A method for improving the coercivity of sintered neodymium-iron-boron magnets by low-temperature grain boundary diffusion under the action of a pulse electric field

CN117174423BActive Publication Date: 2026-11-24FUZHOU UNIV +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311367302.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-21
Publication Date
2026-11-24
Estimated Expiration
2043-10-21

AI Technical Summary

Technical Problem

但是这些含有Dy/Tb元素的合金或化合物熔点高,扩散难度大,扩散效率低,为保证扩散效果,常常进行多次重复扩散或长时间扩散,不利于降低生产成本和缩短生产周期

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117174423B_ABST
    Figure CN117174423B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing sintered NdFeB magnets with improved coercivity through low-temperature grain boundary diffusion under a pulsed electric field. The preparation method of this invention is as follows: First, R... a M b (a+b=100, wt%) The alloy, as a grain boundary diffusion alloy, has a melting point <500℃. R is one or more of Pr, Nd, Gd, Tb, Dy, and Ho, and M is one or more of Ga, Sn, In, and Bi. Then, sintered NdFeB magnets are embedded in R. a M b In the alloy particles, heated to R under argon protection. a M b Alloy particles are melted and diffused under a pulsed electric field, and the diffused magnet is then aged. This invention can effectively improve the coercivity of sintered NdFeB magnets and has advantages such as low diffusion temperature, high diffusion efficiency, short production cycle, and high utilization rate of heavy rare earth elements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of rare earth magnetic material preparation technology, and relates to a method for preparing sintered NdFeB magnets by improving the coercivity of the magnets through low-temperature grain boundary diffusion under the action of a pulsed electric field. Background Technology

[0002] Neodymium iron boron (NdFeB) is the third-generation rare-earth permanent magnet material with the highest magnetic energy product and can be mass-produced. It is widely used in numerous fields such as electronics, automotive, medical equipment, and energy transportation. Although sintered NdFeB magnets have a high magnetic energy product, the intrinsic coercivity of actual magnets is far lower than their theoretical value, making them unsuitable for high-temperature operating environments.

[0003] The traditional way to improve the coercivity of NdFeB magnets is to directly add alloys or compounds containing heavy rare earth elements Dy or Tb during the smelting process to replace the main Nd2Fe phase. 14 In B, Nd atoms form a (Nd,Dy / Tb)2Fe with a high anisotropic field. 14 The B phase significantly enhances the coercivity of NdFeB magnets; however, due to the antiferromagnetic coupling between heavy rare earth Dy and Tb atoms and Fe atoms, the addition of heavy rare earth elements will inevitably reduce the remanence of the magnet. r and maximum magnetic energy product BH (max) On the other hand, heavy rare earth elements are scarce in the Earth's crust and have high raw material prices. How to achieve efficient utilization of heavy rare earth elements has long been a hot topic of research. To address this, grain boundary diffusion technology has been developed in recent years in an attempt to resolve the contradiction between improving the coercivity of magnets and increasing the utilization rate of heavy rare earth elements.

