention of damage to the separator due to pressure. It will be readily understood that other objects and advantages of this disclosure can be achieved using the means or methods described in the claims, and combinations thereof.
[0010] Technical solution
[0011] The present disclosure author has discovered that the above-mentioned problems can be solved by the following separator for an electrochemical device and an electrochemical device having the separator.
[0012] The first embodiment of this disclosure relates to a separator for an electrochemical device.
[0013] As a separator used in electrochemical devices
[0014] The partition includes a porous substrate and a porous coating formed on at least one side of the porous substrate.
[0015] The porous coating comprises an adhesive resin, inorganic particles, and an ionic dispersant.
[0016] The inorganic particles contain particles with a Mohs hardness of less than 3 and a density of 3 g / cm³. 3 The following plate-shaped particles A,
[0017] The plate-shaped particles A contain kaolin.
[0018] The second embodiment relates to a separator for an electrochemical device according to the first embodiment, wherein...
[0019] The ionic dispersant is an anionic surfactant.
[0020] The third embodiment relates to a separator for an electrochemical device according to the first embodiment, wherein...
[0021] The ionic dispersant is any one of ammonium polymethacrylate, ammonium polyacrylate, sodium polymethacrylate, and sodium polyacrylate.
[0022] The fourth embodiment relates to a separator for an electrochemical device according to any one of the first to third embodiments, wherein...
[0023] The kaolin contains hydroxyl groups on its surface.
[0024] The fifth embodiment relates to a separator for an electrochemical device according to any one of the first to fourth embodiments, wherein...
[0025] The kaolin content is 50% or more relative to 100% by weight of the inorganic particles.
[0026] The sixth embodiment relates to a separator for an electrochemical device according to any one of the first to fifth embodiments, wherein...
[0027] The content of the ionic dispersant ranges from 0.3% to 5% by weight relative to 100% by weight of the inorganic particles.
[0028] The seventh embodiment relates to a separator for an electrochemical device according to any one of the first to fifth embodiments, wherein...
[0029] The aspect ratio of the plate-shaped particles A is in the range of 5 to 30, and the aspect ratio is defined as [length in the main axis direction] / [width in the direction perpendicular to the main axis direction].
[0030] The eighth embodiment relates to a separator for an electrochemical device according to any one of the first to fifth embodiments, wherein...
[0031] The bulk density of the porous coating is in the ratio of the density of the plate-shaped particles A to 0.45 to 0.8, and the bulk density is defined as the weight per unit volume of the porous coating.
[0032] The ninth embodiment relates to an electrochemical device comprising a cathode, an anode, and a separator disposed between the cathode and the anode, wherein the separator is the separator according to any one of the first to eighth embodiments.
[0033] The tenth embodiment relates to an electrochemical device according to the ninth embodiment, wherein...
[0034] The electrochemical device is a lithium secondary battery.
[0035] Beneficial effects
[0036] The separator for electrochemical devices according to this disclosure can suppress shrinkage caused by high-temperature heat and exhibit improved heat shrinkage resistance. Furthermore, by suppressing deformation caused by pressure applied during battery assembly, improved compressive strength can be achieved. Attached Figure Description
[0037] The accompanying drawings illustrate preferred embodiments of the present disclosure and help to better understand the technical concept and content of the present disclosure. The present disclosure is not limited to the interpretation of the drawings. Furthermore, for the purpose of clearer description, the shapes, dimensions, scales, or proportions of the technical elements shown in the drawings have been exaggerated.
[0038] Figure 1 This is a schematic diagram illustrating the mechanism of action of plate-shaped kaolin 1 and ionic dispersant 2 in a partition according to one embodiment of the present disclosure.
[0039] Figure 2 An SEM image of a cross-section of the partition of Example 1 is shown.
[0040] Figure 3 SEM images of the cross-section of the partition of Comparative Example 1 are shown.
[0041] Figure 4 SEM images of the cross-section of the partition of Comparative Example 3 are shown. Detailed Implementation
[0042] The following is a detailed description of this disclosure. Before proceeding with the detailed description, it should be noted that the terms and vocabulary used in the specification and claims should not be construed as limited to their common or dictionary meanings, but rather as meanings and concepts that the author of this disclosure uses to best describe the disclosure, based on the principle that the terms and concepts can be appropriately defined and that are consistent with the technical concept of this disclosure.
