A sealing material and sealing method for an aluminizing box used in a powder pack aluminizing process

By using low-melting-point inorganic materials and a sealing method that forms an oxide film through pre-oxidation, the problems of gas discharge and oxidation of the aluminizing agent in the aluminizing box at high temperatures were solved, thereby improving the aluminizing effect and making the aluminizing box easier to open.

CN117167481BActive Publication Date: 2026-11-24ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310917206.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2026-11-24
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

Existing sealing methods for aluminizing boxes are insufficient to effectively expel gas under high-temperature conditions, while also preventing the aluminizing agent from oxidizing and burning off, as well as the oxidation of active surfaces, resulting in poor aluminizing performance.

Method used

Low-melting-point inorganic materials are used as the sealing material for the aluminizing box. An oxide film is formed through pre-oxidation, and its melting temperature and thermal expansion coefficient are controlled to form a liquid seal during the aluminizing process, so as to facilitate the smooth discharge of gas and protect the aluminizing agent.

Benefits of technology

It effectively prevents the aluminizing agent from oxidizing, ensuring the aluminizing effect. The aluminizing box is easy to open, avoiding the sealing failure and oxidation problems caused by gas expansion in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117167481B_ABST
    Figure CN117167481B_ABST
Patent Text Reader

Abstract

This application relates to the field of metal surface treatment technology, and more particularly to a sealing material and sealing method for an aluminizing box used in powder embedding aluminizing process; the sealing material comprises a low-melting-point inorganic material, the melting temperature of which is 400℃~500℃, and the coefficient of thermal expansion of which is 21×10⁻⁶. ‑7 ℃ ‑1 ~73×10 ‑7 ℃ ‑1 During the aluminizing heating process, the low-melting-point inorganic material can melt into a liquid state, and as the temperature rises, the viscosity of the low-melting-point inorganic material changes, thereby providing liquid seal protection at the interface of the aluminizing box. This allows the gas generated inside the aluminizing box to be smoothly discharged through the low-melting-point inorganic material after the viscosity change, while avoiding the oxidation and burning of the aluminizing agent and the oxidation of the active surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal material surface treatment technology, and in particular to a sealing material and sealing method for an aluminizing box used in powder embedding aluminizing process. Background Technology

[0002] Powder embedding aluminizing is a method of surface aluminizing by placing the workpiece and powdered aluminizing agent together in a sealed aluminizing chamber and then performing processes such as heating, holding, and diffusion annealing. The specific principle involves placing the metal workpiece in an aluminizing agent containing aluminum and heating it to a certain temperature. After holding it for an appropriate time, the active atoms of aluminum produced by the thermal decomposition of the aluminizing agent are adsorbed onto the surface of the workpiece and diffuse into the surface layer of the workpiece, thereby changing the chemical composition, structure, and properties of the workpiece surface layer, achieving the effect of high-temperature oxidation resistance and corrosion resistance.

[0003] Since the embedding aluminizing temperature is 850℃~1050℃, it is necessary to ensure complete isolation between the aluminizing agent and oxygen during this process. Once oxygen comes into contact with the aluminizing agent, the highly active aluminizing agent will be directly oxidized, preventing aluminum from diffusing to the surface of the workpiece and causing the embedding aluminizing process to fail.

[0004] Currently, there are two main traditional sealing methods for aluminizing boxes. One method involves introducing a protective atmosphere (H2 or Ar) during the aluminizing process. This method not only requires high sealing of the aluminizing heating equipment but also consumes a large amount of protective gas, increasing the cost of aluminizing. The other method involves pre-sealing the aluminizing box with a high-temperature sealant. While this method can effectively seal the aluminizing box at room temperature, under high-temperature conditions, the volume of gas expands after the aluminizing agent decomposes, generating a large amount of gas that can break open the high-temperature sealant. This leads to significant oxidation of the aluminizing agent, severely affecting the aluminizing effect. Therefore, providing a sealing material for aluminizing boxes used in powder embedding aluminizing processes that allows for the smooth discharge of gas generated inside the aluminizing box while preventing oxidation and burn-off of the aluminizing agent and oxidation of the active surface is a pressing technical problem that needs to be solved. Summary of the Invention

[0005] This application provides a sealing material and sealing method for an aluminizing box used in powder embedding aluminizing process, which solves the problem that the traditional sealing method of aluminizing box in the prior art is difficult to allow the gas generated in the aluminizing box to be discharged smoothly, while also avoiding the oxidation and burning of the aluminizing agent and the oxidation of the active surface.