[0004] Existing grain boundary diffusion treatment technologies mainly employ methods such as slurry coating, electrophoretic deposition, vapor deposition, and screen printing to first attach alloys or compounds containing Dy / Tb elements (such as Dy2O3, DyF3, TbF3, etc.) to the magnet surface. Then, diffusion heat treatment is performed within a certain temperature range, allowing rare earth elements to diffuse along the grain boundaries to the surface of the main phase grains, forming (Nd,Dy / Tb)2Fe. 14B-shell structures enhance the anisotropic field on the surface of the main phase grains, thereby improving the coercivity of the magnet. However, these alloys or compounds containing Dy / Tb elements have high melting points, making diffusion difficult and inefficient. To ensure diffusion effectiveness, multiple repeated diffusion processes or long-term diffusion are often required, which is detrimental to reducing production costs and shortening the production cycle. Furthermore, high diffusion temperatures can generate excessive liquid phase at grain boundaries, leading to an excessively thick heavy rare earth shell (≥3μm) on the surface of the main phase grains, or even an anti-shell structure. This hinders the full utilization of heavy rare earth elements and significantly reduces the remanence of the magnet. For example, the English journal *ActaMaterialia* (2019, Vol. 172, pp. 139-149) reported that Nd... 31.8 Fe 66.0 B 1.0 Cu 0.1 Al 0.15 Co 0.9 Ga 0.05 (wt.%) A heavy rare earth shell with a thickness of 5 μm was formed after the magnet was diffused with Dy vapor at 950 °C for 4 hours. The English journal ScriptaMaterialia (2019, Vol.163, pp.40-43) reported that when a thin layer of Dy or Tb metal was coated on the surface of a commercial N52 NdFeB magnet and then diffused at 900 °C for 0.5 to 5 hours, an anti-shell structure was observed in the magnet. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention aims to improve the coercivity of NdFeB magnets, increase the utilization rate of heavy rare earth elements, and shorten the production cycle. It utilizes the advantages of low-melting-point alloy melt diffusion combined with pulsed electric field treatment to effectively improve the grain boundary diffusion efficiency of heavy rare earth elements. This results in the formation of a relatively ideal shell structure (shell thickness < 3 μm) on the surface of the main phase grains, thereby improving the coercivity of sintered NdFeB magnets and increasing the utilization rate of heavy rare earth elements.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing sintered NdFeB magnets with improved coercivity through low-temperature grain boundary diffusion under pulsed electric field, the specific process steps are as follows:

[0008] (1) Low melting point R is prepared by induction melting or electric arc melting under pure argon protection. a M b Alloy ingot, R a M b The alloy has a melting point below 500℃, and is therefore classified as a grain boundary diffusion alloy. R a M bThe mass percentage of the alloy is a+b=100, a≥3, R is one or more of Pr, Nd, Gd, Tb, Dy, Ho, and the content of Dy or Tb in the total content of R is not less than 60wt%, M is one or more of Ga, Sn, In, Bi, and the sum of Ga and Sn in the total content of M is not less than 70wt%.

[0009] (2) R a M b The alloy ingot is crushed into particles with a diameter of less than 3 mm, and then placed in a corundum crucible. Next, the sintered NdFeB magnet to be diffused and the graphite electrode plate are embedded together in the R... a M b In the alloy particles, the area of ​​the graphite electrode plate should be larger than that of the magnet. The sintered NdFeB magnet and the graphite electrode plate are connected to a pulse power supply. The negative terminal of the pulse power supply is connected to the sintered NdFeB magnet, and the positive terminal is connected to the graphite electrode plate.

[0010] (3) Under pure argon protection, the corundum crucible is heated to 500–650°C. The pulsed power supply connecting the sintered NdFeB magnet and the graphite electrode is turned on, and melt grain boundary diffusion treatment is performed under the action of the pulsed electric field for 1–5 hours. The current density of the pulsed power supply is 5–20 A / cm². 2 The frequency is 50–150 Hz, and the duty cycle is 10%–30%.

[0011] (4) After diffusion treatment, the sintered NdFeB magnet is removed and the residual R on the surface is cleaned. a M b The alloy is then heated to 450–550°C under pure argon protection for 1–3 hours to obtain the final sintered NdFeB magnet.

[0012] Furthermore, the low melting point R... a M b The alloy includes Tb3Dy1Ga 96 Tb3Ga 97 、Dy3Ga 97 、Tb3Gd2Ga 13 Sn 82 Tb5Ga 13 Sn 82 、Dy5Ho1Ga 72 Bi 22 Tb3Pr 0.5 Nd 1.5 Ga 95 Dy5Pr 0.5 Nd 1.5 Ga 80 In 13 .

[0013] The advantages of this invention are as follows:

[0014] (1) This invention rationally designs and prepares a low-melting-point alloy, wherein Tb, Dy, and Ho can effectively improve the melting point of Nd2Fe. 14 The anisotropic field on the surface of the B main phase grains, along with Pr, Nd, Gd, Tb, Dy, and Ho, can effectively repair defects in the epitaxial layer on the main phase grain surface. Ga, Sn, In, and Bi elements can effectively lower the melting point of the alloy, making it below 500℃; on the other hand, they can combine with rare earth atoms and Fe atoms, lowering the melting point of the magnet grain boundary phase and improving its wettability, effectively promoting the grain boundary diffusion of rare earth elements.