[0043] Unless otherwise stated, the use of the phrase "a part contains a certain element" in this specification does not exclude the presence of other elements, and that part may further contain other elements.
[0044] Furthermore, when the meanings used in this specification imply the inherent permissible errors in manufacturing and materials, terms such as “about” and “generally” are used in the sense of that value or close to that value, in order to aid in the understanding of this disclosure and to prevent unscrupulous infringers from using the disclosure of this disclosure in an unreasonable manner.
[0045] The term “A and / or B” as used in this specification means “A, B, or both”.
[0046] This disclosure relates to separators used in electrochemical devices.
[0047] In this disclosure, an electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction, including all devices that carry out electrochemical reactions, such as all types of primary and secondary batteries, fuel cells, solar cells, and capacitors such as supercapacitors. In particular, lithium secondary batteries, including lithium metal secondary batteries, lithium-ion secondary batteries, lithium polymer secondary batteries, or lithium-ion polymer secondary batteries, are preferred among secondary batteries.
[0048] In this disclosure, the partition may include a porous substrate and a porous coating formed on at least one side of the porous substrate.
[0049] A porous substrate refers to a substrate in which multiple pores are formed, serving as a porous ion-conducting barrier that blocks the electrical contact between the anode and cathode while allowing ions to pass through. The pores are interconnected, allowing gas or liquid to permeate from one side of the substrate to the other. From the viewpoint of providing a shutdown function, porous substrates, porous polymer films, etc., including thermoplastic resins, can be used. Here, the shutdown function refers to the function of preventing heat escape from the battery by blocking ion movement when the battery temperature is high by dissolving the thermoplastic resin and closing the pores of the porous substrate. Non-limiting examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polybutene, and polypentene. On the other hand, considering the shutdown function, it is preferable that the melting point of the thermoplastic resin is below 200°C.
[0050] This disclosure does not impose any particular limitation on the thickness of the porous substrate, but it is preferably in the range of 1 to 100 μm, more preferably in the range of 5 to 50 μm or 5 to 30 μm. This disclosure also does not impose any particular limitation on the porosity of the porous substrate, but it is preferably in the range of 10% to 95% or 35% to 65%.
[0051] The porous coating is formed on at least one side of the porous substrate and may include an adhesive resin, inorganic particles and an ionic dispersant.
[0052] In this disclosure, a porous coating is formed by bonding inorganic particles together with the particles in a state where the particles are in contact with each other, thereby creating interstitial volumes between the inorganic particles. These interstitial volumes become empty spaces, resulting in a porous structure. Specifically, in the porous coating of this disclosure, the weight ratio of inorganic particles to adhesive resin can be in the range of 97:3 to 55:45.
[0053] In this disclosure, the adhesive resin is not specifically limited as long as it can provide the bonding force between inorganic particles and the bonding force between the porous coating and the electrode. For example, the adhesive resin can be selected from polyvinylidene fluoride-co-hexafluoropropylene (PVDF-co-HFP), polyvinylidene fluoride-co-trichloroethylene, and polyvinylidene fluoride-co-chlorotrifluoroethylene. ethylene), polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polyisopropyl methacrylate, polybutyl methacrylate, polytert-butyl methacrylate, polysec-butyl methacrylate, polypentyl methacrylate, poly-2-ethylbutyl methacrylate, poly-2-ethylhexyl methacrylate, poly-octyl methacrylate, polyisooctyl methacrylate, polyisononyl methacrylate, polylauryl methacrylate, polytetradecyl methacrylate, poly(N-vinylpyrrolidone), polyacrylonitrile, polyvinyl acetate, ethylene-co-vinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinyl alcohol One or more of the following groups: alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methylcellulose, acrylonitrile-styrene-butadiene copolymer, and polyimide.