[0006] In a first aspect, this application provides a sealing material for an aluminizing box used in powder embedding aluminizing process. The sealing material comprises a low-melting-point inorganic substance with a melting temperature of 400℃ to 500℃ and a coefficient of thermal expansion of 21 × 10⁻⁶. -7 ℃ -1 ~73×10-7 ℃ -1 .

[0007] Optionally, the viscosity of the low-melting-point inorganic material at temperatures above 600°C is ≤10 Pa·S.

[0008] Optionally, the softening temperature of the low-melting-point inorganic material is 300℃~400℃.

[0009] Optionally, the low-melting-point inorganic material is at least one selected from phosphates, borates, vanadates, and bismuthates.

[0010] Optionally, the chemical composition of the low-melting-point inorganic material may also include at least one of Al2O3, Si2O3, Na2O, K2O, CaO, ZnO, SnO, TeO2, and BaO.

[0011] Secondly, this application provides a sealing method for an aluminizing box used in powder embedding aluminizing process, the sealing method comprising:

[0012] The sealing material described in the first aspect is used to fill the interface of the aluminizing box, and then pre-oxidation is performed before sealing the aluminizing box to obtain a sealed aluminizing box.

[0013] Optionally, the thickness of the sealing material used for sealing is 5mm to 30mm.

[0014] Optionally, the pre-oxidation temperature is 500℃~650℃, and the pre-oxidation time is 1h~5h.

[0015] Optionally, the chemical composition of the oxide film formed by the pre-oxidation includes at least one of Fe3O4, FeO, and a mixture of Fe3O4 and FeO.

[0016] Optionally, the thickness of the oxide film formed by the pre-oxidation is 20 μm to 300 μm.

[0017] The technical solutions provided in this application have the following advantages compared with the prior art:

[0018] This application provides a sealing material for an aluminizing box used in a powder-embedded aluminizing process. By using a low-melting-point inorganic material as the sealing medium for the aluminizing box and controlling the specific melting temperature and thermal expansion coefficient of the low-melting-point inorganic material, and since the embedding and aluminizing temperature is 850℃~1050℃, the low-melting-point inorganic material can melt into a liquid state during the aluminizing heating process. As the temperature increases, the viscosity of the low-melting-point inorganic material changes, thereby providing liquid seal protection for the interface of the aluminizing box. This facilitates the smooth discharge of gas generated inside the aluminizing box through the low-melting-point inorganic material after the viscosity change, while avoiding the oxidation and burning of the aluminizing agent and the oxidation of the active surface. Attached Figure Description

[0019] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0020] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 A schematic flowchart illustrating the sealing method of the aluminizing box for the powder embedding aluminizing process provided in this application embodiment;

[0022] Figure 2 A schematic diagram of an aluminized box structure formed by a sealing method according to an embodiment of this application;

[0023] Among them, 1-aluminizing box cover, 2-low melting point inorganic material, 3-aluminizing box body, 4-aluminizing agent, 5-workpiece to be aluminized. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0025] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0026] like Figure 1 As shown in the embodiment of this application, a sealing material for an aluminizing box used in powder embedding aluminizing process is provided. The sealing material comprises a low-melting-point inorganic material with a melting temperature of 400℃~500℃ and a coefficient of thermal expansion of 21×10⁻⁶. -7 ℃ -1 ~73×10 -7 ℃ -1 .

[0027] In this embodiment, the specific melting temperature of the low-melting-point inorganic material is controlled. Since the active aluminum source in the aluminizing agent is easily oxidized and consumed above 500°C, and generates a certain amount of gas, controlling the melting temperature of the low-melting-point inorganic material can ensure a good liquid sealing effect during the aluminizing agent reaction process.

