Chitosan hydrogel and chitosan dry gel, and preparation method and application thereof

By reacting citral and cinnamaldehyde with chitosan to generate Schiff bases, and then crosslinking them with polyols and photoinitiators, the problem of insufficient mechanical strength of chitosan hydrogels was solved, and chitosan hydrogels suitable for the biomedical field were prepared.

CN117164887BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210580199.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-25
Publication Date
2026-11-20
Estimated Expiration
2042-05-25

AI Technical Summary

Technical Problem

The existing chitosan hydrogels have low mechanical strength, which limits their application in the biomedical field, and the cross-linking agents such as formaldehyde and glutaraldehyde are toxic to cells.

Method used

Schiff bases are generated by reacting citral and/or cinnamaldehyde with chitosan powder, and then crosslinked under ultraviolet light using polyols and photoinitiators to form chitosan hydrogels, thereby enhancing their mechanical properties.

Benefits of technology

The prepared chitosan hydrogel has good mechanical properties and is suitable for biomedical applications. Furthermore, the crosslinking agent is a food flavoring, which has good biocompatibility.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a kind of chitosan hydrogel and chitosan dry glue and its preparation method and application.The preparation method of the chitosan hydrogel includes: step 1, chitosan powder is sequentially mixed with acetic acid aqueous solution, polyhydric alcohol aqueous solution, and mixture A is obtained;Step 2, citral and / or cinnamyl aldehyde are mixed with solvent, and mixed with photo initiator, and mixture B is obtained;Step 3, the mixture A is mixed with the mixture B for the first time, and reaction is obtained, and reaction product is obtained;Step 4, the reaction product is irradiated with ultraviolet, and chitosan hydrogel is obtained.The chitosan hydrogel prepared by the method of the application has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a chitosan hydrogel, its preparation method and application, as well as a chitosan dry gel, its preparation method and application. Background Technology

[0002] Chitosan (CS) is a polysaccharide bioactive polymer produced by the deacetylation of chitin. It consists of d-glucosamine and n-acetyl-d-glucosamine linked by β-1,4 glycosidic bonds. Chitosan possesses excellent properties such as antibacterial activity, ease of modification, and biodegradability, and has been applied in wound dressings, tissue repair, and drug sustained release. In 2001, it was recognized by the US FDA as a GRAS (Generally Recognized As Safe) substance.

[0003] The amino groups on chitosan molecules can undergo nucleophilic addition reactions with carbonyl compounds. Formaldehyde and glutaraldehyde are commonly used to crosslink chitosan molecules, but these substances are highly toxic to cells, limiting their application in the biomedical field. Furthermore, existing chitosan hydrogels have relatively low mechanical strength, further restricting their applications. Summary of the Invention

[0004] To address the aforementioned problems in the existing technology, this invention provides a novel chitosan hydrogel and chitosan dry gel, along with their preparation method and applications. The chitosan hydrogel prepared using the method of this invention exhibits excellent mechanical properties.

[0005] The first aspect of this invention provides a method for preparing chitosan hydrogel, comprising:

[0006] Step 1: Chitosan powder is mixed sequentially with aqueous acetic acid solution and aqueous polyol solution to obtain mixture A;

[0007] Step 2: Citral and / or cinnamaldehyde are mixed with a solvent and then mixed with a photoinitiator to obtain mixture B;

[0008] Step 3: Mix the mixture A and the mixture B in a first mixing and reaction to obtain the reaction product;

[0009] Step 4: Irradiate the reaction product with ultraviolet light to obtain chitosan hydrogel.

[0010] According to some embodiments of the preparation method described in this invention, preferably, the degree of deacetylation of the chitosan powder is ≥85%.

[0011] According to some embodiments of the preparation method of the present invention, preferably, the concentration of acetic acid in the aqueous acetic acid solution is 0.1-3% by weight, more preferably 1-2% by weight.

[0012] According to some embodiments of the preparation method of the present invention, preferably, the concentration of chitosan in mixture A is 0.5-5% by weight, more preferably 1-3% by weight.

[0013] According to some embodiments of the preparation method of the present invention, preferably, the polyol is selected from at least one of glycerol, butanediol, hexanediol, pentanediol and polyvinyl alcohol.