[0054] Furthermore, the adhesive resin can be a particulate polymer adhesive resin. For example, the adhesive resin can be an acrylic copolymer, styrene-butadiene rubber, or a mixture of two or more of these. The acrylic copolymer may include a copolymer of ethylhexyl acrylate and methyl methacrylate, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, a copolymer of butyl acrylate and methyl methacrylate, or a mixture of two or more of these.
[0055] In this disclosure, inorganic particles may include plate-shaped particles A.
[0056] According to one embodiment of this disclosure, the plate-shaped particle A has a Mohs hardness of about 3 or less and a density of about 3 g / cm³. 3 The following are preferred: a Mohs hardness of about 2.3 to 2.7 and a density of about 2.5 to 2.8 g / cm³. 3 Within this range, when plate-shaped particles with the aforementioned Mohs hardness and density are included, a lighter and thinner separator can be formed with a high packing density, resulting in excellent heat resistance and safety. Furthermore, separator deformation caused by pressure applied during battery assembly is mitigated, thereby exhibiting excellent compressive strength.
[0057] The aspect ratio of the plate-like particles A mentioned above is in the range of 5 to 100, preferably in the range of 5 to 30. This aspect ratio is defined as [length in the main axis direction] / [width in the direction perpendicular to the main axis direction]. When the aspect ratio is greater than the above range, the path for lithium ion movement becomes longer, and the impedance of the separator increases. In addition, the plate-like particles A can be arranged or stacked in a direction parallel to the porous coating (planar direction).
[0058] According to one embodiment of this disclosure, the plate-shaped particles A may contain kaolin.
[0059] Kaolin is represented by the chemical composition Al2O3·2SiO2·2H2O, and includes common kaolin, metakaolin, and calcined kaolin. Here, kaolin refers to common kaolin with hydroxyl (-OH) groups on its surface.
[0060] Metakaolin is calcined at a temperature of about 500°C or higher to remove almost all hydroxyl groups from its surface, and then calcined at a temperature of about 900°C or higher to completely remove the hydroxyl groups from its surface. In this disclosure, kaolin containing hydroxyl groups on its surface is preferred, while metakaolin and / or calcined kaolin are not preferred.
[0061] Specifically, in this disclosure, the combination of plate-shaped conventional kaolin and the following ionic dispersant has the effect of suppressing shrinkage caused by high temperature heat and suppressing deformation caused by pressure. This is because, when using kaolin with hydroxyl (-OH) groups on the surface and kaolin with ionic dispersant, the plate-shaped kaolin is arranged in the planar direction, so that even when pressure is applied, damage to the porous substrate caused by kaolin will not occur.
[0062] However, when metakaolin or calcined kaolin and ionic dispersants are used together at high temperatures, the charge characteristics of the particles change, and the metakaolin or calcined kaolin cannot align in the planar direction, thus failing to achieve the desired effect of this disclosure. Furthermore, even when metal oxides such as alumina and boehmite are used as inorganic particles commonly used in the art when the porous substrate is compressed by inorganic particles under pressure during battery assembly, the pore structure of the porous substrate may be damaged or the separators may deform under pressure, thus failing to achieve the desired effect of this disclosure.
[0063] Furthermore, when conventional kaolin and the following ionic dispersant are used in this disclosure, a high packing density is observed in the porous coating. In particular, the kaolin contained in the separator of this disclosure has a density of approximately 3 g / cm³. 3 The following is preferred: about 2.5 to 2.8 g / cm³ 3 When the particles are plate-like, the septa can be approximately 1.1 to 1.5 g / cm³. 3 Or approximately 1.1 to 1.3 g / cm³ 3 The bulk density is within a certain range. In this disclosure, the bulk density can be calculated from the weight per unit volume of the porous coating.