[0015] (2) In the process of diffusion treatment of low melting point alloy melt, the present invention introduces a pulsed electric field for auxiliary diffusion. The pulsed electric field can activate the liquid grain boundary phase on the surface of the magnet and in the magnet, reduce the diffusion activation energy of grain boundary elements, thereby accelerating the diffusion of R and M elements in the alloy melt into the grain boundary region of sintered NdFeB, improving diffusion efficiency and increasing diffusion depth.

[0016] (3) The present invention can effectively reduce the excessive melting of the surface layer of the main phase grain during the diffusion process, prevent the heavy rare earth shell layer formed on the surface of the main phase grain from being too thick, improve the utilization rate of heavy rare earth elements, and reduce the decrease in the remanence of the magnet after the diffusion process. Attached Figure Description

[0017] Figure 1 Schematic diagram of a pulsed electric field-assisted low-temperature grain boundary diffusion device;

[0018] Figure 2 This is a backscattered electron image of the magnet prepared in Example 1;

[0019] Figure 3 This is a backscattered electron image of the magnet prepared in Comparative Example 1. Detailed Implementation

[0020] The present invention will be further described below with reference to specific embodiments and comparative examples.

[0021] Example 1:

[0022] (1) Take metals Tb, Dy, and Ga with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 3 Dy 1 Ga 96 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0023] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, Hcj =18.20 kOe, (BH) max =47.76 MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Dy1Ga. 96 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Dy1Ga is then processed under pure argon protection. 96 The alloy was heated to a liquid state and then raised to its diffusion temperature of 550°C; a pulse power supply was turned on, with a pulse current density of 10 A / cm². 2 The diffusion process was carried out for 2 hours at a frequency of 100 Hz and a duty cycle of 20%.

[0024] (3) The surface of the diffused magnet was cleaned, and then heated to 480℃ under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 1.

[0025] Pulse electric field assisted melt diffusion device such as Figure 1 As shown. Figure 2 This is the backscattered electron image after diffusion assisted by an external pulsed electric field in this embodiment. After diffusion at the grain boundaries of the low-melting-point alloy assisted by an external pulsed electric field, a clear and continuous heavy rare earth shell is formed on the surface of the main phase grains (e.g., Figure 2 (As indicated by the middle arrow), the thickness of the heavy rare earth shell on the surface of the main phase grain is ≤2.2μm, and the average thickness is ~1.1μm.

[0026] Example 2:

[0027] (1) Take metals Tb and Ga with a purity of 99.5 wt% or higher, and mix them according to the mass percentage Tb3Ga 97 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0028] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, H cj =18.20 kOe, (BH) max =47.76 MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Ga. 97 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Ga is then processed under pure argon protection. 97The alloy was heated to a liquid state and then raised to its diffusion temperature of 550°C; a pulse power supply was turned on, with a pulse current density of 5 A / cm². 2 The diffusion process was carried out for 2 hours at a frequency of 100 Hz and a duty cycle of 20%.

[0029] (3) The diffused magnet underwent surface cleaning and was then heated to 480℃ under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤2.1μm and an average thickness of ~0.9μm.

[0030] Example 3:

[0031] (1) Take metals Dy and Ga with a purity of 99.5 wt% or higher, and mix them according to the mass percentage Dy3Ga 97 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0032] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, H cj =18.20 kOe, (BH) max =47.76 MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Dy3Ga. 97 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy3Ga is then processed under pure argon protection. 97 The alloy was heated to a liquid state and then raised to its diffusion temperature of 500°C; a pulse power supply was turned on, with a pulse current density of 10 A / cm². 2 The diffusion process was carried out for 1 hour at a frequency of 50 Hz and a duty cycle of 10%.

