Biaxially oriented film
By combining high-density polyethylene homopolymer modified with a nucleating agent in biaxially oriented polyethylene film with low-density ethylene copolymer, the problem of high-density polyethylene being difficult to stretch was solved, achieving effective stretching and improved optical properties of high-density polyethylene, and enhancing recyclability.
Patent Information
- Application Number
- CN202280029330.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-19
- Filing Date
- 2022-04-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-04-14
AI Technical Summary
Existing technologies have difficulty effectively stretching high-density polyethylene, which limits the commercial application of biaxially oriented polyethylene film (BOPE), especially in the tenter frame method, which requires specific process conditions and has a narrow processing window.
A multi-layered biaxially oriented polyethylene film, comprising a core layer and an adjacent or surface layer, is formed by combining a high-density polyethylene homopolymer composition containing a nucleating agent or a mixture of nucleating agents with a lower-density ethylene copolymer and low-density polyethylene, and prepared via a multi-zone reactor system.
It improves the tensile and optical properties of biaxially oriented polyethylene film, enhances recyclability, achieves effective stretching of high-density polyethylene, and expands its commercial applications.
Smart Images

Figure CN117178010B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to BOPE films or film structures comprising at least three layers and having good optical properties. Background Technology
[0002] Biaxially oriented polyethylene (BOPE) film is produced by stretching a thick precursor (or base) film (often called a cast sheet) in two directions: longitudinal (MD) and transverse (TD). Stretching can be performed in a single process (simultaneous biaxial stretching) or in two sequential processes (sequential biaxial stretching). The equipment commonly used in the stretching process is often referred to as a "stenter" production line.
[0003] Compared to traditional blown films, BOPE films can achieve up to twice the stiffness (tensile modulus), with improved tensile strength, impact strength, puncture resistance and flexural crack resistance, as well as improved (i.e., lower) optical haze.
[0004] BOPE film is suitable for a variety of packaging applications, and the improved properties observed in biaxially oriented films or film structures allow for the design of "all-polyethylene" packaging (as opposed to packaging made with different types of polymers). This "all-polyethylene" packaging has higher inherent recyclability.
[0005] Tensile fabrication methods are widely used to prepare biaxially oriented polypropylene (BOPP) films and biaxially oriented polyethylene terephthalate (BOPET) films. However, polyethylene can be relatively difficult to stretch / biaxially oriented, which limits the commercial use of BOPE. Prior to this work, high-density polyethylene (e.g., with a density greater than about 0.950 g / cm³) had been observed to be difficult to stretch / biaxially oriented, which limits the commercial use of BOPE. 3 The density of polyethylene (HDPE) is poor when biaxially oriented. In fact, manufacturing BOPE films from HDPE requires specific or precise process conditions (i.e., a very narrow processing window). Alternatively, HDPE can be co-extruded using an adhesion accelerator layer (“cast accelerator”), such as a layer containing lower-density polyethylene material and its blends, or ethylene / propylene copolymers and terpolymers as adjacent co-extrusion layers.
[0006] There is still a need for new polyethylene compositions, especially higher-density polyethylene compositions that provide improved “stretchability” in BOPE processes, such as the tenter BOPE process. Summary of the Invention
[0007] The embodiments of this disclosure provide an “all-polyethylene” biaxially oriented film structure that has good optical properties and enhanced recyclability compared to BOPE films made of mixed polymer materials.
[0008] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising:
[0009] Core layer;
[0010] The first adjacent layer, which is adjacent to the first side of the core layer; and
[0011] The second adjacent layer is adjacent to the second side of the core layer;
[0012] The core layer includes:
[0013] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0014] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition;
[0015] The polyethylene homopolymer composition contains a nucleating agent or a mixture of nucleating agents; and
[0016] The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0017] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising:
[0018] Core layer;
[0019] The first surface layer adjacent to the first side of the core layer; and
[0020] The second surface layer adjacent to the second side of the core layer;
[0021] The core layer includes:
[0022] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0023] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition;
[0024] The polyethylene homopolymer composition contains a nucleating agent or a mixture of nucleating agents; and
[0025] The first and second outer layers each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0026] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising:
[0027] Core layer;
[0028] The first adjacent layer, which is adjacent to the first side of the core layer; and
[0029] The second adjacent layer is adjacent to the second side of the core layer;
[0030] The core layer includes:
[0031] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0032] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene;
[0033] The high-density polyethylene contains a nucleating agent or a mixture of nucleating agents;
[0034] The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than the density of the first polyethylene; and
[0035] The haze value of the biaxially oriented polyethylene film is less than 15%.
[0036] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising:
[0037] Core layer;
[0038] The first surface layer adjacent to the first side of the core layer; and
[0039] The second surface layer adjacent to the second side of the core layer;
[0040] The core layer includes:
[0041] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0042] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene;
[0043] The high-density polyethylene contains a nucleating agent or a mixture of nucleating agents;
[0044] The first and second surface layers each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene; and
[0045] The haze value of the biaxially oriented polyethylene film structure is less than 15%.
[0046] In one embodiment of this disclosure, the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE). Attached Figure Description
[0047] Figure 1 A schematic diagram of a multi-zone reactor system is shown, comprising a first polymerization zone defined by a first tubular reactor, a second polymerization zone defined by a tank reactor, and a third polymerization zone defined by a second tubular reactor. This schematic diagram represents the multi-zone reactor system only and is not drawn to scale. The approximate locations (locations A and B) for adding hydrogen to the multi-zone reactor system are also shown.
[0048] Description of the implementation plan
[0049] As used in this article, the term "monomer" refers to a small molecule that can chemically react with itself or other monomers and chemically bond to form a polymer.
[0050] The term "α-olefin" as used herein describes monomers having a straight-chain hydrocarbon chain containing 3 to 20 carbon atoms and a double bond at one end of the chain; the equivalent term is "straight-chain α-olefin". α-olefins may also be referred to as comonomers.
[0051] As used herein, the terms “polyethylene,” “polyethylene composition,” or “ethylene polymer” refer to macromolecules produced from ethylene monomers and optionally one or more other monomers, regardless of the specific catalyst or method used to produce the ethylene polymer. In the field of polyethylene, one or more other monomers are generally referred to as “one or more comonomers” and typically include α-olefins. The term “homopolymer” generally refers to a polymer containing only one monomer. The term “copolymer” refers to a polymer containing two or more monomers. Common types of polyethylene include high-density polyethylene (HDPE); medium-density polyethylene (MDPE); linear low-density polyethylene (LLDPE); and very low-density polyethylene (VLPDE) or ultra-low-density polyethylene (ULPDE), also known as plastomers and elastomers. The term polyethylene also includes polyethylene terpolymers, which may contain two or more comonomers other than ethylene. The term polyethylene also includes combinations or blends of the above-mentioned types of polyethylene.
[0052] The term "heterogeneous branched polyethylene" refers to a subset of polymers in the group of ethylene polymers produced using heterogeneous catalyst systems; non-limiting examples of such catalyst systems include Ziegler-Natta catalysts or chromium catalysts, both of which are well known in the art.
[0053] The term “homogeneous branched polyethylene” refers to a subset of polymers in the group of ethylene polymers produced using a single-active-site catalyst; non-limiting examples of said single-active-site catalysts include metallocene catalysts, phosphine-imine catalysts, and confined geometry catalysts, all of which are well known in the art.
[0054] Typically, homogeneous branched polyethylene has a narrow molecular weight distribution, for example, in gel permeation chromatography (GPC). w / M n Values less than approximately 2.8, and especially less than approximately 2.3, although exceptions may occur; M w and M n These refer to weight-average molecular weight and number-average molecular weight, respectively. Conversely, M of heterogeneous branched ethylene polymers... w / M n Typically greater than M of homogeneous polyethylene w / M n Generally, homogeneous branched ethylene polymers also exhibit a narrow compositional distribution, meaning that each macromolecule within the molecular weight distribution has a similar amount of comonomer. Typically, the Compositional Distribution Width Index (CDBI) is used to quantify the distribution of comonomers within the ethylene polymer and to differentiate ethylene polymers produced using different catalysts or methods. 50 "CDBI" is defined as the percentage of the ethylene polymer comprising up to 50% by weight (wt%) of the median comonomer composition; this definition is consistent with that described in WO93 / 03093 assigned to Exxon Chemical Patents Inc. 50 It can be calculated from the TREF curve (temperature elution fractionation); the TREF method is described by Wild et al. in J. Polym. Sci., Part B, Polym. Phys., Vol. 20(3), pp. 441-455. Typically, the CDBI of homogeneous branched ethylene polymers... 50 Greater than approximately 70% or greater than approximately 75%. Conversely, CDBI, a heterogeneous branched ethylene polymer containing α-olefins. 50 Typically lower than the CDBI of homogeneous ethylene polymers. 50 For example, CDBI of heterogeneous branched ethylene polymers. 50 It can be less than approximately 75%, or less than approximately 70%.
[0055] As is known to those skilled in the art, homogeneous branched ethylene polymers are often further subdivided into "linear homogeneous ethylene polymers" and "substantially linear homogeneous ethylene polymers." The difference between these two subgroups lies in the amount of long-chain branches: more specifically, linear homogeneous ethylene polymers have fewer than about 0.01 long-chain branches per 1000 carbon atoms; while substantially linear ethylene polymers have more than about 0.01 to about 3.0 long-chain branches per 1000 carbon atoms. The long-chain branches are essentially macromolecules, i.e., molecules with lengths similar to the macromolecules to which the long-chain branches are connected. Hereinafter, in this disclosure, the terms "homogeneous branched polyethylene" or "homogeneous branched ethylene polymer" refer to both linear homogeneous ethylene polymers and substantially linear homogeneous ethylene polymers.
[0056] In this disclosure, the terms "ethylene homopolymer" or "polyethylene homopolymer" are used to refer to polymers that are the product of a polymerization method, wherein only ethylene is intentionally added as a polymerizable monomer or is intentionally present as a polymerizable monomer.
[0057] In this disclosure, the terms "ethylene copolymer" or "polyethylene copolymer" mean that the polymer mentioned is the product of a polymerization process in which ethylene and one or more α-olefins are intentionally added as polymerizable monomers or are intentionally present as polymerizable monomers.
[0058] As used herein, the term "unsubstituted" means that a hydrogen group is bonded to the molecular group following the term "unsubstituted". The term "substituted" means that the group following the term has one or more portions (non-hydrogen groups) that have replaced one or more hydrogen groups at any position within the group.
[0059] The term "membrane" is used herein to refer to a membrane having one or more layers, which is formed by extruding a polymer through one or more die openings. The term "membrane structure" is used to indicate that the membrane has more than one layer (i.e., a membrane structure may have at least two layers, at least three layers, at least four layers, at least five layers, etc.).
[0060] In this disclosure, the terms “biaxially oriented polyethylene film,” “BOPE film,” “biaxially oriented polyethylene film structure,” or “BOPE film structure” generally describe a biaxially oriented film or film structure in which polyethylene is the main component polymer (i.e., polyethylene is present in a higher weight percentage than other non-polyethylene polymers, based on the total weight of the polymers present in the film or film structure).
[0061] The phrase “all polyethylene” as used in this article, when used to describe a membrane or membrane structure, means that the membrane or membrane structure will contain at least 90% by weight of polyethylene (as opposed to non-polyethylene polymer materials or compositions), based on the total weight of the polymer present in the membrane or membrane structure.
[0062] The "surface" layer is the outer layer of a multilayer membrane structure (i.e., the layer with an outer surface exposed to the environment).
[0063] A "core" layer is an inner layer of a multilayer membrane structure (i.e., a layer adjacent to the inner surface of the outermost layer, another inner layer, or another core layer). A multilayer membrane structure may have one or more core layers, which can also be considered as adjacent inner layers.
[0064] BOPE membrane structure
[0065] In one embodiment of the invention, the biaxially oriented polyethylene film structure has at least three layers, including at least one core layer comprising: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene, wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents.
[0066] In one embodiment of the invention, the biaxially oriented polyethylene film structure has at least three layers, including at least one core layer comprising: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents.
[0067] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer.
[0068] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 The high-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents; and wherein the first adjacent layer and the second adjacent layer each contain a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0069] In embodiments of this disclosure, the biaxially oriented polyethylene film structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer.
[0070] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 The high-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents; and wherein each of the first adjacent layer and the second adjacent layer contains at least 50% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0071] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer;
[0072] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 The high-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents; and wherein the first surface layer and the second surface layer each contain a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0073] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer;
[0074] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 The high-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents; and wherein the first surface layer and the second surface layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0075] In one embodiment of this disclosure, the core layer comprises: i) 70 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 30% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents.
[0076] In one embodiment of this disclosure, the core layer comprises: i) 90 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 10% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene; wherein the high-density polyethylene contains a nucleating agent or a mixture of nucleating agents.
[0077] In one embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the high-density polyethylene is present in amounts of 1 to 1000 ppm (parts per million) of the nucleating agent or mixture of nucleating agents, based on the total weight of the polymer materials used in the core layer (i.e., based on the total weight of i) the first polyethylene used in the core layer; and ii) the high-density polyethylene used).
[0078] In a further embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the high-density polyethylene is present in amounts of 5 to 1,000 ppm (parts per million), or 5 to 750 ppm, or 5 to 500 ppm, or 5 to 400 ppm, or 5 to 350 ppm, or 5 to 250 ppm, or 5 to 150 ppm, or 5 to 100 ppm of nucleating agent or mixture of nucleating agents, based on the total weight of the polymer materials used in the core layer (i.e., based on the total weight of i) the first polyethylene used in the core layer; and ii) the high-density polyethylene used).
[0079] In a further embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the high-density polyethylene is present in amounts of less than 500 ppm (parts per million), or less than 350 ppm, or less than 250 ppm, or less than 150 ppm, or less than 100 ppm, or less than 75 ppm, or less than 50 ppm, or less than 40 ppm, or less than 30 ppm, or less than 25 ppm, or less than 20 ppm, or less than 15 ppm, or less than 10 ppm, based on the total weight of the polymer materials used in the core layer (i.e., based on the total weight of i) the first polyethylene used in the core layer; and ii) the high-density polyethylene used).
[0080] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer.
[0081] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition contains a nucleating agent or a mixture of nucleating agents; and wherein each of the first adjacent layer and the second adjacent layer contains a third polyethylene, wherein the density of the third polyethylene is lower than the density of the first polyethylene.
[0082] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer.
[0083] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents; and wherein each of the first adjacent layer and the second adjacent layer comprises at least 50% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0084] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer;
[0085] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents; and wherein the first surface layer and the second surface layer each comprise a third polyethylene, wherein the density of the third polyethylene is lower than the density of the first polyethylene.
[0086] One embodiment of this disclosure is a biaxially oriented polyethylene film structure, comprising: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer;
[0087] The core layer comprises: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents; and wherein each of the first and second surface layers comprises at least 50% by weight (based on the weight of the polymer material used to manufacture each of the first and second surface layers) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0088] In one embodiment of this disclosure, the core layer comprises: i) 70 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 30% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents.
[0089] In one embodiment of this disclosure, the core layer comprises: i) 90 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ii) 0.5 to 10% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; wherein the polyethylene homopolymer composition comprises a nucleating agent or a mixture of nucleating agents.
[0090] In one embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the polyethylene homopolymer composition is present in amounts of 1 to 1000 ppm (parts per million) of the nucleating agent or mixture of nucleating agents, based on the total weight of the polymer materials used in the core layer (i.e., based on i) the first polyethylene used in the core layer; and ii) the total weight of the polyethylene homopolymer composition).
[0091] In a further embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the polyethylene homopolymer composition is present in amounts of 5 to 1,000 ppm (parts per million), or 5 to 750 ppm, or 5 to 500 ppm, or 5 to 400 ppm, or 5 to 350 ppm, or 5 to 250 ppm, or 5 to 150 ppm, or 5 to 100 ppm of nucleating agent or mixture of nucleating agents, based on the total weight of the polymeric material used in the core layer (i.e., based on i) the first polyethylene used in the core membrane layer; and ii) the total weight of the polyethylene homopolymer composition).