[0064] In the present disclosure, the effects of suppressing shrinkage caused by high-temperature heat and suppressing deformation caused by pressure can be determined by the planar alignment degree of the plate-like particles. The planar alignment degree of the plate-like particles tends to increase correspondingly as the ratio of the bulk density of the porous coating to the density of the plate-like particles (bulk density / density) increases. Generally, when the porous coating contains high-density particles, the bulk density tends to become high due to the high density of the particles. Therefore, it is impossible to determine the alignment of the plate-like particles in the plane direction only based on the bulk density of the porous coating, and the intrinsic density of the plate-like particles needs to be taken into consideration. The present disclosure includes kaolin particles with a relatively low density, and the kaolin particles are aligned in the plane direction, so that a high bulk density can be obtained. At this time, [bulk density] / [density] may be 0.45 to 0.80, preferably 0.46 or more. Thereby, a separator that is lighter and thinner than existing separators can be formed, a high bulk density can be obtained, and excellent heat resistance safety is further exhibited. When the plate-like particles have an aspect ratio exceeding the above aspect ratio range, the plate-like particles will have a [bulk density] / [density] ratio greater than the above range, and at this time, the path for lithium ion movement will become longer, resulting in an increase in the impedance of the separator.
[0065] According to one embodiment of the present disclosure, from the viewpoint of improving the heat resistance of the separator, the content of the plate-like particles A may be 30% by weight or more, or 50% by weight or more relative to 100% by weight of the inorganic particles.
[0066] In the present disclosure, the inorganic particles may include particles other than the plate-like particles A, and the inorganic particles other than the plate-like particles A are not particularly limited as long as the electrochemical performance of the inorganic particles is stable. For example, as long as the inorganic particles other than the particles A are within the operating voltage range of the applicable electrochemical device (for example, with Li / Li + as the reference of 0 to 5 V) do not undergo oxidation and / or reduction reactions, the inorganic particles other than the particles A are not particularly limited. Non-limiting examples include ZrO₂, BaTiO₃, Pb(Zr,Ti)O₃ (PZT), Pb 1-x La x Zr 1-y TiᵧO₃ (PLZT), PB(Mg₃Nb 2 / 3 )O₃-PbTiO₃ (PMN-PT), HfO₂, SrTiO₃, SnO₂, CeO₂, MgO, NiO, CaO, ZnO, ZrO₂, Y₂O₃, Al₂O₃, TiO₂, AlOOH, Al(OH)₃, SiC, or mixtures thereof. Meanwhile, in addition to these, lithium phosphate (Li₃PO₄), lithium titanium phosphate (Li x Ti y (PO₄)₃, 0<x<2, 0<y<3), lithium aluminum titanium phosphate (Li x Aly Ti z (PO4)3, 0<x<2, 0<y<1, 0<z<3), (LiAlTiP) x O y glass (0<x<4, 0<y<13), lithium lanthanum titanate (LixLayTiO3, 0<x<2, 0<y<3), lithium germanium thiophosphate (Li x Ge y P z S w , 0<x<4, 0<y<1, 0<z<1, 0<w<5), lithium nitride (Li x N y , 0<x<4, 0<y<2), SiS2-based glass (Li x Si y S z , 0<x<3, 0<y<2, 0<z<4), P2S5-based glass (Li x P y S z , 0<x<3, 0<y<3, 0<z<7) or a combination of two or more of these inorganic particles.
[0067] According to one embodiment of the present disclosure, an ionic dispersant is added to disperse the inorganic particles, so as to prevent aggregation of solid components during the formation of the porous coating. In particular, in the present disclosure, by using the ionic dispersant as a dispersant, the plate-like particles A contained in the porous coating can be aligned in the planar direction. As a result, the effects of suppressing shrinkage caused by high-temperature heat and suppressing deformation caused by pressure can be obtained. In the present disclosure, the planar direction alignment means that the wide surfaces of the plate-like particles A are aligned in a direction substantially parallel to the surface of the porous substrate.
[0068] In the present disclosure, any ionic dispersant that can align the plate-like particles A in the planar direction can be used, and the present disclosure is not particularly limited in this regard.
[0069] In the present disclosure, when the plate-like particles A include kaolin, an anionic surfactant can be used as the ionic dispersant.
[0070] Figure 1 This is a schematic diagram of the action mechanism when the plate-like particle kaolin 1 and the ionic dispersant 2 are used in the separator. For example, the action mechanism when an anionic surfactant is used as the ionic dispersant is described.