[0033] (3) The diffused magnet underwent surface cleaning and was then heated to 480℃ under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤2.0μm and an average thickness of ~0.8μm.

[0034] Example 4:

[0035] (1) Take metals Tb, Gd, Ga, and Sn with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 3Gd 2Ga 13 Sn 82The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0036] (2) The diffusion magnet used is the commercially available N38SH magnet, with a performance of B. r =12.50kGs, H cj = 20.10 kOe, (BH) max =38.06 MGOe, machined into 12mm×12mm×3mm pieces using wire cutting, with the orientation direction being 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Gd2Ga. 13 Sn 82 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Gd2Ga is then processed under pure argon protection. 13 Sn 82 The alloy was heated to a liquid state and then raised to its diffusion temperature of 600℃; a pulse power supply was turned on, with a pulse current density of 10 A / cm². 2 The diffusion process was carried out for 3 hours at a frequency of 150 Hz and a duty cycle of 30%.

[0037] (3) The diffused magnet underwent surface cleaning and was then heated to 450℃ under pure argon protection for 3 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤2.1μm and an average thickness of ~1.0μm.

[0038] Example 5:

[0039] (1) Take metals Tb, Ga, and Sn with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 5Ga 13 Sn 82 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0040] (2) The diffusion magnet used is the commercially available N38SH magnet, with a performance of B. r =12.50kGs, H cj = 20.10 kOe, (BH) max =38.06 MGOe, machined into 12mm×12mm×3mm pieces using wire cutting, with the orientation direction being 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb5Ga. 13 Sn 82 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb5Ga is then processed under pure argon protection.13 Sn 82 The alloy was heated to a liquid state and then raised to its diffusion temperature of 600℃; a pulse power supply was turned on, with a pulse current density of 12 A / cm². 2 The diffusion process was carried out for 3 hours at a frequency of 100 Hz and a duty cycle of 20%.

[0041] (3) The diffused magnet was surface cleaned and then heated to 450℃ under pure argon protection for 3 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤1.9μm and an average thickness of ~0.9μm.

[0042] Example 6:

[0043] (1) Metals Dy, Ho, Ga, and Bi with a purity of 99.5 wt% or higher are mixed in the following mass percentages: Dy 5 Ho 1 Ga 72 Bi 22 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0044] (2) The diffusion magnet used is the commercially available N38SH magnet, with a performance of B. r =12.50kGs, H cj = 20.10 kOe, (BH) max =38.06 MGOe, wire-cut to a size of 12mm × 12mm × 3mm, with an orientation direction of 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Dy5Ho1Ga. 72 Bi 22 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy5Ho1Ga is then processed under pure argon protection. 72 Bi 22 The alloy was heated to a liquid state and then raised to its diffusion temperature of 600℃; a pulse power supply was turned on, with a pulse current density of 15 A / cm². 2 The diffusion process was carried out for 4 hours at a frequency of 150 Hz and a duty cycle of 20%.

[0045] (3) The diffused magnet was surface cleaned and then aged for 3 hours at 450℃ under pure argon protection. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤1.9μm and an average thickness of ~0.8μm.

[0046] Example 7:

[0047] (1) Take metals Tb, Ga, Pr, and Nd with a purity of 99.5 wt% or higher, and mix them according to the mass percentage of Tb3Pr 0.5 Nd 1.5 Ga 95 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0048] (2) The diffusion magnet is a commercially available N38M magnet with magnetic properties of B. r =12.4kGs, H cj =14.7kOe, (BH) max =37.32MGOe, machined into 12mm×12mm×4.8mm pieces using wire cutting, with the orientation direction at 4.8mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Pr. 0.5 Nd 1.5 Ga 95 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Pr is then subjected to pure argon gas protection. 0.5 Nd 1.5 Ga 95 The alloy was heated to a liquid state and then raised to its diffusion temperature of 650°C; a pulse power supply was turned on, with a pulse current density of 15 A / cm². 2 The diffusion process was carried out for 5 hours at a frequency of 100 Hz and a duty cycle of 30%.