[0092] In a further embodiment of this disclosure, the nucleating agent or mixture of nucleating agents present in the polyethylene homopolymer composition is present in amounts of less than 500 ppm (parts per million), or less than 350 ppm, or less than 250 ppm, or less than 150 ppm, or less than 100 ppm, or less than 75 ppm, or less than 50 ppm, or less than 40 ppm, or less than 30 ppm, or less than 25 ppm, or less than 20 ppm, or less than 15 ppm, or less than 10 ppm, based on the total weight of the polymer material used in the core layer (i.e., based on i) the first polyethylene used in the core membrane layer; and ii) the total weight of the polyethylene homopolymer composition).
[0093] In one embodiment of this disclosure, the first adjacent layer and the second adjacent layer each contain at least 70% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0094] In one embodiment of this disclosure, the first adjacent layer and the second adjacent layer each contain at least 90% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0095] In embodiments of this disclosure, each of the first adjacent layer and the second adjacent layer comprises at least 95% by weight or at least 99% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0096] In one embodiment of this disclosure, the first adjacent layer and the second adjacent layer each comprise 100% by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0097] In embodiments of this disclosure, in addition to the third polyethylene, the first adjacent layer and the second adjacent layer may each contain 50% or less by weight, or 30% or less by weight, or 10% or less by weight, or 5% or less by weight, or 1% or less by weight (based on the weight of the polymer material used to manufacture each of the first adjacent layer and the second adjacent layer):
[0098] a) A first type of polyethylene, wherein the first type of polyethylene has a density greater than 0.940 g / cm³. 3 copolymers, or
[0099] b) A second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene; or
[0100] c) Another type of polyethylene, different from the first, second, and third polyethylenes, and which may be selected from: linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), very low-density polyethylene (VLDPE), and high-pressure low-density polyethylene (HPLDPE) prepared by ethylene free radical polymerization.
[0101] In one embodiment of this disclosure, the first and second outer layers each comprise at least 70% by weight (based on the weight of the polymer material used to manufacture each of the first and second outer layers) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0102] In one embodiment of this disclosure, the first and second outer layers each comprise at least 90% by weight (based on the weight of the polymer material used to manufacture each of the first and second outer layers) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0103] In embodiments of this disclosure, the first and second outer layers each comprise at least 95% by weight or at least 99% by weight (based on the weight of the polymer material used to manufacture each of the first and second outer layers) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0104] In one embodiment of this disclosure, the first and second outer layers each comprise 100% by weight (based on the weight of the polymer material used to manufacture each of the first and second outer layers) of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0105] In embodiments of this disclosure, in addition to the third polyethylene, the first and second surface layers may each comprise 50% or less by weight, or 30% or less by weight, or 10% or less by weight, or 5% or less by weight, or 1% or less by weight (based on the weight of the polymer material used to manufacture each of the first and second surface layers):
[0106] a) A first type of polyethylene, wherein the first type of polyethylene has a density greater than 0.940 g / cm³. 3 copolymers, or
[0107] b) A second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene; or
[0108] c) Another type of polyethylene, different from the first, second, and third polyethylenes, and which may be selected from: linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), very low-density polyethylene (VLDPE), and high-pressure low-density polyethylene (HPLDPE) prepared by ethylene free radical polymerization.
[0109] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer; the core layer accounts for at least 50% of the total weight of the biaxially oriented membrane or membrane structure.
[0110] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer; the core layer accounts for at least 60% of the total weight of the biaxially oriented membrane or membrane structure.
[0111] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer; the core layer accounts for at least 70% of the total weight of the biaxially oriented membrane or membrane structure.
[0112] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer; the core layer accounts for at least 80% of the total weight of the biaxially oriented membrane or membrane structure.
[0113] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer; the core layer accounts for at least 90% of the total weight of the biaxially oriented membrane or membrane structure.
[0114] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer; the core layer accounts for at least 50% of the total weight of the biaxially oriented membrane or membrane structure.
[0115] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer; the core layer accounts for at least 60% of the total weight of the biaxially oriented membrane or membrane structure.
[0116] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer; wherein the core layer accounts for at least 70% of the total weight of the biaxially oriented membrane or membrane structure.
[0117] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer; the core layer accounts for at least 80% of the total weight of the biaxially oriented membrane or membrane structure.
[0118] In one embodiment, the biaxially oriented membrane or membrane structure includes: a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer; wherein the core layer accounts for at least 90% of the total weight of the biaxially oriented membrane or membrane structure.
[0119] In one embodiment of this disclosure, biaxially oriented polyethylene (BOPE) films or film structures can be manufactured using a tenter frame method.
[0120] Tensor-stretching methods are commonly used to prepare biaxially oriented films and are applicable to the embodiments of this disclosure. Tensor-stretching methods are well known to those skilled in the art of film manufacturing. The method begins with an extruder equipped with a slotted die to form a sheet or film. For convenience, this extruded sheet or film may be referred to as a “base film” or “base film structure” or “base structure.” Once the base structure is quenched on cooling rollers, it is reheated and longitudinal (MD) stretching or longitudinal orientation (MDO) is achieved by stretching the base structure using several closely spaced rollers rotating at progressively increasing surface speeds. After MD stretching, a jig (attached to a chain) clamps the edges of the moving sheet (or film or web) and guides it into an oven. In the oven, the edges of the base structure are pulled apart, making the sheet wider, thereby providing transverse orientation (TDO). Orientation / stretching causes the film structure to become thinner proportionally to the orientation or stretching ratio. For example, to prepare a 1-mil finished BOPE film with a stretch ratio of 5:1 in the longitudinal direction (MD) and 8:1 in the transverse direction (TD), the method can begin with a film or sheet 40 mils thick.
[0121] In embodiments of this disclosure, the stretch ratio in the longitudinal direction (MD) can be from about 5:1 to about 9:1, and the stretch ratio in the transverse direction (TD) can be from about 7:1 to 12:1. In other embodiments of this disclosure, the stretch ratio in the longitudinal direction (MD) can be from about 3:1 to about 12:1, and the stretch ratio in the transverse direction (TD) can be from about 3:1 to 12:1. In still other embodiments of this disclosure, the stretch ratio in the longitudinal direction (MD) can be from about 5:1 to about 12:1, and the stretch ratio in the transverse direction (TD) can be from about 5:1 to 12:1. In yet still other embodiments of this disclosure, the stretch ratio in the longitudinal direction (MD) can be from about 3:1 to about 10:1, and the stretch ratio in the transverse direction (TD) can be from about 3:1 to 10:1.
[0122] Further details of the biaxial orientation method are provided by Kanai T. et al. in the textbook “Film Processing Advances” (2014), Hanser Publishers, but the typical sequential biaxial orientation method will include: casting a relatively thick base membrane structure from a slot die, followed by cooling on cooling rollers (or in a water bath); stretching the base membrane structure longitudinally using heated rollers rotating at gradually increasing speeds; stretching the membrane structure transversely by pulling each edge of the membrane structure with clamps attached to the edges of the membrane structure, wherein as the clamps pull the membrane forward, they further move apart to pull the edges of the clamped membrane in a cross direction (i.e., stretching occurs in the transverse direction perpendicular to the longitudinal direction); annealing the membrane structure in an oven; performing optional surface treatments on the membrane structure; trimming the unstretched edges of the membrane structure held by the clamps; and finally winding the membrane structure.
[0123] Although sequential biaxial stretching is employed in the embodiments of this disclosure, in some embodiments, sequential biaxial orientation may lead to film quality problems. For example, in some embodiments, the optical properties of the film or multilayer film structure may be compromised. Therefore, for certain embodiments, alternative unit operations may be preferred, which involve performing longitudinal / transverse stretching simultaneously in a single method step. In one embodiment, during simultaneous stretching, the base film may be held and suspended in the air by a tenter frame fixture (as described above) and stretched simultaneously in both the MD and TD directions.
[0124] In embodiments of this disclosure, a biaxially oriented film or film structure comprising at least three layers has a haze value of ≤20%, or <20%, or ≤15%, or <15%, or ≤10%, or <10%, or ≤7.5%, or <7.5%.
[0125] In embodiments of this disclosure, a biaxially oriented film or film structure comprising at least three layers has a transparency value of ≥80%, or >80%, or ≥85%, or >85%, or ≥90%, or >90%, or ≥95%, or >95%.
[0126] In embodiments of this disclosure, the biaxially oriented film or film structure includes a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer, having a haze value of ≤20%, or <20%, or ≤15%, or <15%, or ≤10%, or <10%, or ≤7.5%, or <7.5%.
[0127] In embodiments of this disclosure, the biaxially oriented film or film structure includes a core layer; a first adjacent layer adjacent to a first side of the core layer; and a second adjacent layer adjacent to a second side of the core layer, having a transparency value of ≥80%, or >80%, or ≥85%, or >85%, or ≥90%, or >90%, or ≥95%, or >95%.
[0128] In embodiments of this disclosure, the biaxially oriented film or film structure includes a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer, having a haze value of ≤20%, or <20%, or ≤15%, or <15%, or ≤10%, or <10%, or ≤7.5%, or <7.5%.
[0129] In embodiments of this disclosure, the biaxially oriented film or film structure includes a core layer; a first surface layer adjacent to a first side of the core layer; and a second surface layer adjacent to a second side of the core layer, having a transparency value of ≥80%, or >80%, or ≥85%, or >85%, or ≥90%, or >90%, or ≥95%, or >95%.
[0130] The biaxially oriented film prepared according to this disclosure is suitable for a variety of packaging applications. In one embodiment, the biaxially oriented film structure can be used as a laminated structure. For example, the biaxially oriented film structure of this disclosure can be used as a printing web when laminated to a sealant web that is also made of polyethylene but may contain a lower-density polyethylene material. This type of laminated structure is easier to recycle than conventional laminated structures that contain polyester or polypropylene layers laminated to polyethylene layers.
[0131] The following provides an alternative embodiment of the first polyethylene for a biaxially oriented film structure.
[0132] The following provides an alternative embodiment of a second polyethylene for a biaxially oriented film structure.
[0133] The following provides an alternative embodiment of a third polyethylene for a biaxially oriented film structure.
[0134] First polyethylene
[0135] In one embodiment of this disclosure, the first polyethylene is prepared using a multi-active-site catalyst system, non-limiting examples of which include Ziegler-Natta polymerization catalysts and chromium catalysts, both of which are well known in the art.
[0136] In one embodiment of this disclosure, the first polyethylene is prepared using a Ziegler-Natta polymerization catalyst known in the art.
[0137] In one embodiment of this disclosure, the first polyethylene is prepared by solution-phase polymerization using a Ziegler-Natta polymerization catalyst.
[0138] In one embodiment of this disclosure, the first polyethylene is prepared by a solution-phase polymerization method using a Ziegler-Natta polymerization catalyst, the solution-phase polymerization method being carried out in a multi-zone polymerization reactor system.
[0139] In one embodiment of this disclosure, the first polyethylene is prepared by a solution-phase polymerization method using a Ziegler-Natta polymerization catalyst, the solution-phase polymerization method being carried out in a multi-zone polymerization reactor system, the multi-zone reactor system comprising a first, second, and third polymerization zone.
[0140] In one embodiment of this disclosure, the first polyethylene is an ethylene copolymer.
[0141] In embodiments of this disclosure, the α-olefin that can be copolymerized with ethylene to prepare the first polyethylene may be selected from 1-butene, 1-pentene, 1-hexene, and 1-octene and mixtures thereof.
[0142] In embodiments of this disclosure, the first polyethylene comprises ethylene and at least one α-olefin having 4 to 8 carbon atoms.
[0143] In one embodiment of this disclosure, the first polyethylene is an ethylene / 1-butene copolymer.
[0144] In embodiments of this disclosure, the first polyethylene has a content of at least 0.940 g / cm³. 3 or greater than 0.940 g / cm 3 or at least 0.941 g / cm 3 The density.
[0145] In embodiments of this disclosure, the density of the first polyethylene is from 0.940 to 0.965 g / cm³. 3 Or 0.940 to 0.963 g / cm³ 3 Or 0.941 to 0.965 g / cm³ 3 Or 0.941 to 0.963 g / cm³3 Or 0.941 to 0.962 g / 10 min, or 0.940 to 0.960 g / cm³ 3 Or 0.940 to 0.958 g / cm³ 3 Or 0.940 to 0.956 g / cm³ 3 Or 0.940 to 0.952 g / cm³ 3 Or 0.940 to 0.950 g / cm³ 3 Or 0.942 to 0.960 g / cm³ 3 Or 0.942 to 0.958 g / cm³ 3 Or 0.942 to 0.956 g / cm³ 3 Or 0.942 to 0.952 g / cm³ 3 Or 0.942 to 0.950 g / cm³ 3 .
[0146] In embodiments of this disclosure, the melt index I2 of the first polyethylene is at least 0.50 g / 10 min, or at least 0.75 g / 10 min, or at least 0.80 g / 10 min, or at least 1.0 g / 10 min.
[0147] In embodiments of this disclosure, the melt index I2 of the first polyethylene may be from about 0.01 g / 10 min to about 10.0 g / 10 min, or from about 0.1 g / 10 min to about 10.0 g / 10 min, or from 0.5 to 10.0 g / 10 min, or from about 0.1 g / 10 min to about 5.0 g / 10 min, or from about 0.1 g / 10 min to about 3.0 g / 10 min, or from about 0.5 g / 10 min to about 5.0 g / 10 min, or from about 0.5 g / 10 min to about 3.0 g / 10 min, or from about 0.5 g / 10 min to about 2.5 g / 10 min.
[0148] In embodiments of this disclosure, the melt flow ratio (MFR) of the first polyethylene is I 21 / I2 is greater than 50, or greater than 60, or greater than 65, or greater than 70, or greater than 75.
[0149] In one embodiment of this disclosure, the melt flow ratio (MFR) of the first polyethylene is I 21 / I2 is less than 115.
[0150] In embodiments of this disclosure, the melt flow ratio (MFR) of the first polyethylene is I 21 / I2 is 50 to 120, or 50 to 115, or greater than 65 to less than 115, or greater than 75 to less than 115.
[0151] In one embodiment of this disclosure, the number-average molecular weight M of the first polyethylene n For about 5,000 to about 75,000, or about 5,000 to about 50,000, or about 5,000 to about 30,000, or about 5,000 to about 25,000, or about 7,500 to about 50,000, or about 7,500 to about 30,000, or about 7,500 to about 25,000, or about 5,000 to about 20,000, or about 5,000 to about 15,000. 00, or about 7,500 to about 20,000, or about 7,500 to about 15,000, or about 10,000 to about 15,000, or about 10,000 to about 12,500, or about 11,000 to about 15,000, or about 11,000 to about 12,500, or greater than 11,000 to less than 12,500, or greater than 11,000 to less than 15,000.
[0152] In one embodiment of this disclosure, the weight-average molecular weight M of the first polyethylene w The range is approximately 75,000 to approximately 250,000, or approximately 80,000 to approximately 200,000, or approximately 90,000 to approximately 175,000, or approximately 100,000 to approximately 175,000, or approximately 90,000 to approximately 150,000, or approximately 100,000 to approximately 150,000, or approximately 100,000 to approximately 125,000, or approximately 90,000 to approximately 130,000, or approximately 90,000 to approximately 125,000, or approximately 85,000 to approximately 140,000, or approximately 85,000 to approximately 150,000, or greater than approximately 85,000 to less than approximately 140,000.
[0153] In one embodiment of this disclosure, the Z-average molecular weight M of the first polyethylene z The amount is at least 500,000, or greater than 500,000, or at least 550,000, or greater than 550,000, or at least 600,000, or greater than 600,000.