[0028] In some alternative embodiments, the viscosity of the low-melting-point inorganic material above 600°C is ≤10 Pa·s.

[0029] In this embodiment, the viscosity of the low-melting-point inorganic material is controlled at a temperature above 600°C. Since the high-temperature gas generated in the aluminizing chamber can be smoothly discharged within this temperature range, and the low-melting-point inorganic material can form a liquid sealing material of sufficient thickness at a temperature above 600°C, the oxidation of the aluminizing agent can be prevented.

[0030] In some alternative embodiments, the softening temperature of the low-melting-point inorganic material is 300°C to 400°C.

[0031] In this embodiment, the specific softening temperature of the low-melting-point inorganic material is controlled. Since the chloride of the aluminizing agent gradually begins to decompose above 300°C and its volume gradually expands, it is necessary to soften synchronously within this temperature to ensure the sealing of the aluminizing box in the later stage. This allows the low-melting-point inorganic material to form a liquid sealing material to seal the aluminizing box.

[0032] In some alternative embodiments, the low-melting-point inorganic material is at least one of phosphate, borate, vanadate, and bismuthate.

[0033] In this embodiment, the specific composition of the low-melting-point inorganic material is controlled so that the overall composition of the low-melting-point inorganic material is mainly low-melting-point glass, thereby ensuring that the melting temperature and thermal expansion coefficient of the low-melting-point inorganic material meet expectations.

[0034] In some alternative embodiments, the chemical composition of the low-melting-point inorganic material further includes at least one of Al2O3, Si2O3, Na2O, K2O, CaO, ZnO, SnO, TeO2, and BaO.

[0035] In this embodiment, the specific chemical composition of the low-melting-point inorganic material is further controlled, utilizing Al2O3 and Si2O3 to reduce the crystallization tendency and crystallization rate of the glass, and to improve the thermal and chemical stability of the glass melt.

[0036] MgO, CaO, ZnO, TeO2 and BaO are then used to accelerate the melting rate of the glass, improve the wettability of the molten glass with the metal material, and enhance the high-temperature stability of the molten glass.

[0037] Since Na₂O and K₂O are network oxides of the glassy structure, and Na+ and K + Located within the cavities of the glass network, the addition of Na₂O and K₂O provides free oxygen and increases oxygen bridges in the glass composition, thereby breaking bonds, reducing the viscosity of the glass and making it easier to melt. They act as good fluxes for the glass. Simultaneously, the addition of Na₂O and K₂O not only increases the coefficient of thermal expansion of the glass but also reduces its room temperature mechanical strength, facilitating the separation of the sealing cap from the casing.

[0038] Based on a general inventive concept, embodiments of this application provide a sealing method for an aluminizing box used in powder embedding aluminizing processes, the sealing method comprising:

[0039] S1. The sealing material is used to fill the interface of the aluminizing box, and then pre-oxidation is performed before sealing the aluminizing box to obtain a sealed aluminizing box.

[0040] In this embodiment of the application, by first filling with a sealing material and then pre-oxidizing, the sealing material can form an oxide film on the surface of the aluminizing box in advance, thereby improving the wettability between the surface of the aluminizing box and the sealing medium and improving the sealing effect.

[0041] This method is based on the above-mentioned sealing material. The specific composition of the sealing material can be referred to in the above embodiments. Since this method adopts some or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated here.

[0042] In some alternative embodiments, the thickness of the sealing material is 5 mm to 30 mm.

[0043] In this embodiment, controlling the specific thickness of the sealing material during filling allows for the formation of a sufficiently thick liquid sealing material during the aluminizing process, thereby ensuring the liquid sealing effect. At the same time, the shell thickness of the solidified glass body formed after aluminizing is moderate, facilitating the opening of the aluminizing box after aluminizing is completed.