[0071] Kaolin's surface portion exhibits a predominantly negative charge (δ-), while its edge portion exhibits a predominantly positive charge (δ+). Therefore, in the absence of anionic surfactants, the kaolin cannot align in the planar direction due to the interaction between the negative charge on the surface and the positive charge on the edge. However, when kaolin is used with anionic surfactants, the anionic surfactant interacts with the positive charge on the kaolin's edge, causing the surfactant to adsorb onto the edge portion of the kaolin surface. As a result, the total negative charge on the kaolin surface increases, suppressing the interaction between the negative charge on the surface and the positive charge on the edge, thus allowing the kaolin to align in the planar direction.
[0072] Typical kaolin is in the form of plate-like particles. Compared to other kaolins such as metakaolin and calcined kaolin, or other plate-like metal hydroxides such as aluminum hydroxide and magnesium hydroxide, it has a greater difference in charge between its surface and edge portions. Therefore, when using ionic dispersants, it achieves relatively superior surface alignment. This can result in a relatively higher bulk density / density ratio.
[0073] Anionic surfactants are surfactants that contain anionic functional groups as ionic or ionizable groups. The anionic functional groups contained in anionic surfactants may include -CO. 2- PO4 3- -SO 3- -OSO 3- -HPO 3- -PO3 2- -HPO 2- -PO2 2- -PO - Or a combination of two or more of these.
[0074] In one embodiment of this disclosure, the anionic surfactant may be at least one metal salt containing the aforementioned anionic functional groups. Examples of metal salts may include one or more metal salts selected from sodium salts, potassium salts, ammonium salts, magnesium salts, etc., and there is no particular limitation on the metal salt. The anionic surfactant may include sodium salts, potassium salts, ammonium salts, magnesium salts of carboxylic acids, or combinations of two or more of these. Specific examples of anionic surfactants may include any one of ammonium polymethacrylate, ammonium polyacrylate, sodium polymethacrylate, and sodium polyacrylate, and this disclosure does not have any particular limitation on anionic surfactants.
[0075] To ensure the planar alignment of the plate-shaped particles A, the content of the ionic dispersant can be from 0.3% to 5% by weight or from 0.5% to 3% by weight relative to 100% by weight of inorganic particles.
[0076] On the other hand, in addition to the aforementioned adhesive resin, inorganic particles and ionic dispersants that are components of the porous coating, the separator may also contain other additives such as flame retardants if necessary.
[0077] According to one embodiment of the present disclosure, a separator can be made by preparing a composition for forming a porous coating comprising inorganic particles, a binder resin and an ionic dispersant, coating the composition on at least one side of a porous substrate and then drying the composition.
[0078] First, a composition for forming a porous coating can be prepared by preparing a polymer solution in which an adhesive resin is dissolved in a solvent, and then adding and dispersing inorganic particles into the polymer solution. The inorganic particles can be pre-crushed to a specified average particle size and added in that state, or the inorganic particles can be crushed to a specified particle size and dispersed using methods such as ball milling. On the other hand, in one embodiment of this disclosure, it is preferable to control the concentration of the solid components other than the solvent in the dispersion to be in the range of 20% to 70% by weight.
[0079] Non-limiting examples of solvents used here may include one or more compounds selected from acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, cyclohexane, methanol, ethanol, isopropanol, propanol, and water, or mixtures of two or more of these compounds.
[0080] There are no particular limitations on the method for coating a porous substrate with a composition for forming a porous coating, but slit coating or dip coating is preferred. In slit coating, the composition supplied by a slit die is coated on the entire surface of the substrate, and the coating thickness can be adjusted based on the supply flow rate of a metering pump. Dip coating, on the other hand, coats the substrate by immersing it in a container holding the composition. The coating thickness can be adjusted based on the concentration of the composition and the speed at which the substrate is removed from the container. Furthermore, for more precise control of the coating thickness, measurements can be taken after immersion using a Meller rod or similar device.
[0081] An inorganic coating is formed on the surface of a porous substrate coated with a composition for forming a porous coating by drying it in a dryer such as an oven. The porous coating can be formed on at least one or both sides of the porous substrate.