[0154] In one embodiment of this disclosure, the Z-average molecular weight M of the first polyethylene z The amount is approximately 500,000 to approximately 800,000, or greater than 500,000 to approximately 800,000, or greater than 500,000 to less than 800,000, or approximately 500,000 to approximately 750,000, or approximately 525,000 to approximately 750,000, or approximately 550,000 to approximately 750,000, or approximately 575,000 to approximately 750,000, or approximately 550,000 to approximately 725,000, or approximately 575,000 to approximately 725,000, or approximately 600,000 to approximately 700,000.
[0155] In embodiments of this disclosure, the molecular weight distribution M of the first polyethylene w / M n The range is 3.0 to 20.0, or greater than 3.0 to 18.0, or 3.5 to 16.0.
[0156] In embodiments of this disclosure, the molecular weight distribution M of the first polyethylene w / M n The range is 8.0 to 12.0, or greater than 8.0 to 12.0, or 8.5 to 12.0, or 9.0 to 12.0, or greater than 9.0 to less than 12.0, or 9.0 to 11.5, or 8.5 to 11.5, or 9.0 to 11.0, or 8.0 to 11.0, or 9.0 to 10.5, or 9.5 to 10.5.
[0157] In the embodiments of this disclosure, the Z-average molecular weight distribution M of the first polyethylene z / M w The values are 3.5 to 8.0, or 4.0 to 8.0, or 4.0 to 7.5, or 4.0 to 7.0, or 4.5 to 7.5, or 4.5 to 7.0, or 4.5 to 6.5, or 5.0 to 7.0, or 5.5 to 7.0, or 5.0 to 6.5, or 5.5 to 6.5, or greater than 5.0 to less than 6.5, or 5.0 to 6.25, or 5.0 to 6.0.
[0158] In one embodiment of this disclosure, the first polyethylene has a value defined as Log 10 [I6 / I2] / Log 10 The stress index of [6.48 / 2.16] is 1.60 to 2.00, or 1.65 to 2.00, or 1.70 to 2.00, or 1.75 to 1.95, or 1.75 to 1.90, or 1.80 to 1.95, or 1.80 to 1.90, or greater than 1.80 to less than 1.90.
[0159] In one embodiment of this disclosure, the first polyethylene is characterized by having a high Mz of about 500,000 or higher and a broad molecular weight distribution (Mw / Mn) of about 9.0 to about 12.0.
[0160] In embodiments of this disclosure, the first polyethylene has a composition distribution width index (CDBI) of 40 to 75 wt%, or 50 to 70 wt%, or 55 to 70 wt%, or 55 to 65 wt%. 50 .
[0161] In embodiments of this disclosure, the first polyethylene has a composition distribution width index (CDBI) of 35 to 65 wt%, or 35 to 60 wt%, or 35 to 55 wt%, or 40 to 60 wt%, or 40 to 55 wt%, or 40 to 50 wt%, or greater than 40 wt% to less than 50 wt%. 25 .
[0162] In one embodiment of this disclosure, the first polyethylene exhibits a single-peak profile in gel permeation chromatography (GPC). The term "single-peak" is defined herein as indicating the presence of only one significant peak or maximum value in the GPC profile. A single-peak profile includes a broad single-peak profile, and may also include shoulders or buried peaks that cannot be easily separated or unconvoluted into well-defined, distinctive peaks.
[0163] In one embodiment of this disclosure, the first polyethylene has a normal comonomer distribution curve measured using GPC-FTIR. If the amount of comonomer incorporated, as measured using GPC-FTIR, decreases with increasing molecular weight, the distribution is described as “normal.” Thus, the term “normal comonomer distribution” is used herein to indicate that, within the molecular weight range of the first polyethylene, the comonomer content of various polymer fractions is substantially non-uniform, and its higher molecular weight fractions have proportionally lower comonomer contents. If the amount of comonomer incorporated, as measured using GPC-FTIR, is substantially constant with molecular weight, the comonomer distribution is described as “flat” or “uniform.” The terms “reverse comonomer distribution” and “partially reverse comonomer distribution” refer to the presence in the GPC-FTIR data obtained for the copolymer that one or more higher molecular weight components have a higher amount of comonomer incorporated than one or more lower molecular weight components. The term "reverse comonomer distribution" as used herein refers to a distribution in which the comonomer content is substantially non-uniform across the various polymer fractions within the molecular weight range of the first polyethylene, with higher molecular weight fractions exhibiting proportionally higher comonomer contents (i.e., the distribution is described as "reverse" or "inverted" if the comonomer incorporation increases with increasing molecular weight). A comonomer distribution is still considered "reverse" when the comonomer incorporation increases and then decreases with increasing molecular weight, but can also be described as "partially reversed."
[0164] In one embodiment, the first polyethylene contains catalyst residues that reflect the chemical composition of the catalyst formulation used to manufacture it. Those skilled in the art will understand that catalyst residues are typically quantified, for example, by parts per million of metals in the first polyethylene, wherein the metals present originate from metals in the catalyst formulation used to manufacture it. Non-limiting examples of metal residues that may be present include Group 4 to 6 metals, such as titanium, zirconium, hafnium, and vanadium.
[0165] In embodiments of this disclosure, the first polyethylene has at least 0.050 ppm of titanium, or at least 0.100 ppm of titanium, or at least 0.250 ppm of titanium, or at least 0.300 ppm of titanium (based on the weight of the first polyethylene).
[0166] In embodiments of this disclosure, the first polyethylene has 0.050 to 3.0 ppm titanium, or 0.050 to 2.5 ppm titanium, or 0.050 to 2.0 ppm titanium, or 0.050 to 1.5 ppm titanium, or 0.050 to 1.0 ppm titanium, or 0.100 to 3.0 ppm titanium, or 0.100 to 2.5 ppm titanium, or 0.100 to 2.0 ppm titanium, or 0.100 to 1.5 ppm titanium, or 0.100 to 1.0 ppm titanium, or 0.250 to 3.0 ppm titanium, or 0.250 to 2.0 ppm titanium, or 0.250 to 1.5 ppm titanium, or 0.250 to 1.0 ppm titanium (based on the weight of the first polyethylene).
[0167] In embodiments of this disclosure, the first polyethylene has at least 0.050 ppm of vanadium, or at least 0.100 ppm of vanadium, or at least 0.200 ppm of vanadium, or at least 0.250 ppm of vanadium, or at least 0.300 ppm of vanadium (based on the weight of the first polyethylene).
[0168] In embodiments of this disclosure, the first polyethylene has 0.050 to 3.0 ppm vanadium, or 0.050 to 2.5 ppm vanadium, or 0.050 to 2.0 ppm vanadium, or 0.050 to 1.5 ppm vanadium, or 0.050 to 1.0 ppm vanadium, or 0.100 to 3.0 ppm vanadium, or 0.100 to 2.5 ppm vanadium, or 0.100 to 2.0 ppm vanadium, or 0.100 to 1.5 ppm vanadium, or 0.100 to 1.0 ppm vanadium, or 0.200 to 3.0 ppm vanadium, or 0.200 to 2.0 ppm vanadium, or 0.200 to 1.5 ppm vanadium, or 0.200 to 1.0 ppm vanadium (based on the weight of the first polyethylene).
[0169] In one embodiment of this disclosure, the first polyethylene does not have long-chain branches or does not contain a measurable amount of long-chain branches (“LCB”). LCB is a well-known structural phenomenon in ethylene copolymers and is known to those skilled in the art. Traditionally, there are three methods for LCB analysis: nuclear magnetic resonance spectroscopy (NMR), e.g. see J. C. Landall, J. Macromol. Sci., Rev. Macromol. Chem. Phys. 1989, 29, 201; triple detection SEC equipped with DRI, viscometer and low-angle laser scattering detector, e.g. see W. Yau and D. D. Hill, Int. J. Polym. Anal. Character. 1996; 2: 151; and rheology, e.g. see W. Graessley, Acc. Chem. Res. 1977, 10, 332-339.
[0170] In one embodiment of this disclosure, the prepared first polyethylene is characterized by having a Mz greater than about 500,000, a molecular weight distribution (Mw / Mn) of about 9.0 to about 12.0, and a melt index greater than 0.5 g / 10 min. Not wishing to be bound by theory, and as shown in the appended examples, we have observed that these properties of the first polyethylene can be achieved when using the aforementioned multi-zone reactor system and by carefully controlling the amount and location of hydrogen addition throughout the multi-zone reactor system.
[0171] Second polyethylene
[0172] In this disclosure, the second polyethylene will contain a nucleating agent or a mixture of nucleating agents.
[0173] In embodiments of this disclosure, the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene.
[0174] In this disclosure, high-density polyethylene (HDPE) is defined as having a density of at least 0.950 g / cm³. 3 ethylene homopolymers or ethylene copolymers.
[0175] In one embodiment of this disclosure, high-density polyethylene (HDPE) contains one or more nucleating agents.
[0176] In embodiments of this disclosure, the second polyethylene is a polyethylene homopolymer composition comprising one or more ethylene homopolymer components.
[0177] In embodiments of this disclosure, the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition.
[0178] In embodiments of this disclosure, the second polyethylene is a polyethylene homopolymer composition comprising: a first ethylene homopolymer; and a second ethylene homopolymer, embodiments of which are further described below.
[0179] In one embodiment of this disclosure, the polyethylene homopolymer composition exhibits a bimodal curve in gel permeation chromatography.
[0180] In one embodiment of this disclosure, the polyethylene homopolymer composition exhibits a multi-peak profile in gel permeation chromatography.
[0181] In one embodiment of this disclosure, the polyethylene homopolymer composition comprises one or more nucleating agents.
[0182] In embodiments of this disclosure, the density of the polyethylene homopolymer composition is at least 0.950 g / cm³. 3 or at least 0.955 g / cm³ 3 or at least 0.960 g / cm³ 3 .
[0183] In embodiments of this disclosure, the density of the polyethylene homopolymer composition is from 0.950 to 0.975 g / cm³. 3 Or 0.952 to 0.975 g / cm³ 3 Or 0.952 to 0.973 g / cm³ 3 Or 0.955 to 0.975 g / cm³ 3 Or 0.955 to 0.970 g / cm³ 3 .
[0184] In embodiments of this disclosure, the melt index I2 of the polyethylene homopolymer composition is 0.5 to 10.0 g / 10 min, or 0.5 to 5.0 g / 10 min. In further embodiments of this disclosure, the melt index I2 of the polyethylene homopolymer composition is 0.8 to 8.0 g / 10 min, or 0.8 to 5 g / 10 min.
[0185] In one embodiment of this disclosure, the polyethylene homopolymer composition has a molecular weight distribution (Mw / Mn) of about 3.0 to about 20.0.
[0186] Polyethylene homopolymer compositions can be prepared by any blending method, such as: 1) physical blending of particulate resins; 2) co-feeding different resins to the same extruder; 3) melt blending (in any conventional polymer blending equipment); 4) solution blending; or 5) polymerization methods using two or more reactors.
[0187] In one embodiment of this disclosure, a polyethylene homopolymer composition is prepared by solution polymerization using two reactors operated under different polymerization conditions. This provides a homogeneous in-situ blend of first and second ethylene homopolymer components. Examples of this method are described in published U.S. Patent Application Publication 2006 / 0047078, the disclosure of which is incorporated herein by reference.
[0188] In one embodiment of this disclosure, a polyethylene homopolymer composition is prepared by melt blending first and second ethylene homopolymers in an extruder.
[0189] In one embodiment of this disclosure, a polyethylene homopolymer composition is prepared by melt blending the following two blend components in an extruder:
[0190] 90 to 70% by weight of I) a first ethylene homopolymer, which has a melt index I2 of about 0.8 to about 2.0 g / 10 min and a melt flow rate of 0.955 to 0.965 g / cm³. 3 A conventional polyethylene homopolymer composition with a density of [missing information], and 10 to 30 wt% of a second ethylene homopolymer having a melt index I2 of about 15 to about 30 g / 10 min and a melt flow rate of 0.950 to 0.960 g / cm³. 3 A conventional polyethylene homopolymer composition (HDPE) with a certain density.
[0191] In one embodiment of this disclosure, a polyethylene homopolymer composition is prepared by solution polymerization using two reactors operated under different polymerization conditions. This provides a homogeneous in-situ blend of the ethylene polymer component prepared in each reactor. Such blends can be prepared, for example, according to U.S. Patent Application Publications US2013 / 0225743 or US2008 / 0118749 and U.S. Provisional Application 63 / 023,270.
[0192] In one embodiment, the polyethylene homopolymer composition is an in-situ blend of a first ethylene homopolymer and a second ethylene homopolymer.
[0193] First ethylene homopolymer
[0194] In one embodiment, the first ethylene homopolymer is prepared using a single-active-site catalyst.
[0195] In one embodiment, the first ethylene homopolymer is prepared using a phosphine imide catalyst.
[0196] In one embodiment, the first ethylene homopolymer is prepared in a solution-phase polymerization reactor using a single-active-center catalyst.
[0197] In one embodiment, the first ethylene homopolymer is prepared in a solution-phase polymerization reactor using a phosphine imide catalyst.
[0198] In one embodiment of this disclosure, the melt index I2 of the first ethylene homopolymer is lower than that of the second ethylene homopolymer.
[0199] In one embodiment of this disclosure, the melt index I2 of the first ethylene homopolymer is at least 50% of the melt index I2 of the second ethylene homopolymer.
[0200] In one embodiment of this disclosure, the melt index I2 of the first ethylene homopolymer is one-tenth the melt index I2 of the second ethylene homopolymer.
[0201] In one embodiment of this disclosure, the weight-average molecular weight M of the first ethylene homopolymer w The weight-average molecular weight M of the second ethylene homopolymer is higher than that of the second ethylene homopolymer. w .
[0202] As those skilled in the art will recognize, the melt index I2 is generally inversely proportional to the molecular weight. Therefore, in one embodiment of this disclosure, the first ethylene homopolymer has a relatively low melt index I2 (or in other words, a relatively high molecular weight) compared to the second ethylene homopolymer.
[0203] In one embodiment of this disclosure, the density of the first ethylene homopolymer is 0.950 g / cm³. 3 Up to 0.975 g / cm 3 In another embodiment of this disclosure, the density of the first ethylene homopolymer is from 0.955 to 0.970 g / cm³. 3 In another embodiment of this disclosure, the density of the first ethylene homopolymer is from 0.955 to 0.965 g / cm³. 3 .
[0204] In one embodiment of this disclosure, the first ethylene homopolymer has a melt index I2 of about 0.01 to about 1.0 g / 10 min (g / 10 min).
[0205] In one embodiment of this disclosure, the first ethylene homopolymer has a melt index I2 of about 0.1 to about 2.0 g / 10 min (g / 10 min).
[0206] In embodiments of this disclosure, the melt index I2 of the first ethylene homopolymer is about 0.1 to about 5.0 g / 10 min (g / 10 min), or about 0.1 to about 10 g / 10 min.
[0207] In one embodiment of this disclosure, the molecular weight distribution (Mw / Mn) of the first ethylene homopolymer is from about 1.7 to about 20.0. In a further embodiment of this disclosure, the molecular weight distribution (Mw / Mn) of the first ethylene homopolymer is from about 2.0 to about 20.0, or from about 1.7 to about 4.0, or from about 2.0 to about 4.0.
[0208] In one embodiment of this disclosure, the first ethylene homopolymer itself may comprise one or more high-density ethylene homopolymer sub-components.
[0209] In one embodiment of this disclosure, the first ethylene homopolymer accounts for 95 to 30 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 95 to 40 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 95 to 50 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 95 to 60 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 90 to 30 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 90 to 40 wt% of the total weight of the first and second ethylene homopolymers. In one embodiment of this disclosure, the first ethylene homopolymer accounts for 90 to 50% by weight (wt%) of the total weight of the first ethylene homopolymer and the second ethylene homopolymer. In another embodiment of this disclosure, the first ethylene homopolymer accounts for 90 to 60% by weight (wt%) of the total weight of the first ethylene homopolymer and the second ethylene homopolymer.