[0044] When the thickness of the sealing material is less than 5mm, the liquid surface after the sealing material melts during the embedding and aluminizing process will be too thin to achieve a liquid sealing effect; when the thickness of the sealing material is greater than 30mm, the glass shell surface after solidification at the end of the embedding and aluminizing process will be too thick and difficult to break and peel off.

[0045] In some optional embodiments, the pre-oxidation temperature is 500°C to 650°C, and the pre-oxidation time is 1 hour to 5 hours.

[0046] In this embodiment, controlling the specific temperature and time of pre-oxidation can initially soften the low-melting-point inorganic matter in the sealing material, and at the same time, it can form iron oxide on the surface of the aluminizing box. The iron oxide can better form a sealing surface with the low-melting-point inorganic matter, thereby facilitating the airtight sealing at the interface of the aluminizing box.

[0047] In some alternative embodiments, the chemical composition of the oxide film formed by the pre-oxidation includes at least one of Fe3O4, FeO, and a mixture of Fe3O4 and FeO.

[0048] In the previous embodiments of this application, controlling the specific composition of the oxide film formed in the pre-oxidation stage of the aluminizing box can enable the oxide film to form a sealing surface with low-melting-point inorganic materials, thereby facilitating the airtight sealing of the aluminizing box interface.

[0049] In some optional embodiments, the oxide film formed by the pre-oxidation has a thickness of 20 μm to 300 μm.

[0050] In this embodiment, controlling the specific thickness of the oxide film formed by pre-oxidation can improve the wettability between the metal surface and the molten low-melting-point inorganic material, thereby improving the sealing performance of the aluminizing box. When the oxide film thickness is less than 20 μm, the wettability between the metal surface of the aluminizing box and the molten glass melt is not significantly improved. When the oxide film thickness is greater than 300 μm, some loose and porous oxide film will remain on the metal surface of the aluminizing box, causing sealing failure.

[0051] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national standards. If there is no corresponding national standard, then general international standards, conventional conditions, or conditions recommended by the manufacturer are followed.

[0052] Example 1

[0053] The weighed Bi2O3, B2O3, K2O, P2O5, ZnO, and Al2O3 were placed in a mortar and ground and mixed thoroughly. Then, the mixture was placed in a muffle furnace and heated to 300°C at a rate of 5°C / min and held for 1 hour. After heating to 900°C at a rate of 8°C / min and holding for 2 hours, the mixture was removed and quenched in water to obtain a transparent glass body.

[0054] Water-quenched glass is ball-milled into powder to obtain low-melting-point inorganic materials. The ball-milling process includes a ball-to-material ratio of 3:1, a ball mill speed of 150 r / min, and a ball-milling time of 45 min.

[0055] Aluminized boxes are made of steel, such as Figure 2As shown, the aluminizing box consists of two parts: the box body and the box cover. The aluminizing box is pre-oxidized in a muffle furnace at a temperature of 600℃ for 1.5h. The resulting oxide film has the composition of Fe3O4 and FeO and a thickness of 180μm.

[0056] The aluminizing agent and the workpiece to be aluminized are placed into the aluminizing box after pre-oxidation treatment. The sealed groove of the box is filled with low-melting-point inorganic material with a filling thickness of 15 mm. Then the aluminizing box is covered and solid powder embedding aluminization is carried out in a muffle furnace at a temperature of 950℃ for 5 hours. Then it is cooled with the furnace. During the aluminizing heating process, the low-melting-point inorganic material filled in the sealed groove melts into liquid glass. As the temperature rises, the viscosity of the liquid glass decreases to below 8 Pa·S. Therefore, the connection of the aluminizing box can be liquid-sealed for protection. At this stage, it can ensure the smooth discharge of gas generated in the aluminizing box and avoid oxidation and burn-off of the aluminizing agent and oxidation of the active surface.

[0057] After the aluminizing box cools to room temperature, tap the top cover of the aluminizing box with a hammer. After the solidified low-melting-point inorganic matter in the sealed groove breaks, the workpiece can be easily removed, completing the solid embedding aluminizing. The effective aluminizing layer depth of the workpiece after aluminizing can reach 200μm, and there is no oxidation or peeling phenomenon.