[0049] (3) The diffused magnet was surface cleaned and then aged for 1 hour at 550°C under pure argon protection. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤2.1μm and an average thickness of ~1.0μm.

[0050] Example 8:

[0051] (1) Metals Dy, Pr, Nd, Ga, and In with a purity of 99.5 wt% or higher are mixed in a mass percentage ratio of Dy / Pr / Nd / Ga / In. 0.5 Nd 1.5 Ga 80 In 13 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0052] (2) The diffusion magnet is a commercially available N38M magnet with magnetic properties of B. r =12.4kGs, H cj =14.7kOe, (BH) max=37.32MGOe, machined into 12mm×12mm×4.8mm pieces using wire cutting, with the orientation direction at 4.8mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in a Dy5Pr magnet. 0.5 Nd 1.5 Ga 80 In 13 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate; under pure argon protection, Dy5Pr 0.5 Nd 1.5 Ga 80 In 13 The alloy was heated to a liquid state and then raised to its diffusion temperature of 650°C; a pulse power supply was turned on, with a pulse current density of 20 A / cm². 2 The diffusion process was carried out for 5 hours at a frequency of 150 Hz and a duty cycle of 30%.

[0053] (3) The diffused magnet was surface cleaned and then aged for 1 hour at 550°C under pure argon protection. The final magnetic properties of the magnet are shown in Table 1. The heavy rare earth shell on the surface of the main phase grains is continuous, with a shell thickness ≤2.2μm and an average thickness of ~1.2μm.

[0054] Table 1 lists the magnetic properties of the magnets before and after diffusion in Examples 1-8, as well as their corresponding diffusion and aging process parameters.

[0055] Table 1 shows the magnetic properties of the magnets before and after diffusion in Examples 1-8 and their corresponding process parameters.

[0056]

[0057] As shown in Table 1, the preparation method of the present invention can effectively improve the intrinsic coercivity H of sintered NdFeB magnets of different grades. cj Meanwhile, the residual magnetism B r And the maximum magnetic energy product (BH) max The impact is relatively small.

[0058] Comparative Example 1:

[0059] (1) Take metals Tb, Dy, and Ga with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 3 Dy 1 Ga 96 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0060] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, H cj =18.20 kOe, (BH)max =47.76 MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Dy1Ga. 96 In alloy particles. Tb3Dy1Ga is added under pure argon protection. 96 The alloy was heated to a liquid state and then heated to the diffusion temperature of 550°C, followed by diffusion for 2 hours.

[0061] (3) The surface of the diffused magnet was cleaned, and then heated to 480°C under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0062] In this comparative example, no pulsed electric field was used for assisted diffusion in the melt diffusion process. The backscattered electron image of the magnet after diffusion is as follows: Figure 3 As shown, heavy rare earth shells formed only in certain regions on the surface of the main phase grains (such as...). Figure 3 (As indicated by the middle arrow), the shell is not continuous. Although the composition of the low-melting-point diffusion alloy in this comparative example is the same as that in Example 1, it failed to effectively improve the intrinsic coercivity of the magnet.

[0063] Comparative Example 2:

[0064] (1) Take metals Dy and Ga with a purity of 99.5 wt% or higher, and mix them according to the mass percentage of Dy 0.5 Ga 99.5 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0065] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, H cj =18.20 kOe, (BH) max =47.76MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface is removed by sanding, and then it is embedded in a Dy... 0.5 Ga 99.5 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy is then subjected to pure argon gas protection. 0.5 Ga 99.5 The alloy was heated to a liquid state and then raised to its diffusion temperature of 550°C; a pulse power supply was turned on, with a pulse current density of 5 A / cm². 2 The diffusion process was carried out for 2 hours at a frequency of 100 Hz and a duty cycle of 20%.

[0066] (3) The surface of the diffused magnet was cleaned, and then heated to 480°C under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0067] In this comparative example, the rare earth content of the low-melting-point diffusion alloy is less than that specified in the claims. Although the parameters of its diffusion process and aging process are the same as those in Example 2, it fails to effectively improve the intrinsic coercivity of the magnet.