[0210] In one embodiment of this disclosure, the first ethylene homopolymer accounts for 75 to 35% by weight (wt%) of the total weight of the first ethylene homopolymer and the second ethylene homopolymer, or 65 to 40% by weight (wt%) of the total weight of the first ethylene homopolymer and the second ethylene homopolymer, or 65 to 45% by weight (wt%) of the first ethylene homopolymer and the second ethylene homopolymer, or 65 to 50% by weight (wt%) of the first ethylene homopolymer and the second ethylene homopolymer, or 60 to 50% by weight (wt%) of the first ethylene homopolymer and the second ethylene homopolymer.
[0211] Second ethylene homopolymer
[0212] In one embodiment, the second ethylene homopolymer is prepared using a single-active-site catalyst.
[0213] In one embodiment, the second ethylene homopolymer is prepared using a phosphine imide catalyst.
[0214] In one embodiment, the second ethylene homopolymer is prepared in a solution-phase polymerization reactor using a single-active-center catalyst.
[0215] In one embodiment, the second ethylene homopolymer is prepared in a solution-phase polymerization reactor using a phosphine imide catalyst.
[0216] In one embodiment of this disclosure, the melt index I2 of the second ethylene homopolymer is higher than that of the first ethylene homopolymer.
[0217] In one embodiment of this disclosure, the melt index I2 of the second ethylene homopolymer is at least 50% greater than the melt index I2 of the first ethylene homopolymer.
[0218] In one embodiment of this disclosure, the melt index I2 of the second ethylene homopolymer is at least 10 times that of the melt index I2 of the first ethylene homopolymer.
[0219] In one embodiment of this disclosure, the weight-average molecular weight M of the second ethylene homopolymer w The weight average molecular weight M of the first ethylene homopolymer is lower than that of the first ethylene homopolymer. w .
[0220] As those skilled in the art will recognize, the melt index I2 is generally inversely proportional to the molecular weight. Therefore, in one embodiment of this disclosure, the second ethylene homopolymer has a relatively high melt index I2 (or in other words, a relatively low molecular weight) compared to the first ethylene homopolymer.
[0221] In one embodiment of this disclosure, the density of the second ethylene homopolymer is 0.950 g / cm³. 3 Up to 0.975 g / cm 3 In another embodiment of this disclosure, the density of the second ethylene homopolymer is from 0.955 to 0.970 g / cm³. 3 In another embodiment of this disclosure, the density of the second ethylene homopolymer is from 0.955 to 0.965 g / cm³. 3 .
[0222] In one embodiment of this disclosure, the melt index I2 of the second ethylene homopolymer is greater than about 100 g / 10 min, or greater than about 250 g / 10 min, or greater than about 500 g / 10 min. In a further embodiment, the second ethylene homopolymer may have a melt index greater than about 500 to about 25,000 g / 10 min, or greater than about 500 to about 15,000 g / 10 min, or greater than about 500 to about 10,000 g / 10 min, or greater than about 500 to about 8,500 g / 10 min.
[0223] In a further embodiment, the second ethylene homopolymer may have a melt index greater than about 5.0 to about 50 g / 10 min, or greater than 5.0 to about 40.0 g / 10 min, or greater than 5.0 to about 30 g / 10 min, or greater than 5.0 to about 20.0 g / 10 min.
[0224] In one embodiment of this disclosure, the molecular weight distribution (Mw / Mn) of the second ethylene homopolymer is from about 1.7 to about 20.0. In a further embodiment of this disclosure, the molecular weight distribution (Mw / Mn) of the second ethylene homopolymer is from about 2.0 to about 20.0, or from about 1.7 to about 4.0, or from about 2.0 to about 4.0.
[0225] In one embodiment of this disclosure, the second ethylene homopolymer itself may comprise one or more high-density ethylene homopolymer sub-components.
[0226] In one embodiment of this disclosure, the second ethylene homopolymer accounts for 5 to 70 wt% of the total weight of the first and second ethylene homopolymers. In another embodiment, the second ethylene homopolymer accounts for 5 to 60 wt% of the total weight of the first and second ethylene homopolymers. In yet another embodiment, the second ethylene homopolymer accounts for 5 to 50 wt% of the total weight of the first and second ethylene homopolymers. In one embodiment, the second ethylene homopolymer accounts for 5 to 40 wt% of the total weight of the first and second ethylene homopolymers. In one embodiment, the second ethylene homopolymer accounts for 10 to 70 wt% of the total weight of the first and second ethylene homopolymers. In yet another embodiment, the second ethylene homopolymer accounts for 10 to 60 wt% of the total weight of the first and second ethylene homopolymers. In one embodiment of this disclosure, the second ethylene homopolymer accounts for 10 to 50% by weight (wt%) of the total weight of the first and second ethylene homopolymers. In another embodiment of this disclosure, the second ethylene homopolymer accounts for 10 to 40% by weight (wt%) of the total weight of the first and second ethylene homopolymers.
[0227] In one embodiment of this disclosure, the second ethylene homopolymer accounts for 25 to 65% by weight (wt%) of the total weight of the first and second ethylene homopolymers, or 35 to 60% by weight (wt%) of the total weight of the first and second ethylene homopolymers, or 35 to 55% by weight (wt%) of the total weight of the first and second ethylene homopolymers, or 35 to 55% by weight (vt%) of the total weight of the first and second ethylene homopolymers, or 40 to 50% by weight (wt%) of the total weight of the first and second ethylene homopolymers.
[0228] nucleating agent
[0229] The term “nucleating agent” as used herein is intended to convey its conventional meaning to those skilled in the art of preparing nucleating polyolefin compositions, namely, an additive that alters the crystallization behavior of a polymer when the polymer melt is cooled.
[0230] U.S. Patents 5,981,636, 6,465,551 and 6,599,971 provide a review of nucleating agents, the disclosures of which are incorporated herein by reference.
[0231] A commercially available nucleating agent that can be added to a second polyethylene (e.g., high-density polyethylene or polyethylene homopolymer composition) is dibenzyl sorbitol ester. Other examples of nucleating agents that can be added to the second polyethylene include cyclic organic structures (and their salts, such as disodium bicyclic [2.2.1]heptenedioate) disclosed in U.S. Patent 5,981,636; saturated versions of the structures disclosed in U.S. Patent 5,981,636 (such as those disclosed in U.S. Patent 6,465,551 (Zhao et al., granted to Milliken); salts of certain cyclic dicarboxylic acids having a hexahydrophthalic acid structure (or “HHPA” structure), such as those disclosed in U.S. Patent 6,599,971 (Dotson et al., granted to Milliken); and phosphate esters, such as those disclosed in U.S. Patent 5,342,868 and those sold by Asahi Denka Kogyo under the trade names NA-11 and NA-21, cyclic dicarboxylic acid esters of the HHPA structure disclosed in U.S. Patent 6,599,971, and their salts, such as divalent metal or metalloid salts (especially calcium salts). For clarity, the HHPA structure comprises a ring having six carbon atoms and two carboxylic acid groups as substituents on adjacent atoms of the ring structure. The other four carbon atoms in the ring can be substituted, as disclosed in U.S. Patent 6,599,971. One example is calcium 1,2-cyclohexanedicarboxylate (CAS Registry No. 491589-22-1). Other examples of nucleating agents that can be added to the second polyethylene include those disclosed in WO2015042561, WO2015042563, WO2015042562, and WO2011050042.
[0232] Another commercially available nucleating agent that can be added to the second polyethylene in one embodiment of this disclosure is talc (as...). AG 609 for sale).
[0233] A commercially available nucleating agent that can be added to the second polyethylene in one embodiment of this disclosure is NA 287.
[0234] A commercially available nucleating agent that can be added to the second polyethylene in one embodiment of this disclosure is 210M.
[0235] Many of the aforementioned nucleating agents may be difficult to mix with the nucleating second polyethylene, and it is known to use dispersing aids such as zinc stearate to alleviate this problem.
[0236] In one embodiment of this disclosure, the nucleating agent is well dispersed in the second polyethylene.
[0237] In one embodiment of this disclosure, the amount of nucleating agent used is relatively small—from 100 to 3,000 parts per million by weight (based on the weight of the polymer), and those skilled in the art will understand that care should be taken to ensure good dispersion of the nucleating agent. In one embodiment of this disclosure, the nucleating agent is added to the second polyethylene in a finely ground form (less than 50 micrometers, particularly less than 10 micrometers) to promote mixing. This type of “physical blend” (i.e., a mixture of the nucleating agent and the resin in solid form) is preferred in some embodiments over the use of a “masterbatch” of nucleating agent (where the term “masterbatch” refers to the practice of first melt-mixing the additive (in this example, the nucleating agent) with a small amount of the second polyethylene, and then melt-mixing the “masterbatch” with the remaining second polyethylene).
[0238] In one embodiment of this disclosure, an additive, such as a nucleating agent, may be added to the second polyethylene as a “masterbatch,” wherein the term “masterbatch” refers to the practice of first melt-mixing the additive (e.g., a nucleating agent) with a small amount of the second polyethylene, and then melt-mixing the “masterbatch” with the remaining second polyethylene.
[0239] In one embodiment of this disclosure, the second polyethylene comprises a nucleating agent or a mixture of nucleating agents.
[0240] In one embodiment of this disclosure, the nucleating agent or mixture of nucleating agents comprises a salt of dicarboxylic acid.
[0241] In one embodiment, the nucleating agent or nucleating mixture comprises 1,2-cyclohexanedicarboxylic acid in the form of a calcium salt (CAS Registry No. 491589-22-1).
[0242] In one embodiment, the nucleating agent or mixture of nucleating agents is 1,2-cyclohexanedicarboxylic acid in the form of a calcium salt mixed with zinc stearate (CAS Registry No. 491589-22-1).
[0243] In the embodiments, the nucleating agent or mixture of nucleating agents is added in an amount of 50 to 5,000 ppm, or 100 to 4,000 ppm, or 200 to 4,000 ppm, or 100 to 3,000 ppm, or 200 to 3,000 ppm, or 100 to 2,000 ppm, or 200 to 2,000 ppm, or 500 to 5,000 ppm, or 500 to 4,000 ppm, or 500 to 3,000 ppm, or 500 to 2,000 ppm, or 500 to 1,500 ppm based on the weight of the second polyethylene.
[0244] Third polyethylene
[0245] In embodiments of this disclosure, the density of the third polyethylene is lower than that of the first polyethylene.
[0246] In one embodiment of this disclosure, the third polyethylene is an ethylene copolymer.
[0247] In embodiments of this disclosure, the third polyethylene is selected from linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), very low-density polyethylene (VLDPE), and high-pressure low-density polyethylene (HPLDPE) prepared by ethylene free radical polymerization.
[0248] In embodiments of this disclosure, the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE).
[0249] In embodiments of this disclosure, the third polyethylene is a polymer blend comprising two or more polymer blend components selected from: linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), very low-density polyethylene (VLDPE), and high-pressure low-density polyethylene (HPLDPE) prepared by ethylene free radical polymerization.
[0250] Very low density polyethylene (VLDPE)
[0251] The terms "very low density polyethylene" and "VLDPE" as used in this article refer to polyethylene with a density of less than approximately 0.910 g / cm³. 3 or approximately 0.910 g / cm³ 3 Ethylene copolymer.
[0252] Very low density polyethylene includes plasmons and elastomers.
[0253] In the implementation scheme, the density of VLDPE is approximately 0.870 g / cm³. 3 Approximately 0.910 g / cm³ 3 or approximately 0.880 g / cm³ 3 Approximately 0.910 g / cm³ 3 or approximately 0.890 g / cm³ 3 Approximately 0.910 g / cm³ 3 .
[0254] In one embodiment of this disclosure, VLDPE is an ethylene copolymer comprising ethylene and an α-olefin selected from propylene, 1-butene, 1-hexene, 1-octene, and mixtures thereof as polymerizable monomers.
[0255] In one embodiment of this disclosure, VLDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerizable monomer.
[0256] In embodiments of this disclosure, the melt index I2 of VLDPE is about 0.5 to about 20 g / 10 min, or 0.5 to 10 g / 10 min.
[0257] In the implementation scheme, VLDPE can be homogeneous branched polyethylene.
[0258] In the implementation plan, VLDPE can be heterogeneous branched polyethylene.
[0259] In one embodiment of this disclosure, VLDPE is prepared using a multi-active-site catalyst.
[0260] In one embodiment of this disclosure, VLDPE is prepared using a Ziegler-Natta catalyst.
[0261] In one embodiment of this disclosure, VLDPE is prepared using a single-active-site catalyst.
[0262] In embodiments of this disclosure, VLDPE is prepared using a metallocene catalyst, a phosphine imide catalyst, or a confined geometry catalyst.
[0263] In one embodiment of this disclosure, VLDPE is prepared using a Ziegler-Natta catalyst in a solution-phase polymerization process.
[0264] In one embodiment of this disclosure, VLDPE is prepared by solution-phase polymerization using a single-active-site catalyst.
[0265] In embodiments of this disclosure, VLPDE has a melt index (I2) of 0.1 to 10 g / 10 min, or 0.9 to 2.3 g / 10 min, and a melt flow rate of about 0.890 to about 0.910 g / cm³. 3 The density.
[0266] Linear low-density polyethylene (LLDPE)
[0267] As used in this article, the terms "linear low-density polyethylene" and "LLDPE" refer to polyethylene with a density of approximately 0.910 g / cm³. 3 Approximately 0.935 g / cm³ 3 Polyethylene homopolymers or copolymers.
[0268] In one embodiment, LLDPE is a linear polymer containing a minimal or relatively small, or undetectable amount, of long-chain branches.
[0269] In one implementation, the LLDPE may contain long chain branches.
[0270] As used herein, "long-chain branching" refers to a branch with a chain length greater than any short-chain branch, resulting from the incorporation of comonomers. In embodiments, the length of the long-chain branching can be approximately the same as or equal to the length of the polymer backbone. Long-chain branching (LCB) can be determined using conventional techniques known in industry, such as 13C nuclear magnetic resonance (13C NMR) spectroscopy, and can be quantified using, for example, Randall's method (Rev. Macromol. Chem. Phys., C29(2&3), pp. 285-297). Two other methods that can be used include gel permeation chromatography coupled with a low-angle laser scattering detector (GPC-LALLS) and gel permeation chromatography coupled with a differential viscometer detector (GPC-DV). The detection of long-chain branching using these techniques and the underlying theory are well documented in the literature. For example, see Zimm, BH and Stockmayer, WH, J. Chem. Phys., 17, 1301 (1949) and Rudin A., Modern Methods of Polymer Characterization, John Wiley & Sons, New York (1991), pp. 103-112.
[0271] In the implementation scheme, linear low-density polyethylene can be replaced by an average of 0.001 long chain branches / 10,000 carbon to 3 long chain branches / 10,000 carbon, 0.001 long chain branches / 10,000 carbon to 1 long chain branch / 10,000 carbon, or 0.05 long chain branches / 10,000 carbon to 1 long chain branch / 10,000 carbon.
[0272] In other embodiments, the linear low-density polyethylene is replaced with an average of less than 1 long chain branch / 10,000 carbon, less than 0.5 long chain branches / 10,000 carbon, or less than 0.05 long chain branches / 10,000 carbon, or less than 0.01 long chain branches / 10,000 carbon.
[0273] In one embodiment of this disclosure, LLDPE is an ethylene copolymer.
[0274] In one embodiment, the LLDPE is an ethylene / α-olefin copolymer, wherein at least 50% by weight of the ethylene copolymer is polymerized ethylene. In a further embodiment, the LLDPE is an ethylene / α-olefin copolymer, wherein at least 60% by weight, or at least 70% by weight, or at least 80% by weight, or at least 90% by weight, or at least 95% by weight of the ethylene copolymer is polymerized ethylene.
[0275] In embodiments of this disclosure, LLDPE is an ethylene / α-olefin copolymer comprising less than 15 mol%, or less than 10 mol%, or less than 8 mol%, or less than 7 mol%, or less than 5 mol%, or less than 4 mol%, or less than 3 mol% of units derived from one or more α-olefin comonomers.