[0014] According to some embodiments of the preparation method of the present invention, preferably, the concentration of the polyol aqueous solution is 5-20% by weight, more preferably 7-12% by weight.

[0015] According to some embodiments of the preparation method of the present invention, preferably, the final concentration of the polyol in the mixture A is 0.1-10% by weight, more preferably 3-6% by weight.

[0016] According to some embodiments of the preparation method of the present invention, preferably, the solvent is acetone and / or anhydrous ethanol.

[0017] According to some embodiments of the preparation method described in this invention, preferably, the concentration of citral and / or cinnamaldehyde in the solvent is 1-50% by weight, more preferably 5-25% by weight.

[0018] According to some embodiments of the preparation method of the present invention, preferably, the total weight ratio of citral and / or cinnamaldehyde to chitosan powder is 0.1:1-10:1, more preferably 3:1-7:1.

[0019] According to some embodiments of the preparation method of the present invention, preferably, the photoinitiator is selected from at least one of lithium phenyl-2,4,6-trimethylbenzoylphosphonate and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.

[0020] According to some embodiments of the preparation method of the present invention, preferably, the amount of photoinitiator is 0.01-5% by weight of chitosan, more preferably 0.1-2% by weight.

[0021] According to some embodiments of the preparation method of the present invention, preferably, the ultraviolet irradiation conditions include: irradiation at 365 nm for 1-6 hours, preferably irradiation at 365 nm for 2-4 hours.

[0022] According to some embodiments of the preparation method of the present invention, preferably, the conditions for the first mixing include: a temperature of 0-60°C, preferably 10-40°C, and light-protected conditions.

[0023] According to some embodiments of the preparation method of the present invention, preferably, the mixture B is added dropwise to the mixture A, and more preferably, the dropping rate is 5-10 seconds / drop.

[0024] According to some embodiments of the preparation method of the present invention, preferably, the reaction conditions include: a temperature of 20-60°C, under light-protected conditions, and a time of 5-60 minutes, preferably 10-40 minutes.

[0025] According to some specific embodiments of the preparation method described in this invention, the chitosan hydrogel preparation method includes:

[0026] Step 1: Add a certain amount of chitosan powder to an acetic acid aqueous solution, stir thoroughly until completely dissolved, then add a certain amount of polyol aqueous solution and mix evenly.

[0027] Step 2: Dissolve a certain amount of citral and / or cinnamaldehyde in acetone or anhydrous ethanol, then add a certain amount of photoinitiator and mix well.

[0028] Step 3: Under conditions of 0-60℃, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0029] Step 4: Under conditions of 20-60℃, keep in the dark and let the reaction continue for 5-60 minutes;

[0030] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365nm for 1-6 hours to obtain chitosan hydrogel.

[0031] A second aspect of the present invention provides a chitosan hydrogel obtained according to the preparation method described above. The chitosan hydrogel of the present invention is a colorless to yellow hydrogel in appearance.

[0032] A third aspect of the present invention provides a method for preparing chitosan dry gel, comprising: soaking the chitosan hydrogel obtained according to the above-described method for preparing chitosan hydrogel or the above-described chitosan hydrogel in distilled water and then freeze-drying it.

[0033] According to the preparation method of the present invention, in some ways of preparing chitosan dry gel, preferably, the soaking conditions include: soaking time of 2-4 days, and changing distilled water 2-4 times a day.

[0034] According to the preparation method of the present invention, in some ways of preparing chitosan dry gel, preferably, the freeze-drying conditions include: a temperature of -40 to -60°C and a time of 24 to 48 hours.

[0035] According to some specific embodiments of the preparation method described in this invention, the method for preparing the chitosan dry gel includes:

[0036] Step 1: Add a certain amount of chitosan powder to an acetic acid aqueous solution, stir thoroughly until completely dissolved, then add a certain amount of polyol aqueous solution and mix evenly.

[0037] Step 2: Dissolve a certain amount of citral and / or cinnamaldehyde in acetone or anhydrous ethanol, then add a certain amount of photoinitiator and mix well.