[0068] Comparative Example 3:

[0069] (1) Take metals Dy and Ga with a purity of 99.5 wt% or higher, and mix them according to the mass percentage Dy3Ga 97 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0070] (2) The diffusion matrix is ​​a commercially available N50H magnet, whose magnetic properties are B. r =13.98kGs, H cj =18.20 kOe, (BH) max =47.76 MGOe, machined into 12mm×12mm×2mm pieces using wire cutting, with an orientation direction of 2mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Dy3Ga. 97 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy3Ga is then processed under pure argon protection. 97 The alloy was heated to a liquid state and then raised to its diffusion temperature of 500°C; a pulse power supply was turned on, with a pulse current density of 1 A / cm². 2 The diffusion was carried out for 0.5 hours at a frequency of 50 Hz and a duty cycle of 10%.

[0071] (3) The surface of the diffused magnet was cleaned, and then heated to 480°C under pure argon protection for 2 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0072] In this comparative example, the diffusion time and pulse current density are lower than those specified in the claims, i.e., a shorter diffusion time and a lower pulse current density are used. Although the low-melting-point diffusion alloy composition and aging process parameters are the same as in Example 3 in this comparative example, they failed to effectively improve the intrinsic coercivity of the magnet.

[0073] Comparative Example 4:

[0074] (1) Take metals Tb, Gd, Ga, and Sn with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 3Gd 2Ga 13Sn 82 The ingredients are batched and placed into a vacuum induction melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0075] (2) The diffusion magnet is a commercially available N38SH magnet, whose magnetic properties are B. r =12.50kGs, H cj = 20.10 kOe, (BH) max =38.06 MGOe, wire-cut into block magnets with dimensions of 12mm × 12mm × 3mm, with an orientation direction of 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Gd2Ga. 13 Sn 82 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Gd2Ga is then processed under pure argon protection. 13 Sn 82 The alloy was heated to a liquid state and then raised to its diffusion temperature of 600℃; a pulse power supply was turned on, with a pulse current density of 50 A / cm². 2 The diffusion was carried out for 10 hours at a frequency of 150 Hz and a duty cycle of 20%.

[0076] (3) The surface of the diffused magnet was cleaned, and then heated to 450°C under pure argon protection for 3 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0077] In this comparative example, the diffusion time and pulse current density are higher than those specified in the claims, i.e., a longer diffusion time and a higher pulse current density are used. Although the low-melting-point diffusion alloy composition and aging process parameters are the same as in Example 4 in this comparative example, they failed to effectively improve the intrinsic coercivity of the magnet.

[0078] Comparative Example 5:

[0079] (1) Take metals Tb, Ga, and Sn with a purity of 99.5 wt% or higher, and mix them in the following mass percentages: Tb 5Ga 13 Sn 82 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0080] (2) The diffusion magnet is a commercially available N38SH magnet, whose magnetic properties are B. r =12.50kGs, H cj = 20.10 kOe, (BH) max=38.06 MGOe, machined into 12mm×12mm×3mm pieces using wire cutting, with the orientation direction being 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb5Ga. 13 Sn 82 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb5Ga is then processed under pure argon protection. 13 Sn 82 The alloy was heated to a liquid state and then raised to its diffusion temperature of 600℃; a pulse power supply was turned on, with a pulse current density of 12 A / cm². 2 The diffusion process was carried out for 3 hours at a frequency of 300 Hz and a duty cycle of 60%.

[0081] (3) The surface of the diffused magnet was cleaned, and then heated to 450°C under pure argon protection for 3 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0082] In this comparative example, the frequency and duty cycle of the pulse current are higher than those specified in the claims, i.e., a higher pulse current frequency and a larger duty cycle are used. Although the low-melting-point diffusion alloy composition and aging process parameters are the same as in Example 5, this comparative example fails to effectively improve the intrinsic coercivity of the magnet.