[0276] In embodiments of this disclosure, LLDPE is an ethylene / α-olefin copolymer comprising 0.5 to 15 mol%, or 0.5 to 12 mol%, or 0.5 to 10 mol%, or 0.5 to 8 mol%, or 0.5 to 5 mol%, or 0.5 to 3 mol%, or 1 to 12 mol%, or 1 to 10 mol%, or 1 to 8 mol%, or 1 to 5 mol%, or 2 to 12 mol%, or 2 to 10 mol%, or 2 to 8 mol%, or 2 to 5 mol%, or 3 to 12 mol%, or 3 to 10 mol%, or 3 to 7 mol% of units derived from one or more α-olefin comonomers.
[0277] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and an α-olefin selected from 1-butene, 1-hexene, 1-octene, and mixtures thereof as polymerizable monomers.
[0278] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and 1-butene as a polymerizable monomer.
[0279] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and 1-hexene as a polymerizable monomer.
[0280] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerizable monomer.
[0281] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerizable monomer.
[0282] In one embodiment, LLDPE has a content of approximately 0.910 g / cm³. 3 Approximately 0.935 g / cm³ 3 The density. In embodiments of this disclosure, LLDPE has a density of approximately 0.910 g / cm³. 3 or approximately 0.912 g / cm³ 3 or approximately 0.915 g / cm³ 3 or approximately 0.916 g / cm³ 3 or approximately 0.917 g / cm³ 3 or approximately 0.918 g / cm³ 3 The lowest value was approximately 0.927 g / cm³. 3or approximately 0.930 g / cm³ 3 or approximately 0.932 g / cm³ 3 Or approximately 0.935 g / cm³ 3 The LLDPE has a high density. In embodiments of this disclosure, the LLDPE has a density of approximately 0.910 g / cm³. 3 Approximately 0.935 g / cm³ 3 or approximately 0.910 g / cm³ 3 Approximately 0.932 g / cm³ 3 or approximately 0.912 g / cm³ 3 Approximately 0.935 g / cm³ 3 Or approximately 0.912 to 0.932 g / cm³ 3 or approximately 0.915 g / cm³ 3 Approximately 0.935 g / cm³ 3 or approximately 0.915 g / cm³ 3 Approximately 0.932 g / cm³ 3 Or approximately 0.915 to approximately 0.930 g / cm³ 3 Or approximately 0.916 to approximately 0.935 g / cm³ 3 Or approximately 0.916 to approximately 0.932 g / cm³ 3 Or approximately 0.916 to approximately 0.930 g / em 3 Or approximately 0.915 to approximately 0.927 g / em 3 Or 0.915 to approximately 0.925 g / cm³ 3 or approximately 0.916 to approximately 0.924 g / cm³ 3 Or 0.920 to 0.935 g / cm³ 3 Or approximately 0.920 to 0.932 g / cm³ 3 The density.
[0283] In one embodiment of this disclosure, the LLDPE has a molecular weight distribution (Mw / Mn) of 10.0 or less. In further embodiments of this disclosure, the LLDPE has a molecular weight distribution (Mw / Mn) of 9.0 or less, 8.0 or less, 7.0 or less, or 6.0 or less.
[0284] In one embodiment of this disclosure, the LLDPE has a molecular weight distribution (Mw / Mn) of about 1.6 to about 6.0.
[0285] In embodiments of this disclosure, LLDPE has a molecular weight distribution (Mw / Mn) ranging from a low of about 1.6, or about 1.7, or about 2.0, or about 2.5, or about 3.0, or about 3.5 to a high of about 4.5, or about 5.0, or about 5.25, or about 5.5, or about 6.0. In embodiments of this disclosure, LLDPE has a molecular weight distribution (Mw / Mn) ranging from about 1.7 to about 5.5, or about 1.7 to 5.0, or about 1.7 to about 4.5, or about 1.7 to about 4.0, or about 1.8 to about 3.5, or about 2.0 to about 3.0, or about 2.0 to about 10.0, or about 2.0 to about 9.0, or about 2.0 to about 8.0, or about 2.0 to about 7.0, or about 2.0 to about 6.0, or about 2.0 to about 5.0, or about 2.0 to about 4.0, or about 2.0 to about 3.5, or about 2. Molecular weight distribution (Mw / Mn) of 5 to 10.0, or about 2.5 to 9.0, or about 2.5 to 8.0, or about 2.5 to 7.0, or about 2.5 to 6.0, or about 2.5 to 5.0, or about 2.5 to 4.0, or about 2.5 to 3.5, or about 3.0 to 10.0, or about 3.0 to 9.0, or about 3.0 to 8.0, or about 3.0 to 7.0, or about 3.0 to 6.0, or about 3.0 to 5.0, or about 3.0 to 4.0.
[0286] In some embodiments, LLDPE may have a Z-mean molecular weight distribution Mz / Mw ratio of 1.5 to 6.0, including all values and sub-ranges covered by this range. For example, in a further embodiment, LLDPE may have a Z-mean molecular weight distribution Mz / Mw ratio of 1.5, or 1.75, or 2.0, or 2.5, or 2.75, or 3.0, or 3.5 to 2.0, or 2.5, or 3.0, or 3.5, or 4.0, or 4.5, or 5.0, or 5.5, or 6.0. In some embodiments, LLDPE has a Z-mean molecular weight distribution Mz / Mw ratio of 1.5 to 5.5, or 1.5 to 5.0, or 1.5 to 4.0, or 1.5 to 3.5, or 1.5 to 3.0, or 1.5 to 2.5.
[0287] In embodiments of this disclosure, LLDPE may be single-peaked, bimodal, or multimodal in gel permeation chromatography (GPC) analysis. The term "single-peaked" is defined herein as indicating the presence of only one significant peak or maximum value in a molecular weight distribution curve generated according to the method of ASTM D6474-99. Conversely, the term "bimodal" is used to express that, in addition to the first peak, there will be a second peak or shoulder representing a higher or lower molecular weight component (i.e., a molecular weight distribution curve, which can be said to have two maximum values). Alternatively, the term "bimodal" indicates the presence of two maximum values in a molecular weight distribution curve generated according to the method of ASTM D6474-99. The term "multimodal" indicates the presence of two or more, typically more than two, maximum values in a molecular weight distribution curve generated according to the method of ASTM D6474-99.
[0288] In one embodiment of this disclosure, LLDPE has a melt index (I2) of about 0.1 g / 10 min to about 20 g / 10 min. In another embodiment of this disclosure, LLDPE has a melt index (I2) of about 0.75 g / 10 min to about 15 g / 10 min, or about 0.85 g / 10 min to about 10 g / 10 min, or about 0.9 g / 10 min to about 8 g / 10 min. In yet another embodiment of this disclosure, LLDPE has a melt index (I2) of a low value of about 0.20 g / 10 min, or about 0.25 g / 10 min, or about 0.5 g / 10 min, or about 0.75 g / 10 min, or about 1 g / 10 min, or about 2 g / 10 min to a high value of about 3 g / 10 min, or about 4 g / 10 min, or about 5 g / 10 min, or about 10 g / 10 min.
[0289] In embodiments of this disclosure, LLDPE has a melt index (I2) of 0.1 to 10 g / 10 min, or 0.5 to 10.0 g / 10 min, or 0.5 to 5.0 g / 10 min, or 0.8 to 5.0 g / 10 min, or 0.8 to 10 g / 10 min.
[0290] In embodiments of this disclosure, LLDPE has a melt index (I2) of about 0.75 g / 10 min to about 6 g / 10 min, or about 1 g / 10 min to about 8 g / 10 min, or about 0.8 g / 10 min to about 6 g / 10 min, or about 1 g / 10 min to about 4.5 g / 10 min, or about 0.20 g / 10 min to about 5.0 g / 10 min, or about 0.30 g / 10 min to about 5.0 g / 10 min, or about 0.40 g / 10 min to about 5.0 g / 10 min, or about 0.50 g / 10 min to about 5.0 g / 10 min, or 0.5 to 2.5 g / 10 min, or 0.5 to 2.0 g / 10 min.
[0291] In embodiments of this disclosure, LLDPE may have a melt flow ratio of 20 to 80. 21 / I2, including all values and sub-ranges covered by this range. For example, in a further embodiment, LLDPE may have a melt index ratio of 20 to 75, or 20 to 70, or 20 to 65, or 20 to 60, or 20 to 55, or 20 to 50, or 25 to 75, or 25 to 70, or 25 to 65, or 25 to 60, or 25 to 55, or 25 to 50, or 30 to 80, or 30 to 75, or 30 to 70, or 30 to 65, or 30 to 60, or 30 to 55, or 30 to 50, or 35 to 80, or 35 to 75, or 35 to 70, or 35 to 65, or 35 to 60, or 35 to 55 g / 10min. 21 / I2.
[0292] In other embodiments, LLDPE may have a melt flow ratio I of less than 50, less than 47, less than 45, less than 42, less than 40, less than 35, or less than 30. 21 / I2. In a further embodiment, the LLDPE may have a melt index ratio of 20 to 40, or 20 to 37, or 22 to 37, or 22 to 35, or 25 to 35, or 25 to 30. 21 / I2.
[0293] In embodiments of this disclosure, the LLDPE has a melt flow ratio (IL) of less than about 36, or less than about 35, or less than about 32, or less than about 30, or less than about 28, or less than about 26, or less than about 24, or less than about 22, or less than about 20. 21 / I2). In embodiments of this disclosure, LLDPE has a melt flow ratio (I) of about 16 to about 36, or about 16 to about 35, or about 16 to about 32, or about 16 to about 30, or about 18 to about 35, or about 18 to about 32, or about 18 to about 30, or about 16 to about 27, or about 16 to about 25, or about 16 to about 22, or about 16 to about 20. 21 / I2).
[0294] In one embodiment of this disclosure, the LLDPE has ≥ about 50% by weight CBDI 50 Or ≤ 50% by weight of CBDI 50 For example, as determined by TREF analysis.
[0295] In embodiments disclosed herein, the LLDPE has a compositional distribution width index (CDBI) of about 25 wt% to about 95 wt%, or about 35 wt% to about 90 wt%, or about 40 wt% to about 85 wt%, or about 40 wt% to about 80 wt%. 50 For example, as determined by temperature elution fractionation (TREF).
[0296] In embodiments of this disclosure, LLDPE can be prepared using gas-phase polymerization, solution-phase polymerization, or slurry-phase polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art (e.g., fluidized bed gas-phase reactor, circulating reactor, stirred tank reactor, and batch reactor; and the reactors can be connected in series or in parallel, or any combination thereof).
[0297] In embodiments of this disclosure, LLDPE has a melt index (I2) of 0.1 to 10 g / 10 min, or 0.9 to 2.3 g / 10 min, and a melt flow rate of about 0.910 to about 0.935 g / cm³. 3 The density.
[0298] In the implementation plan, LLDPE can be homogeneous branched polyethylene.
[0299] In the implementation plan, LLDPE can be heterogeneous branched polyethylene.
[0300] In one embodiment of this disclosure, LLDPE is prepared using a multi-active-site catalyst.
[0301] In one embodiment of this disclosure, LLDPE is prepared using a Ziegler-Natta catalyst.
[0302] In one embodiment of this disclosure, LLDPE is prepared using a single-active-site catalyst.
[0303] In embodiments of this disclosure, LLDPE is prepared using a metallocene catalyst, a phosphine imide catalyst, or a confined geometry catalyst.
[0304] In one embodiment of this disclosure, LLDPE is prepared using a Ziegler-Natta catalyst in a solution-phase polymerization process.
[0305] In one embodiment of this disclosure, LLDPE is prepared by solution-phase polymerization using a single-active-site catalyst.
[0306] In one embodiment of this disclosure, LLDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerization monomer, having a density of 0.910 to 0.935 g / cm3 and a melt index I2 of 0.8 to 10 g / 10 min.
[0307] Medium-density polyethylene (MDPE)
[0308] The terms "medium-density polyethylene" and "MDPE" used in this article refer to polyethylene with a density of approximately 0.936 g / cm³. 3 Approximately 0.949 g / cm³ 3 Polyethylene homopolymers or copolymers.
[0309] In one embodiment of this disclosure, MDPE is an ethylene copolymer.
[0310] In one embodiment of this disclosure, MDPE is an ethylene copolymer comprising ethylene and an α-olefin selected from 1-butene, 1-hexene, 1-octene, and mixtures thereof as polymerizable monomers.
[0311] In one embodiment of this disclosure, MDPE is an ethylene copolymer comprising ethylene and 1-butene as a polymerizable monomer.
[0312] In one embodiment of this disclosure, MDPE is an ethylene copolymer comprising ethylene and 1-hexene as a polymerizable monomer.
[0313] In one embodiment of this disclosure, MDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerizable monomer.
[0314] In one embodiment of this disclosure, MDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerization monomer.
[0315] In one embodiment, MDPE has a concentration of approximately 0.936 g / cm³. 3 Approximately 0.949 g / cm³ 3 The density. In embodiments of this disclosure, MDPE has a density of approximately 0.936 g / cm³. 3 or approximately 0.938 g / cm³3 or approximately 0.940 g / cm³ 3 The lowest value was approximately 0.949 g / cm³. 3 or approximately 0.947 g / cm³ 3 or approximately 0.945 g / cm³ 3 or approximately 0.942 g / cm³ 3 The MDPE has a high density. In embodiments of this disclosure, the MDPE has a density of approximately 0.936 g / cm³. 3 Approximately 0.948 g / cm³ 3 or approximately 0.936 g / cm³ 3 Approximately 0.946 g / cm³ 3 or approximately 0.938 g / cm³ 3 Approximately 0.948 g / cm³ 3 Or approximately 0.938 to 0.946 g / cm³ 3 or approximately 0.940 g / cm³ 3 Approximately 0.949 g / cm³ 3 or approximately 0.940 g / cm³ 3 Approximately 0.948 g / cm³ 3 Or approximately 0.940 to approximately 0.946 g / cm³ 3 Or approximately 0.936 to approximately 0.945 g / cm³ 3 Or approximately 0.938 to approximately 0.945 g / cm³ 3 Or 0.940 to approximately 0.945 g / cm³ 3 The density.
[0316] In one embodiment of this disclosure, MDPE has a molecular weight distribution (Mw / Mn) of 10.0 or less. In further embodiments of this disclosure, MDPE has a molecular weight distribution (Mw / Mn) of 9.0 or less, 8.0 or less, 7.0 or less, or 6.0 or less.
[0317] In one embodiment of this disclosure, MDPE has a molecular weight distribution (Mw / Mn) of about 1.6 to about 8.0.
[0318] In embodiments of this disclosure, MDPE has a molecular weight distribution (Mw / Mn) of low values of about 1.6, or about 1.7, or about 2.0, or about 2.5, or about 3.0, or about 3.5, and high values of about 4.5, or about 5.0, or about 5.25, or about 5.5, or about 6.0, or about 7.0, or about 8.0. In embodiments of this disclosure, the MDPE has a density of about 1.7 to about 5.5, or about 1.7 to 5.0, or about 1.7 to about 4.5, or about 1.7 to about 4.0, or about 1.8 to about 3.5, or about 2.0 to about 3.0, or about 2.0 to about 10.0, or about 2.0 to about 9.0, or about 2.0 to about 8.0, or about 2.0 to about 7.0, or about 2.0 to about 6.0, or about 2.0 to about 5.0, or about 2.0 to about 4.0, or about 2.0 to about 3.5, or about 2. Molecular weight distribution (Mw / Mn) of 5 to 10.0, or about 2.5 to 9.0, or about 2.5 to 8.0, or about 2.5 to 7.0, or about 2.5 to 6.0, or about 2.5 to 5.0, or about 2.5 to 4.0, or about 2.5 to 3.5, or about 3.0 to 10.0, or about 3.0 to 9.0, or about 3.0 to 8.0, or about 3.0 to 7.0, or about 3.0 to 6.0, or about 3.0 to 5.0, or about 3.0 to 4.0.