[0038] Step 3: Under conditions of 0-60℃, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0039] Step 4: Under conditions of 20-60℃, keep in the dark and let the reaction continue for 5-60 minutes;

[0040] Step 5: Place the reaction mixture under a UV lamp and irradiate it at 365nm for 1-6 hours to obtain chitosan hydrogel;

[0041] Step 6: Soak the prepared chitosan hydrogel in distilled water for 3 days, changing the distilled water three times a day, and freeze-dry to obtain the hydrogel dry gel.

[0042] The fourth aspect of this invention provides a method for preparing the above-described chitosan hydrogel, the above-described chitosan hydrogel, a method for preparing the above-described chitosan dry gel, or an application of the above-described chitosan dry gel. Preferably, it is used in biomedicine.

[0043] The beneficial effects of this invention are:

[0044] Citral and cinnamaldehyde are both aldehyde compounds with unsaturated double bonds and are permitted food flavorings in my country. Citral can be used to synthesize vitamin A, while cinnamaldehyde has medicinal effects such as anti-ulcer, antiviral, vasodilatory, and blood circulation-promoting properties. Both aldehydes have bactericidal and disinfectant effects. In the preparation method of this invention, chitosan powder reacts with citral and / or cinnamaldehyde to form a Schiff base through the reaction of amino and aldehyde groups. Preliminary gelation occurs under the action of hydrogen bonds, but the resulting gel is brittle and has low strength. Adding polyols can improve the gel's flexibility, and the hydroxyl groups on the chitosan molecular chain can form hydrogen bonds with the hydroxyl groups on the polyol, increasing the gel's strength. The photoinitiator used in this invention has good biocompatibility, and under ultraviolet light initiation, it crosslinks the double bonds on the citral and / or cinnamaldehyde molecules, further enhancing the gel's strength. The preparation method of this invention is simple, and the resulting chitosan hydrogel has good mechanical properties. This hydrogel is expected to be applied in biomedical fields such as dressings. Detailed Implementation

[0045] To make the present invention easier to understand, the present invention will be described in detail below with reference to embodiments. These embodiments are for illustrative purposes only and are not limited to the scope of application of the present invention.

[0046]

Example 1

[0047] Step 1: Add 0.3g of chitosan powder (90% degree of deacetylation) to 10g of acetic acid aqueous solution (1% by weight) and stir thoroughly until completely dissolved. Then add 20g of glycerol aqueous solution (7.5% by weight) and mix well to obtain a mixed solution.

[0048] Step 2: Dissolve 1.5g of citral in 20g of acetone, then add 0.0015g of photoinitiator lithium phenyl-2,4,6-trimethylbenzoylphosphonate, mix well to obtain a mixture.

[0049] Step 3: Under conditions of 25°C, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0050] Step 4: Under conditions of 25°C, keep the container in the dark and let it stand for another 20 minutes to continue the reaction.

[0051] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365 nm for 4 hours to obtain a pale yellow chitosan hydrogel.

[0052]

Example 2

[0053] Step 1: Add 2g of chitosan powder (95% degree of deacetylation) to 80g of acetic acid aqueous solution (1.5% by weight) and stir thoroughly until completely dissolved. Then add 20g of polyvinyl alcohol aqueous solution (10% by weight) and mix well to obtain a mixed solution.

[0054] Step 2: Dissolve 6g of cinnamaldehyde in 40g of anhydrous ethanol, then add 0.003g of photoinitiator 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, mix well to obtain a mixture.

[0055] Step 3: Under conditions of 40°C, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0056] Step 4: Under conditions of 40℃, keep in the dark and let the reaction continue for 15 minutes.

[0057] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365nm for 3 hours to obtain a transparent chitosan hydrogel.

[0058]

Example 3

[0059] Step 1: Add 3g of chitosan powder (degree of deacetylation 88%) to 50g of acetic acid aqueous solution (concentration 2% by weight) and stir thoroughly until completely dissolved. Then add 50g of butanediol aqueous solution (concentration 12% by weight) and mix well to obtain a mixed solution.