[0083] Comparative Example 6:

[0084] (1) Metals Dy, Ho, Ga, and Bi with a purity of 99.5 wt% or higher are mixed in the following mass percentages: Dy 5 Ho 1 Ga 72 Bi 22 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0085] (2) The diffusion magnet is a commercially available N38SH magnet, whose magnetic properties are B. r =12.50kGs, H cj = 20.10 kOe, (BH) max =38.06 MGOe, machined into 12mm×12mm×3mm pieces using wire cutting, with the orientation direction being 3mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Dy5Ho1Ga. 72 Bi 22 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy5Ho1Ga is then processed under pure argon protection. 72 Bi 22 The alloy was heated to a liquid state and then raised to its diffusion temperature of 900℃; a pulse power supply was turned on, with a pulse current density of 15 A / cm².2 The diffusion was carried out for 10 hours at a frequency of 150 Hz and a duty cycle of 20%.

[0086] (3) The surface of the diffused magnet was cleaned, and then heated to 450°C under pure argon protection for 3 hours for aging treatment. The final magnetic properties of the magnet are shown in Table 2.

[0087] In this comparative example, the diffusion temperature and diffusion time are higher than those specified in the claims, i.e., a higher diffusion temperature and a longer diffusion time are used. Although the low-melting-point diffusion alloy composition and aging process parameters in this comparative example are the same as in Example 6, they failed to effectively improve the intrinsic coercivity of the magnet.

[0088] Comparative Example 7:

[0089] (1) Take metals Tb, Ga, Pr, and Nd with a purity of 99.5 wt% or higher, and mix them according to the mass percentage of Tb3Pr 0.5 Nd 1.5 Ga 95 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0090] (2) The diffusion magnet is a commercially available N38M magnet, whose magnetic properties are B. r =12.40kGs, H cj =14.70 kOe, (BH) max =37.32MGOe, machined into 12mm×12mm×4.8mm pieces using wire cutting, with the orientation direction at 4.8mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in Tb3Pr. 0.5 Nd 1.5 Ga 95 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Tb3Pr is then subjected to pure argon gas protection. 0.5 Nd 1.5 Ga 95 The alloy was heated to a liquid state and then raised to its diffusion temperature of 650°C; a pulse power supply was turned on, with a pulse current density of 15 A / cm². 2 The diffusion process was carried out for 5 hours at a frequency of 100 Hz and a duty cycle of 30%.

[0091] (3) The surface of the diffused magnet is cleaned. The final magnetic properties of the magnet are shown in Table 2.

[0092] In this comparative example, no aging treatment process was used. Although the composition of the low-melting-point diffusion alloy and the diffusion process parameters were the same as in Example 7, they failed to effectively improve the intrinsic coercivity of the magnet.

[0093] Comparative Example 8:

[0094] (1) Metals Dy, Pr, Nd, Ga, and In with a purity of 99.5 wt% or higher are mixed in a mass percentage ratio of Dy / Pr / Nd / Ga / In. 0.5 Nd 1.5 Ga 80 In 13 The ingredients are batched and placed into a vacuum arc melting furnace. Under the protection of pure argon gas, the raw materials are melted into ingots. The ingots are then removed and crushed into particles with a diameter of less than 3 mm.

[0095] (2) The diffusion magnet used is the commercially available N38M magnet, with performance of B. r =12.40kGs, H cj =14.70 kOe, (BH) max =37.32MGOe, machined into 12mm×12mm×4.8mm pieces using wire cutting, with the orientation direction at 4.8mm. The oxide layer on the magnet surface was removed by sanding, and then it was embedded in a Dy5Pr magnet. 0.5 Nd 1.5 Ga 80 In 13 In the alloy particles, the magnet is connected to the negative terminal of the pulse power supply, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. Dy5Pr is then subjected to pure argon gas protection. 0.5 Nd 1.5 Ga 80 In 13 The alloy was heated to a liquid state and then raised to its diffusion temperature of 650°C; a pulse power supply was turned on, with a pulse current density of 20 A / cm². 2 The diffusion process was carried out for 5 hours at a frequency of 150 Hz and a duty cycle of 30%.

[0096] (3) The surface of the diffused magnet is cleaned and then heated to 600°C under pure argon protection for 4 hours of aging treatment.