[0319] In some embodiments, MDPE may have a Z-mean molecular weight distribution Mz / Mw ratio of 1.5 to 6.0, including all values and sub-ranges covered by this range. For example, in a further embodiment, MDPE may have a Z-mean molecular weight distribution Mz / Mw ratio of 1.5, or 1.75, or 2.0, or 2.5, or 2.75, or 3.0, or 3.5 to 2.0, or 2.5, or 3.0, or 3.5, or 4.0, or 4.5, or 5.0, or 5.5, or 6.0. In some embodiments, MDPE has a Z-mean molecular weight distribution Mz / Mw ratio of 1.5 to 5.5, or 1.5 to 5.0, or 1.5 to 4.0, or 1.5 to 3.5, or 1.5 to 3.0, or 1.5 to 2.5.
[0320] In embodiments of this disclosure, MDPE can be single-peaked, bimodal, or multimodal in gel permeation chromatography (GPC) analysis. The term "single-peaked" is defined herein as indicating the presence of only one significant peak or maximum value in a molecular weight distribution curve generated according to the method of ASTM D6474-99. Conversely, the term "bimodal" is used to express that, in addition to the first peak, there will be a second peak or shoulder representing a higher or lower molecular weight component (i.e., a molecular weight distribution curve, which can be said to have two maximum values). Alternatively, the term "bimodal" indicates the presence of two maximum values in a molecular weight distribution curve generated according to the method of ASTM D6474-99. The term "multimodal" indicates the presence of two or more, typically more than two, maximum values in a molecular weight distribution curve generated according to the method of ASTM D6474-99.
[0321] In one embodiment of this disclosure, MDPE has a melt index (I2) of about 0.1 g / 10 min to about 20 g / 10 min. In another embodiment of this disclosure, MDPE has a melt index (I2) of about 0.75 g / 10 min to about 15 g / 10 min, or about 0.85 g / 10 min to about 10 g / 10 min, or about 0.9 g / 10 min to about 8 g / 10 min. In yet another embodiment of this disclosure, MDPE has a melt index (I2) of a low value of about 0.20 g / 10 min, or about 0.25 g / 10 min, or about 0.5 g / 10 min, or about 0.75 g / 10 min, or about 1 g / 10 min, or about 2 g / 10 min to a high value of about 3 g / 10 min, or about 4 g / 10 min, or about 5 g / 10 min, or about 10 g / 10 min.
[0322] In embodiments of this disclosure, MDPE has a melt index (I2) of 0.1 to 10 g / 10 min, or 0.5 to 10.0 g / 10 min, or 0.5 to 5.0 g / 10 min, or 0.8 to 5.0 g / 10 min.
[0323] In embodiments of this disclosure, MDPE has a melt index (I2) of about 0.75 g / 10 min to about 6 g / 10 min, or about 1 g / 10 min to about 8 g / 10 min, or about 0.8 g / 10 min to about 6 g / 10 min, or about 1 g / 10 min to about 4.5 g / 10 min, or about 0.20 g / 10 min to about 5.0 g / 10 min, or about 0.30 g / 10 min to about 5.0 g / 10 min, or about 0.40 g / 10 min to about 5.0 g / 10 min, or about 0.50 g / 10 min to about 5.0 g / 10 min, or 0.5 to 2.5 g / 10 min, or 0.5 to 2.0 g / 10 min.
[0324] In embodiments of this disclosure, MDPE may have a melt flow ratio of 20 to 80. 21 / I2, including all values and sub-ranges covered by this range. For example, in a further embodiment, MDPE may have a melt index ratio of 20 to 75, or 20 to 70, or 20 to 65, or 20 to 60, or 20 to 55, or 20 to 50, or 25 to 75, or 25 to 70, or 25 to 65, or 25 to 60, or 25 to 55, or 25 to 50, or 30 to 80, or 30 to 75, or 30 to 70, or 30 to 65, or 30 to 60, or 30 to 55, or 30 to 50, or 35 to 80, or 35 to 75, or 35 to 70, or 35 to 65, or 35 to 60, or 35 to 55 g / 10min. 21 / I2.
[0325] In other embodiments, MDPE may have a melt flow ratio I of less than 50, less than 47, less than 45, less than 42, less than 40, less than 35, or less than 30. 21 / I2. In a further embodiment, MDPE may have a melt index ratio of 20 to 40, 20 to 37, 22 to 37, 22 to 35, 25 to 35, or 25 to 30. 21 / I2.
[0326] In embodiments of this disclosure, MDPE has a melt flow ratio (IL) of less than about 36, or less than about 35, or less than about 32, or less than about 30, or less than about 28, or less than about 26, or less than about 24, or less than about 22, or less than about 20. 21 / I2). In embodiments of this disclosure, MDPE has a melt flow ratio (I) of about 16 to about 36, or about 16 to about 35, or about 16 to about 32, or about 16 to about 30, or about 18 to about 35, or about 18 to about 32, or about 18 to about 30, or about 16 to about 27, or about 16 to about 25, or about 16 to about 22, or about 16 to about 20.21 / I2).
[0327] In embodiments disclosed herein, the MDPE has ≥ about 50% by weight CBDI 50 Or ≤ 50% by weight of CBDI 50 For example, as determined by TREF analysis.
[0328] In embodiments of this disclosure, MDPE has a compositional distribution width index (CDBI) of about 25 wt% to about 95 wt%, or about 35 wt% to about 90 wt%, or about 40 wt% to about 85 wt%, or about 40 wt% to about 80 wt%. 50 For example, as determined by temperature elution fractionation (TREF).
[0329] In embodiments of this disclosure, MDPE can be prepared using gas-phase polymerization, solution-phase polymerization, or slurry-phase polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art (e.g., fluidized bed gas-phase reactor, circulating reactor, stirred tank reactor, and batch reactor; and the reactors can be connected in series or in parallel, or any combination thereof).
[0330] In embodiments of this disclosure, MDPE has a melt index (I2) of 0.1 to 10 g / 10 min, or 0.9 to 2.3 g / 10 min, and a melt density of about 0.936 to about 0.949 g / cm³. 3 The density.
[0331] In the implementation plan, MDPE can be homogeneous branched polyethylene.
[0332] In the implementation plan, MDPE can be heterogeneous branched polyethylene.
[0333] In one embodiment of this disclosure, MDPE is prepared using a multi-active-site catalyst.
[0334] In one embodiment of this disclosure, MDPE is prepared using a Ziegler-Natta catalyst.
[0335] In one embodiment of this disclosure, MDPE is prepared using a single-active-site catalyst.
[0336] In embodiments of this disclosure, MDPE is prepared using a metallocene catalyst, a phosphine imide catalyst, or a confined geometry catalyst.
[0337] In one embodiment of this disclosure, MDPE is prepared using a Ziegler-Natta catalyst in a solution-phase polymerization process.
[0338] In one embodiment of this disclosure, MDPE is prepared by solution-phase polymerization using a single-active-site catalyst.
[0339] In one embodiment, MDPE is an ethylene copolymer comprising ethylene and 1-octene as a polymerization monomer, having a density of 0.936 to 0.949 g / cm³. 3 The melt index I2 is 0.8 to 10 g / 10 min.
[0340] Other additives
[0341] In embodiments of this disclosure, the first, second, or third polyethylene may contain conventional additives selected from: primary antioxidants (e.g., hindered phenols, including vitamin E); secondary antioxidants (e.g., phosphites and phosphonites); UV absorbers and light stabilizers; processing aids (e.g., processing aids combined with fluorinated elastomers and / or polyethylene glycol); slip agents; fillers, anti-blocking agents, and reinforcing agents; or other miscellaneous additives.
[0342] Further details of other additives added to the first, second, or third polyethylene according to embodiments of this disclosure are provided below.
[0343] In embodiments of this disclosure, the amount of other additives may also be 100 to 5,000 ppm, or 100 to 3,000 ppm, or 200 to 3,000 ppm, or 200 to 2,000 ppm (based on the weight of the polymer).
[0344] Main antioxidants
[0345] In embodiments of this disclosure, the primary antioxidant is selected from alkylated monophenols, such as: 2,6-di-tert-butyl-4-methylphenol; 2-tert-butyl-4,6-dimethylphenol; 2,6-di-tert-butyl-4-ethylphenol; 2,6-di-tert-butyl-4-n-butylphenol; 2,6-di-tert-butyl-4-isobutylphenol; 2,6-dicyclopentyl-4-methylphenol; 2-(α-methylcyclohexyl)-4,6-dimethylphenol; 2,6-di-octadecyl-4-methylphenol; 2,4,6-tricyclohexylphenol; and 2,6-di-tert-butyl-4-methoxymethylphenol.
[0346] In embodiments of this disclosure, the primary antioxidant is selected from alkylated hydroquinones, such as 2,6-di-tert-butyl-4-methoxyphenol; 2,5-di-tert-butylhydroquinone; 2,5-di-tert-pentylhydroquinone; and 2,6-diphenyl-4-octadecyloxyphenol.
[0347] In embodiments of this disclosure, the primary antioxidant is selected from hydroxylated thiodiphenyl ethers, such as 2,2′-thio-bis-(6-tert-butyl-4-methylphenol); 2,2′-thio-bis-(4-octylphenol); 4,4′-thio-bis-(6-tert-butyl-3-methylphenol); and 4,4′-thio-bis-(6-tert-butyl-2-methylphenol).
[0348] In embodiments of this disclosure, the primary antioxidant is selected from alkylene bisphenols, such as 2,2′-methylene-bis-(6-tert-butyl-4-methylphenol); 2,2′-methylene-bis-(6-tert-butyl-4-ethylphenol); 2,2′-methylene-bis-(4-methyl-6-(α-methylcyclohexyl)phenol); 2,2′-methylene-bis-(4-methyl-6-cyclohexylphenol); 2,2′-methylene-bis-(6-nonyl-4-methyl)phenol. 2,2′-Methylene-bis-(6-nonyl-4-methylphenol); 2,2′-Methylene-bis-(6-(α-methylbenzyl)-4-nonylphenol); 2,2′-Methylene-bis-(6-(α,α-dimethylbenzyl)-4-nonylphenol); 2,2′-Methylene-bis-(4,6-di-tert-butylphenol); 2,2′-Ethylene-bis-(6-tert-butyl-4-isobutylphenol); 4,4′-Methylene-bis(2,6- 4,4′-Methylene-bis-(6-tert-butyl-2-methylphenol); 1,1-bis-(5-tert-butyl-4-hydroxy-2-methylphenol)butane; 2,6-di-(3-tert-butyl-5-methyl-2-hydroxybenzyl)-4-methylphenol; 1,1,3-tris-(5-tert-butyl-4-hydroxy-2-methylphenyl)butane; 1,1-bis-(5-tert-butyl-4-hydroxy-2-methylphenyl)-3-dodecyl- Mercaptobutane; ethylene glycol-bis-(3,3'-bis-(3′-tert-butyl-4′-hydroxyphenyl)-butyrate)-bis-(3-tert-butyl-4-hydroxy-5-methylpentyl)-dicyclopentadiene; bis-(2-(3′-tert-butyl-2′-hydroxy-5′-methylbenzyl)-6-tert-butyl-4-methylphenyl) terephthalate; and other phenolic substances, such as monoacrylates of bisphenols, such as ethylene bis-2,4-ditert-butylphenol monoacrylate.
[0349] In embodiments of this disclosure, the amount of the primary antioxidant may be 100 to 5,000 ppm, or 100 to 3,000 ppm, or 200 to 3,000 ppm, or 200 to 2,000 ppm (based on the weight of the polymer).
[0350] Co-oxidants
[0351] In embodiments of this disclosure, the auxiliary antioxidant is selected from phosphites and phosphonates, such as triphenyl phosphite; diphenylalkyl phosphate; phenyl dialkyl phosphate; tri(nonylphenyl) phosphite; trilauryl phosphite; tri(octadecyl) phosphite; distearyl pentaerythritol diphosphite; tris(2,4-di-tert-butylphenyl) phosphite; diisodecyl pentaerythritol diphosphite; 2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl-1,3-propanediol phosphite; bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite; tripearyl sorbitol triphosphite; and tetra(2,4-di-tert-butylphenyl)4,4′-biphenyl diphosphite.
[0352] In embodiments of this disclosure, the auxiliary antioxidant is selected from hydroxylamines and amine oxides, such as N,N-dibenzylhydroxylamine; N,N-diethylhydroxylamine; N,N-dioctylhydroxylamine; N,N-dilaurylhydroxylamine; N,N-bistetradecylhydroxylamine; N,N-bishexadecylhydroxylamine; N,N-bisoctadecylhydroxylamine; N-hexadecyl-N-octadecylhydroxylamine; N-heptadecyl-N-octadecylhydroxylamine; and N,N-dialkylhydroxylamine derived from hydrogenated tallow amine. Similar amine oxides are also suitable.
[0353] In embodiments of this disclosure, the amount of auxiliary antioxidant may also be 100 to 5,000 ppm, or 100 to 3,000 ppm, or 200 to 3,000 ppm, or 200 to 2,000 ppm (based on the weight of the polymer).
[0354] UV absorbers and light stabilizers
[0355] In embodiments of this disclosure, the UV absorber or light stabilizer is selected from 2-(2′-hydroxyphenyl)-benzotriazoles, such as 5′-methyl-, 3′,5′-di-tert-butyl-, 5′-tert-butyl-5′(1,1,3,3-tetramethylbutyl)-, 5-chloro-3′,5′-di-tert-butyl-, 5-chloro-3′-tert-butyl-5′-methyl-3′-sec-butyl-5′-tert-butyl-, 4′-octoxy, 3′,5′-di-tert-pentyl-3′,5′-bis-(α,α-dimethylbenzyl)- derivatives.
[0356] In embodiments of this disclosure, the UV absorber or light stabilizer is selected from 2-hydroxybenzophenones, such as 4-hydroxy-4-methoxy-, 4-octoxy, 4-decoxy-, 4-dodecoxy-, 4-benzyloxy, 4,21,4′-trihydroxy- and 2′-hydroxy-4,4′-dimethoxy derivatives.
[0357] In embodiments of this disclosure, the UV absorber or light stabilizer is selected from sterically hindered amines, such as bis(2,2,6,6-tetramethylpiperidinyl) sebacate; bis-5-(1,2,2,6,6-pentamethylpiperidinyl) sebacate; n-butyl-3,5-di-tert-butyl-4-hydroxybenzylmalonate bis(1,2,2,6,6-pentamethylpiperidinyl) ester; and the condensation product of 1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidine and succinic acid. The condensation products of N,N′-(2,2,6,6-tetramethylpiperidinyl)-hexamethylenediamine and 4-tert-octylamino-2,6-dichloro-1,3,5-s-triazine; tris-(2,2,6,6-tetramethylpiperidinyl)-hydantoin triacetate; tetra-(2,2,6,6-tetramethyl-4-piperidinyl)-1,2,3,4-butane-tetracarbonic acid; and 1,1′(1,2-ethylenediyl)-bis-(3,3,5,5-tetramethylpiperazinone). These amines are commonly referred to as HALS (hindered amine light stabilizers), including 2,2,6,6-tetramethylpiperidinol butanetetracarboxylate. Such amines include hydroxylamines derived from hindered amines, such as bis(1-hydroxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; 1-hydroxy-2,2,6,6-tetramethyl-4-benzoxypiperidine; 1-hydroxy-2,2,6,6-tetramethyl-4-(3,5-di-tert-butyl-4-hydroxyhydrocinnamoyloxy)-piperidine; and N-(1-hydroxy-2,2,6,6-tetramethyl-piperidin-4-yl)-ε-caprolactam.
[0358] Lubricant
[0359] In embodiments of this disclosure, the lubricant is selected from oleamide, erucamide, stearamide, and betaine.
[0360] Fillers, anti-blocking agents and reinforcing agents
[0361] In embodiments of this disclosure, the filler, anti-blocking agent, or reinforcing agent is selected from calcium carbonate; diatomaceous earth; natural and synthetic silica; silicates; glass fiber; asbestos; talc; kaolin; mica; barium sulfate; metal oxides and hydroxides; carbon black and graphite.