[0060] Step 2: Dissolve 6g of citral and 6g of cinnamaldehyde in 50g of acetone, then add 0.032g of photoinitiator lithium phenyl-2,4,6-trimethylbenzoylphosphonate, mix well to obtain a mixture.

[0061] Step 3: Under conditions of 10°C, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0062] Step 4: Under conditions of 10℃, keep in the dark and let the reaction continue for 40 minutes.

[0063] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365 nm for 4 hours to obtain a yellow chitosan hydrogel.

[0064]

Example 4

[0065] The chitosan hydrogel prepared in Example 1 was soaked in distilled water for 3 days, with the distilled water being changed three times a day, and then freeze-dried at -45°C for 48 hours to obtain the dry hydrogel.

[0066]

Example 5

[0067] The chitosan hydrogel prepared in Example 2 was soaked in distilled water for 3 days, with the distilled water being changed three times a day, and then freeze-dried at -55°C for 24 hours to obtain the dry hydrogel.

[0068]

Example 6

[0069] The chitosan hydrogel prepared in Example 3 was soaked in distilled water for 3 days, with the distilled water being changed three times a day, and then freeze-dried at -50°C for 38 hours to obtain the dry hydrogel.

[0070] Comparative Example 1

[0071] The method is the same as in Example 2, except that an aqueous solution of polyol is not added, i.e.:

[0072] Step 1: Add 1.5g of chitosan powder (degree of deacetylation 95%) to 80g of acetic acid aqueous solution (concentration 1.5% by weight), stir thoroughly until completely dissolved, and obtain a mixed solution.

[0073] Step 2: Dissolve 6g of cinnamaldehyde in 40g of anhydrous ethanol, then add 0.003g of photoinitiator 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, mix well to obtain a mixture.

[0074] Step 3: Under conditions of 40°C, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0075] Step 4: Under conditions of 40℃, keep in the dark and let the reaction continue for 15 minutes.

[0076] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365nm for 3 hours to obtain a transparent chitosan hydrogel.

[0077] Comparative Example 2

[0078] The method is the same as in Example 2, except that no photoinitiator is added, i.e.:

[0079] Step 1: Add 1.5g of chitosan powder (degree of deacetylation 95%) to 80g of acetic acid aqueous solution (concentration 1.5% by weight) and stir thoroughly until completely dissolved. Then add 20g of polyvinyl alcohol aqueous solution (concentration 10% by weight) and mix well to obtain a mixed solution.

[0080] Step 2: Dissolve 6g of cinnamaldehyde in 40g of anhydrous ethanol to obtain a mixture.

[0081] Step 3: Under conditions of 40°C, stirring, and protection from light, add the mixture from Step 2 dropwise to the mixed solution from Step 1 at a rate of one drop every 5 seconds.

[0082] Step 4: Under conditions of 40℃, keep in the dark and let the reaction continue for 15 minutes.

[0083] Step 5: Place the reaction mixture under a UV lamp and irradiate at 365nm for 3 hours to obtain a transparent chitosan hydrogel.

[0084] [Test Example]

[0085] Rheological analysis

[0086] The rheological properties of chitosan hydrogels from Examples 1-3 and Comparative Examples 1-2 were tested using a rheometer in small-amplitude oscillation mode. A 20mm plate was used, with a plate spacing of 1mm, and the test temperature was 37℃. The frequency was set to 10 rad·s during the test. -1 The strain in the linear viscoelastic region was 1%, and the results are shown in Table 1.

[0087] Table 1

[0088] Energy storage modulus, kPa Loss modulus, kPa Example 1 1.1 0.4 Example 2 1.5 0.6 Example 3 1.8 0.8 Comparative Example 1 1.0 0.4 Comparative Example 2 0.75 0.3

[0089] As can be seen from Table 1, the chitosan hydrogel prepared by the method of the present invention has good mechanical properties, and also has good storage modulus and loss modulus.