[0097] In this comparative example, the aging temperature and aging time are higher than those specified in the claims, i.e., a higher aging temperature and a longer aging time are used. Although the low-melting-point diffusion alloy composition and diffusion process parameters in this comparative example are the same as in Example 8, they failed to effectively improve the intrinsic coercivity of the magnet.

[0098] Table 2 lists the magnetic properties of the magnets before and after diffusion in Comparative Examples 1–8, along with their corresponding diffusion and aging process parameters.

[0099] Table 2 shows the magnetic properties of the magnets before and after diffusion and their corresponding process parameters in Comparative Examples 1–8.

[0100]

[0101] As shown in Table 2, if the low-melting-point alloy composition, diffusion temperature and time, pulse current density, pulse power supply frequency and duty cycle, aging temperature and time, and other parameters are not within the range specified in the claims, the intrinsic coercivity H of the magnet cannot be achieved. cj The effective improvement may even cause residual magnetism B. r And the maximum magnetic energy product (BH) max A significant decrease.

[0102] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing sintered NdFeB magnets with improved coercivity through low-temperature grain boundary diffusion under a pulsed electric field, characterized in that, The preparation method includes the following steps: (1) Low melting point R is prepared by induction melting or electric arc melting under pure argon protection. a M b Alloy ingots were used as grain boundary diffusion source alloys. (2) R a M b The alloy ingot is crushed into particles with a diameter of less than 3 mm, and then placed in a corundum crucible. Next, the sintered NdFeB magnet to be diffused and the graphite electrode plate are embedded together in the R... a M b In the alloy particles, sintered NdFeB magnets and graphite electrode plates are respectively connected to a pulse power supply; (3) Under the protection of pure argon gas, heat the corundum crucible to R. a M b Above the alloy's melting point, turn on the pulsed power supply connecting the sintered NdFeB magnet and the graphite electrode, and perform melt grain boundary diffusion treatment under the action of the pulsed electric field; (4) After diffusion treatment, the sintered NdFeB magnet is taken out, the residual low melting point diffusion alloy on the surface is cleaned, and then the magnet is heated to 450~550℃ under pure argon protection for 1~3h aging treatment to obtain the final sintered NdFeB magnet. The low melting point R mentioned in step (1) a M b The alloy has a melting point below 500℃, and the mass percentage a+b=100, a≥3; R is one or more of Pr, Nd, Gd, Tb, Dy, and Ho, and the sum of the contents of Dy and Tb in the total content of R is not less than 60wt%; M is one or more of Ga, Sn, In, and Bi, and the sum of the contents of Ga and Sn in the total content of M is not less than 70wt%. In step (3), the current density of the pulse power supply is 5–20 A / cm. 2 The frequency is 50–150 Hz, and the duty cycle is 10%–30%. In step (3), the temperature of the melt grain boundary diffusion treatment is 500~650℃ and the treatment time is 1~5 hours.

2. The preparation method of sintered NdFeB magnet with improved coercivity through low-temperature grain boundary diffusion under pulsed electric field according to claim 1, characterized in that, The low melting point R a M b The alloy includes Tb3Dy1Ga 96 Tb3Ga 97 、Dy3Ga 97 、Tb3Gd2Ga 13 Sn 82 Tb5Ga 13 Sn 82 、Dy5Ho1Ga 72 Bi 22 Tb3Pr 0.5 Nd 1.5 Ga 95 Dy5Pr 0.5 Nd 1.5 Ga 80 In 13 .

3. The preparation method of sintered NdFeB magnet with improved coercivity through low-temperature grain boundary diffusion under pulsed electric field according to claim 1, characterized in that, In step (2), the negative terminal of the pulse power supply is connected to the sintered NdFeB magnet, and the positive terminal of the pulse power supply is connected to the graphite electrode plate. The area of ​​the graphite electrode plate should be larger than the area of ​​the magnet.

Citation Information

Patent Citations

  • Grain boundary diffusion method for improving properties of sintered NdFeB magnets