[0082] This disclosure does not impose any particular limitation on the thickness of the separator, which can be in the range of 5 μm to less than 50 μm. However, from the viewpoint of improving insulation and thermal stability, the range of 5 μm to 20 μm or 10 μm to 16 μm is preferred.
[0083] The electrochemical device of this disclosure includes a cathode, an anode, and a separator inserted between the cathode and the anode, wherein the separator is a separator of one embodiment of the present disclosure described above.
[0084] There are no particular limitations on the electrodes used in conjunction with the separators of this disclosure. Electrodes can be fabricated by incorporating electrode active materials onto electrode current collectors in accordance with common methods known in the art.
[0085] Non-limiting examples of cathode active materials in electrode active materials may include conventional cathode active materials that can be used in the cathodes of existing lithium secondary batteries, specifically lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or combinations thereof.
[0086] Non-limiting examples of anode active materials may include conventional anode active materials that can be used in the anodes of existing lithium secondary batteries. Specifically, lithium metal or lithium alloys and lithium adsorbent materials such as carbon, petroleum coke, activated carbon, graphite or other carbon materials may be used.
[0087] Non-limiting examples of cathode current collectors may include foils made of aluminum, nickel, or combinations thereof, and non-limiting examples of anode current collectors may include foils made of copper, gold, nickel, copper alloys, or combinations thereof.
[0088] The electrolyte that can be used in the electrochemical device described in this disclosure is such as A + Salts of the B-structure, A + Including Li + Na + K + Alkali metal cations or combinations thereof forming ions, or B-including PF6 - BF4 - Cl - ,Br - I - ClO4 - AsF6 - CH3CO2 - CF3SO3 - N(CF3SO2)2 - C(CF2SO2)3 -Or combinations thereof. These salts can be dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), or γ-butyrolactone, or mixtures of these organic solvents, to obtain an electrolyte, and this disclosure does not specifically limit this.
[0089] Depending on the manufacturing process and required physical properties of the final product, electrolyte injection can be performed at an appropriate stage of the battery manufacturing process. That is, the electrolyte can be injected before battery assembly or at the final stage of battery assembly.
[0090] Furthermore, this disclosure provides a battery module including a battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source, wherein the battery includes an electrode assembly. Specific examples of the device include power tools powered by a battery motor, electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), electric two-wheelers including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and power storage systems; this disclosure does not specifically limit these categories.
[0091] The present disclosure will now be illustrated with examples. These examples may have various other variations, and the scope of the disclosure should not be construed as limited to the examples described below. The examples are provided to provide a more complete explanation of the disclosure to those skilled in the art.
[0092] Example
[0093] The partitions for the embodiments and comparative examples were prepared according to the following method.
[0094] Example 1
[0095] 1) A porous polyethylene film (9 μm thick, 45% porosity) was fabricated as a porous polymer substrate.
[0096] 2) Next, 20g of plate-shaped kaolin (20 aspect ratio), 0.3g of ionic dispersant (ammonium polyacrylate), and 20g of 0.5mm zirconia beads were added to 30g of solvent containing water and ethanol in a 95:5 ratio. The mixture was stirred with a paint mixer for 2 hours to prepare an inorganic dispersion.
[0097] 3) Subsequently, 1g of 40% solid acrylic adhesive (TRD202A manufactured by JSR Corporation) and 10g of 40% water-dispersed acrylic particulate adhesive (APAC AP-0821, particle size 350nm) were added to the above inorganic dispersion and stirred to prepare the coating slurry.
[0098] 4) The above coating slurry was filtered through a 200-mesh filter and coated onto one side of the polyethylene porous film using a doctor blade coater, and then dried using a dryer. Under the same conditions, the same coating was applied again to the opposite side of the polyethylene porous film, thus creating a double-coated separator.
[0099] The results are shown in Table 2.
[0100] Example 2 and Comparative Examples 1 to 4
[0101] As shown in Table 1 below, the separator was fabricated in the same manner as in Example 1, except that the types of inorganic materials and dispersants were changed. The results of this method are shown in Table 2.