[0362] Miscellaneous Additives
[0363] In embodiments of this disclosure, the miscellaneous additives are selected from plasticizers; epoxidized vegetable oils, such as epoxidized soybean oil; lubricants; emulsifiers; pigments; fluorescent whitening agents; flame retardants; antistatic agents; antifogging agents; foaming agents; and thiosynergists, such as dilauryl thiodipropionate or distearate thiodipropionate.
[0364] The following embodiments are provided to illustrate selected embodiments of this disclosure; it should be understood that the provided embodiments do not limit the scope of the claims. Example
[0365] Polymer characterization and testing methods
[0366] Prior to testing, each polymer sample was conditioned at 23±2°C and 50±10% relative humidity for at least 24 hours, and subsequent tests were performed at 23±2°C and 50±10% relative humidity. In this document, the term "ASTM conditions" refers to a laboratory maintained at 23±2°C and 50±10% relative humidity; and the samples to be tested were conditioned in this laboratory for at least 24 hours prior to testing. ASTM stands for American Society for Testing and Materials.
[0367] density
[0368] Polymer density was determined using ASTM D792-13 (November 1, 2013).
[0369] Melt index
[0370] The polymer melt index was determined using ASTM D1238 (August 1, 2013). Melt indices I2, I6, and I... 10 and I 21 Measurements were taken at 190°C using weights of 2.16 kg, 6.48 kg, 10 kg, and 21.6 kg, respectively. In this document, the term "stress index" or its acronym "S.Ex." is defined by the following relationship:
[0371] S.Ex.=log(I6 / I2) / log(6480 / 2160)
[0372] Wherein I6 and I2 are melt flow rates measured at 190°C using loads of 6.48 kg and 2.16 kg, respectively. In this disclosure, the melt index is expressed in units of g / 10 min, g / 10 min, dg / min, or dg / min; these units are equivalent.
[0373] Neutron activation (elemental analysis)
[0374] The catalyst metal residue in the polymer was determined using neutron activation analysis (hereinafter referred to as NAA) as follows: Radiation vials (composed of ultrapure polyethylene, internal volume 7 mL) were filled with the polymer sample, and the sample weight was recorded. The sample was then placed into a SLOWPOKE tube using a pneumatic transfer system. TMThe reactor (Atomic Energy of Canada Limited, Ottawa, Ontario, Canada) is irradiated with short-half-life elements (e.g., Ti, V, Al, Mg, and Cl) for 30 to 600 seconds, or with long-half-life elements (e.g., Zr, Hf, Cr, Fe, and Ni) for 3 to 5 hours. The average thermal neutron flux within the reactor is 5 × 10⁻⁶. 11 / em 2 / s. After irradiation, the samples were removed from the reactor and aged to allow for radioactivity decay; short-lived elements were aged for 300 seconds, while long-lived elements were aged for several days. Following aging, the gamma-ray spectra of the samples were recorded using a germanium semiconductor gamma-ray detector (Ortec model GEM55185, Advanced Measurement Technology Inc., OakRidge, TN, USA) and a multichannel analyzer (Ortec model DSPEC Pro). The amount of each element in the sample was calculated from the gamma-ray spectra and recorded as parts per million relative to the total weight of the polymer sample. The NAA system was calibrated using Specpure standards (1000 ppm of a solution of the desired element (purity >99%)). 1 mL of the solution (of the element of interest) was aspirated onto a 15 mm × 800 mm rectangular filter paper and air-dried. The filter paper was then placed in a 1.4 mL polyethylene irradiation vial and analyzed using the NAA system. The standards were used to determine the sensitivity of the NAA process (in counts / µg).
[0375] Gel permeation chromatography (GPC)
[0376] Polymer sample (polymer) solutions (1 to 3 mg / mL) were prepared by heating the polymer in 1,2,4-trichlorobenzene (TCB) and rotating it on a wheel at 150 °C in an oven for 4 hours. An antioxidant (2,6-di-tert-butyl-4-methylphenol (BHT)) was added to the mixture to stabilize the polymer and prevent oxidative degradation. The BHT concentration was 250 ppm. The polymer solution was analyzed at 140 °C using a PL 220 high-temperature chromatography unit equipped with four Shodex columns (HT803, HT804, HT805, and HT806), with TCB as the mobile phase and a flow rate of 1.0 mL / min, using differential refractive index (DRI) as the concentration detector. BHT was added to the mobile phase at a concentration of 250 ppm to protect the GPC column from oxidative degradation. The sample injection volume was 200 μL. The GPC column was calibrated using a narrow-distribution polystyrene standard. As described in ASTM standard test method D6474-12 (December 2012), the Mark-Houwink equation is used to convert the molecular weight of polystyrene to that of polyethylene. GPC raw data is used... GPC software processing to generate molar mass average (M n M w M z ) and molar mass distribution (e.g., polydispersity, M w / M n In the polyethylene industry, the commonly used term equivalent to GPC is SEC, which stands for size exclusion chromatography.
[0377] GPC-FTIR
[0378] A polyethylene composition (polymer) solution (2 to 4 mg / mL) was prepared by heating the polymer in 1,2,4-trichlorobenzene (TCB) and rotating it on a wheel at 150°C in an oven for 4 hours. The antioxidant 2,6-di-tert-butyl-4-methylphenol (BHT) was added to the mixture to stabilize the polymer and prevent oxidative degradation. The BHT concentration was 250 ppm. The sample solution was chromatographically analyzed at 140°C on a Waters GPC 150C chromatographic unit equipped with four Shodex columns (HT803, HT804, HT805, and HT806) using TCB as the mobile phase at a flow rate of 1.0 mL / min. An FTIR spectrometer coupled to the chromatographic unit via a heated transfer line and a heated FTIR flow cell were used as the detection system. BHT was added to the mobile phase at a concentration of 250 ppm to protect the SEC column from oxidative degradation. The sample injection volume was 300 μL. The raw FTIR spectra were processed using OPUS FTIR software, and polymer concentration and methyl content were calculated in real time using Chemometric Software (PLS technology) associated with OPUS. Polymer concentration and methyl content were then acquired and baseline corrected using CIRRUS GPC software. The SEC column was calibrated using narrow-distribution polystyrene standards. The polystyrene molecular weight was converted to polyethylene molecular weight using the Mark-Houwink equation, as described in ASTM standard test method D6474. Comonomer content was calculated based on the polymer concentration and methyl content predicted by the PLS technology, as described in Paul J. DesLauriers, Polymer 43, pp. 159–170 (2002), which is incorporated herein by reference.
[0379] Short Chain Branch - GPC - FTIR
[0380] Short-chain branching per 1000 carbon atoms is measured relative to copolymer fractions of different molecular weights. When plotted on a semi-logarithmic scale, the slant lines (from low to high molecular weight fractions on the logarithmic x-axis and the number of short-chain branches on the vertical y-axis) represent the distribution of short-chain branching for different molecular weight fractions as determined by Fourier transform infrared (FTIR) spectroscopy. The GPC-FTIR method measures the total methyl content, which includes methyl groups located at the ends of each macromolecular chain, i.e., methyl terminal groups. Therefore, the raw GPC-FTIR data must be corrected by subtracting the contribution from the methyl terminal groups. More specifically, the raw GPC-FTIR data overestimate the amount of short-chain branching (SCB), and this overestimation increases as the molecular weight (M) decreases. In this disclosure, 2-methyl correction is used to correct the raw GPC-FTIR data. At a given molecular weight (M), the number of methyl terminal groups (N) E Calculate using the following equation: N E =28000 / M, and N is subtracted from the original GPC-FTIR data. E (M-dependent) to produce SCB / 1000C (2-methyl corrected) GPC-FTIR data.
[0381] Unsaturated content
[0382] The amount of unsaturated groups (i.e., double bonds) in the polyethylene composition was determined according to ASTM D3124-98 (Vinylene Unsaturation, March 2011) and ASTM D6248-98 (Vinyl and Trans Unsaturation, July 2012). Ethylene interpolymer samples: a) were first subjected to carbon disulfide extraction to remove additives that might interfere with the analysis; b) the samples (in granule, film, or particle form) were pressed into plates of uniform thickness (0.5 mm); and c) the plates were analyzed by FTIR.
[0383] Comonomer content: Fourier transform infrared (FTIR) spectroscopy
[0384] The amount of comonomer in the polyethylene composition was determined by FTIR and reported as the content of short-chain branched (SCB) molecules (number of methyl branches per 1000 carbon atoms) with dimensions CH3# / 1000C. This test was performed according to ASTM D6645-01 (2001) using compression-molded polymer sheets and a Thermo-Nicolet 750 Magna-IR spectrophotometer. Polymer sheets were prepared according to ASTM D4703-16 (April 2016) using a compression molding apparatus (Wabash-Genesis series press).
[0385] Differential scanning calorimetry (DSC)
[0386] DSC testing is typically performed according to ASTM D3418. This analysis is conducted by subjecting a polymer sample (5 to 10 mg, prepared in an aluminum dish) and a reference material (empty aluminum dish) to a constant rate of temperature change within the DSC cell. The actual temperatures of the sample and reference are monitored by the instrument as the sample temperature increases or decreases linearly over time. If the sample undergoes a transition, reaction, or transformation, its rate of temperature change will differ from that of the reference. The instrument is first calibrated with indium (TA Instruments Q2000); after calibration, the polymer sample is equilibrated at 0°C and then heated to 200°C at a heating rate of 10°C / min; the melt is then held isothermally at 200°C for five minutes; the melt is then cooled to 0°C at a cooling rate of 10°C / min and held at 0°C for five minutes; the sample is then heated to 200°C at a heating rate of 10°C / min. The temperature difference between the sample and the reference (DT = T) is then recorded. 参比物 -T 样品 Plot the temperature relative to the sample temperature to generate a differential thermal spectrum. From this graph, determine the melting peak temperature (°C), enthalpy of fusion (J / g), and crystallinity (%).
[0387] Dynamic mechanical analysis (DMA)
[0388] Oscillatory shear measurements were performed at small strain amplitudes in a N2 atmosphere at 190°C, with a strain amplitude of 10% and a frequency range of 0.02–126 rad / s, at 5 points per decade to obtain the linear viscoelastic function. Frequency sweep experiments were conducted using a TA Instruments DHR3 stress-controlled rheometer with a conical geometry having a 5° cone angle, a 137 μm intercept, and a 25 mm diameter. In this experiment, sinusoidal strain waves were applied, and the stress response was analyzed in terms of the linear viscoelastic function. The zero-shear rate viscosity (η0) based on the DMA frequency sweep results was predicted by either the Ellis model (see RBBird et al., “Dynamics of Polymer Liquids. Volume 1: Fluid Mechanics”, Wiley-Interscience Publications (1987), p. 228) or the Carreau-Yasuda model (see K. Yasuda (1979) PhD Thesis, IT Cambridge). Dynamic rheological data were analyzed using rheometer software (i.e., Rheometrics RHIOS V4.4 or Orchestrator software) to determine the melt elastic modulus G′ (G″ = 500) at a reference melt viscous modulus (G″) value of G″ = 500 Pa. If necessary, these values were obtained by interpolation between available data points using Rheometrics software.
[0389] Shear thinning index SHI (0.5,50) The complex viscosity is calculated as the ratio of the estimated complex viscosity at a shear stress of 0.5 kPa to that at a shear stress of 50 kPa. Shear thinning index (SHI) (0.5,50) This provides information about the shear-thinning behavior of the polymer melt. High values indicate a strong dependence of viscosity on changes in deformation rate (shear or frequency).
[0390] Capillary Rheology
[0391] Viscosity profiles of different resins at varying shear rates were obtained using rheological data from a Dynisco LCR7000 capillary rheometer. In the capillary extrusion rheometer, the material is held in a temperature-controlled cylinder and forced through a precisely sized die by a piston. The orifice size, die size, and piston speed determine the apparent rate of shear applied to the material, and the apparent shear stress is calculated using force and die size. Shear viscosity can be obtained using Poiseuille's law from the capillary flow method.
[0392]
[0393]
[0394] Where P = the pressure drop across the capillary (N / m) 2 R = radius of capillary (m); L = length of capillary (m); Q = volumetric flow rate (m³ / s). 3 / sec); σ s = Apparent shear stress;
[0395] The shear rate, shear stress, and shear viscosity determined using the Poiseuille equation are commonly referred to as apparent shear viscosity, shear stress, and shear rate. This is due to the fact that the non-Newtonian properties of most fluids and the pressure drop across the die inlet and outlet pressures are not considered. The test temperature was set at 200°C. In this evaluation, the capillary length used was 30.48 mm, and the die diameter was 1.524 mm.
[0396] melt strength
[0397] Melt strength was measured at 190°C using a Rosand RH-7 capillary rheometer (barrel diameter = 15 mm) with a flat die head having a 2-mm diameter and an L / D ratio of 10:1. Pressure sensor: 10,000 psi (68.95 MPa). Piston speed: 5.33 mm / min. Traction angle: 52°. Traction increment speed: 50 to 80 m / min 2 Or 65+15m / min 2 The polymer melt is extruded through a capillary die at a constant rate and then stretched at an increasing traction speed until it breaks. The maximum stable value of the force in the plateau region of the force-time curve is defined as the melt strength of the polymer.
[0398] Vicat softening point (temperature)
[0399] The Vicat softening point of the polymer samples was determined according to ASTM D1525-07 (released in December 2009). This test determines the temperature at which the specified penetration occurs when the sample is subjected to the ASTM D1525-07 test conditions, namely heating rate B (120 ± 10 °C / h and 938 g load (10 ± 0.2 N load)).
[0400] CYTSAF / TREF (CTREF)
[0401] The compositional width index (CDBI) of the polymer samples was measured using a CRYSTAF / TREF 200+ unit (CTREF) equipped with an IR detector. The acronym "TREF" stands for temperature-elution fractionation. CTREF was provided by Polymer Characterization, SA (Valencia Technology Park, Gustave Eiffel, 8, Paterna, E-46980, Valencia, Spain). CTREF operated in TREF mode, which produced the chemical composition of the polymer sample as a subset of the elution temperature, Co / Ho ratio (polymer / homopolymer ratio), and CDBI (compositional width index). 50 and CDBI 25 The polymer sample (80 to 100 mg) was placed in a CTREF reactor vessel. The reactor vessel was filled with 35 mL of 1,2,4-trichlorobenzene (TCB), and the polymer was dissolved by heating the solution to 150 °C for 2 hours. Aliquots (1.5 mL) of the solution were then loaded into a CTREF column packed with stainless steel beads. The column containing the sample was stabilized at 110 °C for 45 minutes. The polymer was then crystallized from the solution by cooling the column to 30 °C at a cooling rate of 0.09 °C / min. The column was then equilibrated at 30 °C for 30 minutes. The crystallized polymer was then eluted from the column with TCB flowing through it at 0.75 mL / min, while the column was slowly heated from 30 °C to 120 °C at a heating rate of 0.25 °C / min. The raw CTREF data were processed using PolymerChar software, Excel spreadsheets, and the internally developed CTREF software. CDBI 50 Defined as the percentage of a polymer whose composition comprises within 50% of the median comonomer composition; CDBI 50 It is calculated from the composition distribution curve and the normalized cumulative integral of the composition distribution curve, as described in U.S. Patent 5,376,439. Those skilled in the art will understand that a calibration curve is needed to convert the CTREF elution temperature into comonomer content, i.e., the amount of comonomer in the ethylene / α-olefin polymer fraction eluted at a specific temperature. The generation of such calibration curves is described in the prior art, for example, Wild et al., J. Polym. Sci., Part B, Polym. Phys., Vol. 20(3), pp. 441-455; which is hereby fully incorporated by reference. CDBI 25 Calculated in a similar manner; CDBI 25Defined as the percentage of polymers whose composition is within 25% of the median comonomer composition. At the end of each sample run, the CTREF column was cleaned for 30 minutes; specifically, the CTREF column temperature was 160°C, and TCB was flowed through the column (0.5 mL / min) for 30 minutes.