[0090] The above description is merely a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, based on the technical teachings provided by the present invention and as common knowledge in the field, other equivalent modifications and improvements can be made, and these should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing chitosan hydrogel, comprising: Step 1: Chitosan powder is mixed sequentially with acetic acid aqueous solution and polyol aqueous solution to obtain mixture A; Step 2: Citral and / or cinnamaldehyde are mixed with a solvent and then mixed with a photoinitiator to obtain mixture B; Step 3: Mix the mixture A and the mixture B in a first mixing and reaction to obtain the reaction product; Step 4: Irradiate the reaction product with ultraviolet light to obtain chitosan hydrogel; The photoinitiator is selected from at least one of lithium phenyl-2,4,6-trimethylbenzoylphosphonate and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone; the amount of the photoinitiator is 0.01-5% by weight of chitosan. The concentration of chitosan in mixture A is 0.5-5% by weight. In the mixture A, the final concentration of the polyol is 0.1-10% by weight. The total weight ratio of citral and / or cinnamaldehyde to chitosan powder is 0.1:1 to 10:

1.

2. The preparation method according to claim 1, characterized in that, The degree of deacetylation of the chitosan powder is ≥85%; and / or, The concentration of acetic acid in the acetic acid aqueous solution is 0.1-3 by weight.

3. The preparation method according to claim 2, characterized in that, The concentration of acetic acid in the acetic acid aqueous solution is 1-2% by weight; and / or, The concentration of chitosan in mixture A is 1-3% by weight.

4. The preparation method according to claim 1, characterized in that, The polyol is selected from at least one of glycerol, butanediol, hexanediol, pentanediol, and polyvinyl alcohol; and / or, The concentration of the polyol in the aqueous polyol solution is 5-20% by weight.

5. The preparation method according to claim 4, characterized in that, The concentration of the polyol in the aqueous polyol solution is 7.2-12% by weight; and / or, In the mixture A, the final concentration of the polyol is 3-6 by weight.

6. The preparation method according to any one of claims 1-5, characterized in that, The solvent is acetone and / or anhydrous ethanol; the concentration of citral and / or cinnamaldehyde in the solvent is 1-50% by weight.

7. The preparation method according to claim 6, characterized in that, The concentrations of citral and / or cinnamaldehyde in the solvent are 5-25% by weight; and / or, The total weight ratio of citral and / or cinnamaldehyde to chitosan powder is 3:1 to 7:

1.

8. The preparation method according to any one of claims 1-5, characterized in that, The amount of photoinitiator used is 0.1-2% by weight of chitosan. And / or, The conditions for ultraviolet irradiation include irradiation at 365nm for 1-6 hours.

9. The preparation method according to claim 8, characterized in that, The conditions for ultraviolet irradiation include irradiation at 365nm for 2-4 hours.

10. The preparation method according to any one of claims 1-5, characterized in that, The conditions for the first mixing include: a temperature of 0-60°C and protection from light; And / or, add mixture B dropwise to mixture A; And / or, the reaction conditions include: a temperature of 20-60°C, in the dark, for a time of 5-60 minutes.

11. The preparation method according to claim 10, characterized in that, The conditions for the first mixing include: a temperature of 10-40°C; And / or, the dripping rate is 5-10 seconds / drop; And / or, the reaction conditions include a time of 10-40 minutes.

12. Chitosan hydrogel obtained by the preparation method according to any one of claims 1-11.

13. A method for preparing chitosan dry gel, comprising: The chitosan hydrogel obtained by the method of preparing chitosan hydrogel according to any one of claims 1-11 or the chitosan hydrogel according to claim 12 is soaked in distilled water and then freeze-dried.

14. The preparation method according to claim 13, characterized in that, The soaking conditions include: soaking time of 2-4 days, with distilled water changed 2-4 times a day; And / or, the freeze-drying conditions include: a temperature of -40 to -60°C and a time of 24 to 48 hours.

15. Chitosan dry gel obtained by the preparation method according to claim 13 or 14.

16. The method for preparing chitosan hydrogel according to any one of claims 1-11, the chitosan hydrogel according to claim 12, the method for preparing chitosan dry gel according to claim 13 or 14, or the application of chitosan dry gel according to claim 15.

17. The application according to claim 16, characterized in that, Applications in biomedicine.

Citation Information

Patent Citations

  • Preparation method of chitosan / polyvinyl alcohol hydrogel dressing

    CN111234266A

  • Preparation method of chitosan gel with high water absorbability

    CN113512206A