[0102] Table 1
[0103]
[0104] Table 2
[0105]
[0106]
[0107] As shown in Table 2, the thickness of the partitions produced in Comparative Examples 1, 2 and 1 to 4 is the same or similar. However, since the deformation caused by pressure in Comparative Examples 1 to 4 is greater than that in Examples 1 and 2, it is confirmed that there is a large difference between the thickness of the compressed partition and the thickness of the produced partition.
[0108] Furthermore, it can be confirmed that Examples 1 and 2 exhibit higher packing densities compared to Comparative Examples 1 to 3. For reference, Comparative Example 4 exhibits a higher packing density than Example 1, but due to the high alumina particle count, the [packing density] / [density] ratio is relatively low.
[0109] Furthermore, when measuring the air permeability of the separator before compression, Examples 1 and 2 showed greater air permeability, but after compression, Comparative Examples 1 to 4 showed greater air permeability than the Examples, indicating that the air permeability of lithium-intercalated Comparative Examples 1 to 4 decreased due to compression.
[0110] Furthermore, compared to those of Comparative Examples 1 to 4, it was confirmed that Examples 1 and 2 had lower thermal shrinkage rates in the MD and TD directions of the fabricated partitions.
[0111] Evaluation of the physical properties of the partition
[0112] The physical properties of the partitions fabricated in the embodiments and comparative examples were evaluated in the following manner.
[0113] (1) Thickness
[0114] The thickness of the partition was measured using a thickness gauge (Mitutoyo VL-50S-B).
[0115] (2) Measurement of air permeability
[0116] Air permeability was measured using a Gurley air permeability meter according to JIS P-8117. The measured diameter of 100cc of air was 28.6mm, and the area was 645mm². 2 The time spent.
[0117] (3) Evaluation method of heat shrinkage rate
[0118] The partition was cut into 5×5cm pieces and stored in a 135℃ convection oven for 30 minutes. The length changes in the MD and TD directions were then measured.
[0119] Heat shrinkage rate (%) = {(size before shrinkage - size after shrinkage) / size before shrinkage} × 100
[0120] (4) Preparation of compression diaphragm specimens
[0121] The separator was cut into 5×5cm pieces, and 10×10cm square peelable PET films were laminated onto its upper and lower parts. The peelable surface of the PET film was then brought into contact with the separator. The separator with the laminated PET film was then hot-pressed at 70°C and 5MPa for 10 seconds to produce a compressed separator sample.
Claims
1. A separator for an electrochemical device, the separator comprising a porous substrate and a porous coating formed on at least one side of the porous substrate, wherein the porous coating comprises an adhesive resin, inorganic particles, and an ionic dispersant, the inorganic particles comprising a Mohs hardness of less than 3 and a density of 3 g / cm³. 3 The following are plate-shaped particles A, which contain kaolinite with hydroxyl groups on its surface. The ionic dispersant mentioned above is an anionic surfactant. The ratio of the bulk density of the porous coating to the density of the plate-shaped particles A is 0.45 to 0.8, and the bulk density is defined as the weight per unit volume of the porous coating.
2. The separator as claimed in claim 1, wherein the ionic dispersant is any one of ammonium polymethacrylate, ammonium polyacrylate, sodium polymethacrylate, and sodium polyacrylate.
3. The partition as claimed in claim 1, wherein the kaolin content is 50% by weight or more relative to 100% by weight of the inorganic particles.
4. The separator of claim 1, wherein the content of the ionic dispersant is from 0.3% to 5% by weight relative to 100% by weight of the inorganic particles.
5. The partition as claimed in claim 1, wherein the aspect ratio of the plate-shaped particles A is in the range of 5 to 30, and the aspect ratio is defined as [length in the main axis direction] / [width in the direction perpendicular to the main axis direction].
6. An electrochemical device comprising a cathode, an anode, and a partition disposed between the cathode and the anode. The partition is the partition according to any one of claims 1 to 5.
7. The electrochemical device of claim 6, wherein the electrochemical device is a lithium secondary battery.
Citation Information
Patent Citations
Mask
KR1020210109732A
Separator, manufacturing method thereof, and lithium ion secondary cell
CN104641490A
Separator for rechargeable battery and rechargeable battery including the same
US20170133653A1