[0058] Example 2

[0059] Weigh out V2O5, P2O5, Sb2O3, SiO2, and K2O, grind them thoroughly and mix them evenly in a mortar, then place them in a muffle furnace, raise the temperature to 320℃ at a rate of 6℃ / min and hold for 1 hour, then raise the temperature to 950℃ at a rate of 9℃ / min and hold for 2 hours, then take them out and quench them in water to obtain a transparent glass body.

[0060] Water-quenched glass is ball-milled into powder to obtain low-melting-point inorganic materials. The ball-milling process includes a ball-to-material ratio of 3:1, a ball mill speed of 140 r / min, and a ball-milling time of 50 min.

[0061] Aluminized boxes are made of steel, such as Figure 2 As shown, the aluminizing box consists of two parts: the box body and the box cover. The aluminizing box is pre-oxidized in a muffle furnace at a temperature of 580℃ for 1.5 hours. The resulting oxide film consists of Fe3O4 and FeO with a thickness of 160μm.

[0062] The aluminizing agent and the workpiece to be aluminized are placed into the aluminizing box after pre-oxidation treatment. The sealed groove of the box is filled with low-melting-point inorganic material with a filling thickness of 20 mm. Then the aluminizing box is covered and solid powder embedding aluminization is carried out in a muffle furnace at a temperature of 965℃ for 5 hours. Then it is cooled with the furnace. During the aluminizing heating process, the low-melting-point inorganic material filled in the sealed groove melts into liquid glass. As the temperature rises, the viscosity of the liquid glass decreases to below 7 Pa·S. Therefore, the connection of the aluminizing box can be liquid-sealed for protection. At this stage, it can ensure the smooth discharge of gas generated in the aluminizing box and avoid oxidation and burn-off of the aluminizing agent and oxidation of the active surface.

[0063] After the aluminizing chamber cools to room temperature, tap the top cover of the aluminizing chamber with a hammer. After the solidified low-melting-point inorganic matter in the sealed groove breaks, the workpiece can be easily removed, completing the solid embedding aluminizing. The effective aluminizing layer depth of the workpiece after aluminizing can reach 270μm, and there is no oxidation or peeling phenomenon.

[0064] Example 3

[0065] Weigh out P2O5, SnO, ZnO, NaO, and CaO, place them in a mortar and grind them thoroughly until they are evenly mixed. Then place them in a muffle furnace and heat them to 350°C at a rate of 5°C / min and hold for 1 hour. Then heat them to 950°C at a rate of 8°C / min and hold for 1.5 hours. After that, take them out and quench them in water to obtain a transparent glass.

[0066] Water-quenched glass is ball-milled into powder to obtain low-melting-point inorganic materials. The ball-milling process includes a ball-to-material ratio of 3:1, a ball mill speed of 150 r / min, and a ball-milling time of 60 min.

[0067] The aluminizing box is made of steel and consists of a box body and a box cover. The aluminizing box is pre-oxidized in a muffle furnace at a temperature of 550℃ for 2 hours. The resulting oxide film has the composition of Fe3O4 and FeO and a thickness of 130μm.

[0068] The aluminizing agent and the workpiece to be aluminized are placed into the aluminizing box after pre-oxidation treatment. The sealed groove of the box is filled with low-melting-point inorganic material with a filling thickness of 10 mm. Then the aluminizing box is covered and solid powder embedding aluminization is carried out in a muffle furnace at a temperature of 940℃ for 6 hours. Then it is cooled with the furnace. During the aluminizing heating process, the low-melting-point inorganic material filled in the sealed groove melts into liquid glass. As the temperature rises, the viscosity of the liquid glass decreases to below 8.5 Pa·S. Therefore, the connection of the aluminizing box can be liquid-sealed for protection. At this stage, it can ensure the smooth discharge of gas generated in the aluminizing box and avoid oxidation and burn-off of the aluminizing agent and oxidation of the active surface.

[0069] After the aluminizing box cools to room temperature, tap the top cover of the aluminizing box with a hammer. After the solidified low-melting-point inorganic matter in the sealed groove breaks, the workpiece can be easily removed, completing the solid embedding aluminizing. The effective aluminizing layer depth of the workpiece after aluminizing can reach 180μm, and there is no oxidation or peeling phenomenon.

[0070] Example 4

[0071] Weigh out B2O3, SiO2, ZnO, Al2O3, and MgO, grind them thoroughly and mix them evenly in a mortar, then place them in a muffle furnace, raise the temperature to 300℃ at a rate of 5℃ / min and hold for 2 hours, then raise the temperature to 900℃ at a rate of 7℃ / min and hold for 2 hours, then take them out and quench them in water to obtain a transparent glass body.

[0072] Water-quenched glass is ball-milled into powder to obtain low-melting-point inorganic materials. The ball-milling process includes a ball-to-material ratio of 3:1, a ball mill speed of 170 r / min, and a ball-milling time of 40 min.

[0073] The aluminizing box is made of 45# steel and consists of a box body and a box cover. The aluminizing box is pre-oxidized in a muffle furnace at a temperature of 620℃ for 0.5h. The resulting oxide film has the composition of Fe3O4 and FeO and a thickness of 150μm.

[0074] The aluminizing agent and the workpiece to be aluminized are placed into the aluminizing box after pre-oxidation treatment. Low-melting-point inorganic material with a thickness of 25 mm is filled into the sealed groove of the box. Then the aluminizing box is covered and solid powder embedding aluminization is carried out in a muffle furnace at a temperature of 950℃ for 8 hours. Then it is cooled with the furnace. During the aluminizing heating process, the low-melting-point inorganic material filled in the sealed groove melts into liquid glass. As the temperature rises, the viscosity of the liquid glass decreases to below 8 Pa·S. Therefore, the connection of the aluminizing box can be liquid-sealed for protection. At this stage, it can ensure the smooth discharge of gas generated in the aluminizing box and avoid oxidation and burn-off of the aluminizing agent and oxidation of the active surface.

[0075] After the aluminizing chamber cools to room temperature, tap the top cover of the aluminizing chamber with a hammer. After the solidified low-melting-point inorganic matter in the sealed groove breaks, the workpiece can be easily removed, completing the solid embedding aluminizing. The effective aluminizing layer depth of the workpiece after aluminizing can reach 250μm, and there is no oxidation or peeling phenomenon.

[0076] Comparative Example 1

[0077] Comparative Example 1 and Example 1 will be compared. The difference between Comparative Example 1 and Example 1 is as follows:

[0078] Replacing the sealing material with a phosphorus-containing material, such as using metallic phosphorus instead of low-melting-point inorganic materials for sealing the aluminizing box, can achieve good liquid sealing and venting effects at low temperatures due to the low melting point of metallic phosphorus. However, as the aluminizing temperature gradually increases, phosphorus reacts with carbon in the steel material to produce Widmanstätten, which significantly reduces the strength of the sealing groove of the aluminizing box, causing high-temperature deformation of the sealing groove and leading to sealing failure. At the same time, phosphorus is easily oxidized by air at high temperatures to form gray-black lead oxide, resulting in continuous oxidation and loss of metallic phosphorus. This not only reduces the liquid seal height and the liquid seal effect, but also causes a large amount of harmful lead and lead oxide to volatilize under high-temperature conditions, resulting in personal injury and environmental pollution.

[0079] Comparative Example 2

[0080] Comparative Example 2 and Example 1 will be compared. The difference between Comparative Example 2 and Example 1 is as follows:

[0081] Replacing the sealing material with a Sn-containing material, such as using metallic Sn instead of low-melting-point inorganic materials for sealing the aluminizing tank, can achieve good liquid sealing and venting effects at low temperatures due to the low melting point of metallic Sn. However, as the aluminizing temperature gradually increases, the molten metallic Sn diffuses with the steel material, causing the compound FeSn2 to grow from the Sn phase. This leads to the gradual alloying of metallic Sn, forming an Fe-Sn alloy, which results in a strong metallurgical bond between the aluminizing tank body and the aluminizing tank cover within the sealing groove.

[0082] At the same time, the coefficients of thermal expansion of the two are very close, and they still have a high bonding strength after cooling to room temperature, making it difficult to separate the sealing cover of the aluminized box from the box body. The aluminized box body can only be opened by destructive separation methods such as cutting, which makes it difficult to promote its application.

[0083] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0084] (1) The sealing material of the aluminizing box for powder embedding aluminizing process provided in the embodiment of this application uses a low melting point inorganic material as the sealing medium of the aluminizing box. During the aluminizing heating process, the low melting point inorganic material melts into a liquid state, and as the temperature rises, the viscosity of the sealing medium changes, which provides liquid seal protection for the connection of the aluminizing box. This can ensure the smooth discharge of the gas generated in the aluminizing box and avoid the oxidation and burning of the aluminizing agent and the oxidation of the active surface.

[0085] (2) The sealing material of the aluminizing box for the powder embedding aluminizing process provided in this application uses a low-melting-point inorganic material as the sealing medium of the aluminizing box. After the aluminizing process is completed, the expansion coefficients of the inorganic sealing medium and the metal aluminizing box are significantly different, and the room temperature bonding strength of the two is low, which makes it easy for the sealing cover of the aluminizing box to separate from the box body. Traditional low-melting-point liquid sealing metals often use Pb sealing or Sn sealing. The expansion coefficients of the liquid sealing metal and the aluminizing are close, and the interdiffusion of elements between the metals is easy. The metallurgical bond formed by the two makes it difficult to separate the sealing cover of the aluminizing box from the box body.

[0086] (3) The sealing method of the aluminizing box for powder embedding aluminizing process provided in this application embodiment is to pre-oxidize the aluminizing box before sealing, and use the pre-oxidation to form an oxide film on its surface, thereby improving the wettability of the aluminizing box surface and the sealing medium, and thus improving the high-temperature sealing effect of the aluminizing box.

[0087] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0088] In this application, unless otherwise stated, directional terms such as "upper" and "lower" specifically refer to the drawing directions in the accompanying drawings. Furthermore, in the description of this application, terms such as "comprising" and "including" mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than one" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.

[0089] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A sealing material for an aluminizing box used in powder embedding aluminizing process, characterized in that, The aluminizing temperature for the embedding process is 850℃~1050℃. The sealing material comprises a low-melting-point inorganic substance with a melting temperature of 400℃~500℃ and a coefficient of thermal expansion of 21×10⁻⁶. -7 ℃ -1 ~73×10 -7 ℃ -1 The low-melting-point inorganic material has a viscosity ≤10 Pa·S above 600℃, a softening temperature of 300℃~400℃, and is at least one of borates, vanadates and bismuthates. The chemical composition of the low-melting-point inorganic material also includes at least one of Al2O3, Si2O3, Na2O, K2O, CaO, ZnO, SnO, TeO2 and BaO.

2. A sealing method for an aluminizing box used in powder embedding aluminizing process, characterized in that, The sealing method includes: The sealing material as described in claim 1 is used to fill the interface of the aluminizing box, and then pre-oxidation is performed before sealing the aluminizing box to obtain a sealed aluminizing box. The thickness of the low melting point inorganic material used for filling is 5mm to 30mm, the temperature of the pre-oxidation is 500℃ to 650℃, and the time of the pre-oxidation is 1h to 5h. The chemical composition of the oxide film formed by the pre-oxidation includes at least one of Fe3O4, FeO, and a mixture of Fe3O4 and FeO; the thickness of the oxide film formed by the pre-oxidation is 20 μm to 300 μm.

Citation Information

Patent Citations

  • Pretreatment method for improving lead-bismuth corrosion resistance of ferrite-martensite steel

    CN112646957A

  • Method of using low melting point fusant as sealing material to prevent evaporation of lead oxide

    CN1442390A

  • Sealing material

    JP2005035840A