[0402] Hexane extract
[0403] The hexane extractable was determined in accordance with Sections (c) 3.1 and 3.2 of 21 CFR 177.1520 of the Code of Federal Registration, wherein the amount of hexane extractable in the sample was determined by gravimetric analysis.
[0404] Membrane optics
[0405] The optical properties of the film were measured as follows: haze and transparency were measured according to ASTM D1003-13 (November 15, 2013).
[0406] Membrane mechanical properties
[0407] Tensile tests are typically performed according to ASTM D882 (ASTM D882-10 and ASTM D882-12) for longitudinal and transverse (MD and TD) tensile properties, respectively. The specimen width for tensile property measurements is 1.0 inch. The initial tensile speed is 1.0 inch / min to 5% strain, then the speed is increased to 20.0 inch / min until fracture. The clamp spacing is 2.0 inches. The mechanical properties measured are tensile fracture stress (reported in MPa), yield strain (%), yield stress (MPa), fracture strain (%), and fracture stress (MPa). The modulus of elasticity (MPa) is measured using a 1.0-inch wide specimen, a 2-inch clamp spacing, and a test speed of 1.0 inch / min.
[0408] Membrane thermal shrinkage rate (%)
[0409] Using a 10×10cm membrane sample, the sample was placed in an oven at 120°C for 5 minutes, and the shrinkage rate of the membrane was measured. The relative reduction in length of the heated membrane in both the longitudinal and transverse directions compared to the original membrane was reported as a percentage shrinkage rate.
[0410] (%) Shrinkage rate = (L 初始 -L 最终 ) / L 初始
[0411] Where L 初始 and L 最终 It refers to the length before and after heat treatment.
[0412] film thickness
[0413] The film thickness of a stretched multilayer film is measured according to ASTM D 6988-13.
[0414] First polyethylene
[0415] For use as a first polyethylene, the ethylene copolymer is prepared essentially according to the disclosure of co-pending Canadian patent application 3,102,574. The ethylene copolymer (used as the first polyethylene) is prepared using a multi-zone solution polymerization method, wherein three polymerization zones are arranged in series, each zone being defined by a different polymerization reactor (see...). Figure 1 The first polymerization zone is defined by a first tubular reactor (reactor 1); the second polymerization zone is defined by an optionally stirred tank reactor (reactor 2); and the third polymerization zone is defined by a second tubular reactor (reactor 3). Each reactor has an inlet and an outlet, with the process flow entering the reactor at the inlet and exiting at the outlet. For the tubular reactor, the inlet is located at the upstream end of the reactor, while the outlet is located at the downstream end. In the polymerization method of the present invention, the tank reactor (reactor 2), which receives the process flow from the first tubular reactor, although it is an optionally stirred tank reactor in which a stirrer is present, operates without stirring and thus functions as a plug flow reactor. Therefore, in this disclosure, the tank reactor optionally equipped with a stirrer is referred to as operating in "plug flow mode" when the stirrer is turned off.
[0416] The first tubular reactor (reactor 1) is a 6-inch diameter pipe, 36.6 meters long, with a total volume of 500 liters. At the beginning of the first tubular reactor (reactor 1), at the inlet of the tubular reactor ( Figure 1 Position A in the middle, along with solvent (cyclohexane), hydrogen, ethylene, and 1-butene, is injected into the Ziegler-Natta polymerization catalyst to initiate the polymerization reaction (Note: The Ziegler-Natta polymerization catalyst components, as further described below, are located immediately upstream of the inlet of the first tubular reactor). Figure 1 (Not shown in the image) are gathered together. Hydrogen is also fed to a second location in the first tubular reactor, approximately 50% of the length along the tubular reactor, downstream of the inlet ( Figure 1 (Position B in the diagram). In the solution-phase polymerization method of the present invention, as the process flow moves from the first tubular reactor to and into the tank reactor, and then into the second tubular reactor, the polymerization reaction continues along the entire length of the first tubular reactor (reactor 1), within the tank reactor (reactor 2), and then along the entire length of the second tubular reactor (reactor 3). Eight temperature indicators placed along the first tubular reactor are used to monitor the temperature distribution of the polymerization reaction.
[0417] Reactor 2 is a tank reactor (or "autoclave") with a volume of 3,640 liters and protected by a safety valve set at 19.1 MPa. The tank reactor vessel is made of carbon steel, with the inlet nozzle plated with Monel alloy. Four 11.4 cm wide baffles extend vertically, 6.35 cm from the wall, at 90° to each other, preventing any circulation within the vessel due to the presence of the agitator. The agitator is equipped with five hubs, each with six impeller blades, evenly spaced along the height of the reactor vessel. In the solution-phase polymerization method of this invention, the tank reactor agitator is not used (although present, it is not activated), therefore the tank reactor operates in "piston flow mode." Temperature indicators placed on the tank reactor are used to monitor the temperature distribution of the polymerization reaction. The tank reactor vessel is also traced using high-pressure steam.
[0418] Reactor 3 is the second tubular reactor, with 10-inch diameter tubing and a length of 53 meters. Temperature indicators placed on the tank reactor are used to monitor the temperature distribution of the polymerization reaction.
[0419] The polymerization in the solution polymerization process was terminated by adding a catalyst deactivator to the effluent stream exiting the outlet of the second tubular reactor (reactor 3). The catalyst deactivator used was nonanoic acid.
[0420] Solution absorbents (active aluminum) are used to remove Ziegler-Natta catalyst metal residues (vanadium and zirconium) to trace levels.
[0421] Ethylene copolymers are recovered from process solvents using a two-stage devolatification method, which involves using two gas / liquid separators and passing the second bottom stream (from the second V / L separator) through a gear pump / granulator combination.
[0422] DHT-4V (hydrotalcite), supplied by Kyowa Chemical Industry Co., Ltd., Tokyo, Japan, can be used as a passivating agent or deacidifying agent in solution processes. A slurry of DHT-4V in the process solvent can be added before the first V / L separator.
[0423] Two single-screw extruders granulate the resin product, and then the granules are deactivated in a stripping tower fed with nitrogen and steam.
[0424] Prior to granulation, by adding 1,000 ppm of the ethylene copolymer composition by weight. 1010 (primary antioxidant) and 1,000 ppm 168 (auxiliary antioxidant) is used to stabilize the ethylene copolymer. The antioxidant is dissolved in the process solvent and added between the first and second V / L separators.
[0425] The Ziegler-Natta polymerization catalyst used for the polymerization reaction was fed into the inlet of the first tubular reactor and consisted of three components: (i) a vanadium precatalyst compound VOCl3; (ii) a titanium precatalyst component, titanium tetrachloride, TiCl4; and (iii) a cocatalyst compound, triethylaluminum, (C2H5)3Al. The VOCl3 and TiCl4 compounds were first combined in a weight ratio of 80 / 20 (in cyclohexane), then combined with triethylaluminum, immediately at the inlet of the first tubular reactor. Figure 1 Inject at position A) into the first tubular reactor.
[0426] Table 1 provides details of the solution-phase polymerization carried out in the multi-zone reaction system. Table 2 provides details of the resulting ethylene copolymers.
[0427] Table 1
[0428] Polymerization process conditions
[0429]
[0430]
[0431] Note 1: These are the locations of hydrogen injection points along the length of the first tubular reactor. "A" is at the inlet of the first tubular reactor; this is also known as the reactor feed pump (RFP) location. "B" is located downstream of the first tubular reactor, but still within the length of the first tubular reactor and before the (unstirred) tank reactor. Location "B" is located approximately 50% of the length of the first tubular reactor, downstream of inlet location "A".
[0432] Note 2: The molar ratio of the metal content (V+Ti) of Al in the co-catalyst triethylaluminum to the pre-catalytic mixture of VOCl3 and TiCl4 mixed in an 80 / 20 weight ratio.
[0433] Note 3: Inlet temperature of the first tubular reactor (reactor 1).
[0434] Note 4: Average temperature of the (unstirred) tank reactor (reactor 2).
[0435] Note 5: Temperature difference from inlet to outlet of the (unstirred) tank reactor (reactor 2).
[0436] Note 6: Outlet temperature of the (unstirred) tank reactor (reactor 2).
[0437] Note 7: The temperature difference between the outlet temperature of the (unstirred) tank reactor (reactor 2), which is also the inlet temperature of the second tubular reactor (reactor 3), and the outlet temperature of the second tubular reactor (reactor 3).
[0438] Note 8: The outlet temperature of the second tubular reactor (reactor 3) is before the polymerization catalyst is deactivated.
[0439] Note 9: TSR is Total Solution Rate, defined as the sum of all mass flow rates at the reactor inlet (of the first tubular reactor), in tons per hour.
[0440] Note 10: (For the first tubular reactor) Ethylene concentration at the reactor inlet, in weight percentage (wt%).
[0441] Note 11: The mass ratio of 1-butene to ethylene fed to the reactor inlet (of the first tubular reactor).
[0442] Note 12: Hydrogen concentration at the reactor inlet (of the first tubular reactor), in ppm by mass, based on the total mass flow weight of the multi-zone reactor system (e.g., cyclohexane + monomers (ethylene, 1-butene) + catalyst + hydrogen).
[0443] Note 13: Hydrogen concentration fed into the first tubular reactor at the second injection point, in ppm by mass, based on the weight of the total mass flow of the multi-zone reactor system (e.g., cyclohexane + monomers (ethylene, 1-butene) + catalyst + hydrogen).
[0444] Note 14: The ratio given is equal to the weight ratio (wt%) of the ethylene copolymer prepared in the first tubular reactor (reactor 1) relative to the total ethylene copolymer prepared throughout the multi-zone reactor system.
[0445] Table 2
[0446] Properties of ethylene copolymers
[0447]
[0448] Second polyethylene
[0449] For use as a second polyethylene, a polyethylene homopolymer composition is prepared substantially according to the disclosures in U.S. Patent Application Publication US2013 / 0225743 or US2008 / 0118749 and the teachings in U.S. Provisional Application 63 / 023,270.
[0450] The polyethylene homopolymer composition used in this embodiment is: polyethylene homopolymer composition "C1", with a density of 0.968 g / cm³. 3 The melt index (I2) is 2.0 g / 10 min, and the molecular weight distribution is 8.8; and the polyethylene homopolymer composition "C2" has a density of 0.967 g / cm³. 3The melt index (I2) was 1.2 g / 10 min, and the molecular weight distribution (M) was... w / M n The value is 8.5, and it can be obtained from NOVA Chemicals as... HPs 167-AB (commercial purchase).
[0451] Further details of the polyethylene homopolymer compositions are shown in Table 3.
[0452] Table 3
[0453] Properties of polyethylene homopolymer compositions
[0454]
[0455]
[0456] Add nucleating agent
[0457] Use 1,200 ppm (parts per million by weight) HPN-20E (commercially available from Milliken) nucleates polyethylene homopolymer compositions (“C1” or “C2”). The nucleating agent is reportedly a combination of the following substances: a) a calcium salt of HHPA; and b) zinc stearate, in a weight ratio of 2 / 1. To nucleate the polyethylene homopolymer composition, an HPN-20E masterbatch is prepared and formulated to a suitable level and melt-blended into the polyethylene homopolymer composition.
[0458] Alternatively, the ethylene copolymer (“EC2”) can be nucleated using 4,000 ppm (parts per million by weight) of MICROTUFF AG 609 (commercially available from Specialty Minerals). To nucleate the ethylene copolymer, a masterbatch containing MICROTUFF AG 609 is produced, and the masterbatch is formulated to the appropriate level and melt-blended into the ethylene copolymer.
[0459] Third polyethylene
[0460] In this embodiment, the linear low-density polyethylene (LLDPE1) used as the third polyethylene is FPs123-A is an ethylene copolymer containing ethylene and 1-octene, with a density of 0.923 g / cm³. 3 It has a melt index (I2) of 1.3 g / 10 min and is commercially available from NOVA Chemicals.
[0461] In this embodiment, the medium-density polyethylene (MDPE1) used as the third polyethylene is SURPASS FPs236-A, an ethylene copolymer containing ethylene and 1-octene, with a density of 0.936 g / cm3, a melt index I2 of 2.9 g / 10 min, and is commercially available from NOVA Chemicals.
[0462] In this embodiment, another medium-density polyethylene (MDPE2) used as the third polyethylene is SURPASSRMs341-U, an ethylene copolymer containing ethylene and 1-octene, with a density of 0.941 g / cm³. 3 The melt index I2 is 3.5 g / cm³. 3 It can be purchased from NOVA Chemicals.
[0463] A. Preparation of the unstretched membrane (or "basic structure")
[0464] Multilayer (triple) sheets are co-extruded using a combination of twin-screw and single-screw extruders through a 17.2-inch slot or flat die equipped with a flexible die lip (adjustable gap). The melt stream merges near the die inlet. After extrusion from the die, the multilayer web is secured to a casting roll or cooling roll using air knives and edge pins, and quenched on the cooling roll. The primary cooling roll temperature is set to 76°C. For convenience, this unstretched multilayer sheet is sometimes referred to herein as the “base structure.” The weight of the polymer used in each of the three layers is expressed in A / B / C format. For example, a base structure with two outer layers (or surface layers) and one core layer is described as a 15 / 70 / 15 structure, where each outer layer contains 15% by weight of the total polymer used in the membrane structure, and the core layer contains 70% by weight of the total polymer used in the membrane structure.
[0465] Several three-layer base film structures with structures ranging from 10 / 80 / 10 to 16 / 68 / 16 were prepared using the various polyethylene materials described in Table 4. For a layer comprising a blend of two polyethylene materials (e.g., a core layer comprising an ethylene copolymer and a nucleated ethylene homopolymer composition), the layer was cast as a polymer blend by blending the particles using an online gravity blending system just before extrusion.
[0466] Table 4
[0467] Basic membrane structure
[0468]
[0469]
[0470] * = Nucleating material (nucleating agent = HPN-20E)
[0471] ** = Nucleating material (nucleating agent = MICROTUFF AG 609)
[0472] Biaxially oriented polyethylene (BOPE) membranes are prepared from each of these basic multilayer membrane structures (basic membrane structures numbered 1-15) using the procedures described in Part B below.
[0473] Part B. Preparation of BOPE film - Sequential stretching
[0474] BOPE membrane structures are prepared using a sequential stretching method on a biaxial stretching line of a tenter frame. First, longitudinal stretching / orientation is performed. Then, the "oriented" sheet is stretched transversely.
[0475] Longitudinal orientation (MDO) is performed in a single-stage or multi-stage short-gap stretching process, with temperatures up to 245°F and draw ratios up to approximately 6.5:1. Transverse orientation (TDO) is performed in multiple zones: a preheating zone, a stretching zone, an annealing zone, and a final single cooling zone. TDO stretching zone temperatures reach up to 280°F and draw ratios up to approximately 5.5:1.
[0476] MDO (Medium-density Filtration) is achieved by preheating a base film and stretching the sheet between groups or clusters of heated rollers rotating at different speeds. The speed difference of the rollers determines the stretch ratio. Stretching can be performed on a single set of stretching rollers or on a series of stretching rollers. Stretching is typically performed at a temperature below the film's crystallization melting temperature (Tm). The MDO film is then fed into a tenter oven using clamps on chains attached to tracks and preheated. As the tracks separate, the film is stretched, the tracks pulling the edges of the film, causing the film to stretch laterally. The width of the film is set by the distance between the tracks and can be adjusted to achieve the desired stretch ratio. TDO (Transient Density Filtration) is typically performed at a temperature similar to or slightly higher than MDO. Upon exiting the TDO unit, the film can be annealed or relaxed. After TDO, the film can be cooled and wound. Table 5 provides a summary of the general process conditions used in the tenter oven method.
[0477] Table 5
[0478] BOPE preparation process conditions
[0479] Target melt temperature (F) in the extruder 450-480 Die head width (inches) 17.2 Layer ratio 10 / 80 / 10-16 / 68 / 16 Casting roll temperature (F) 160-185 Casting roll speed (ft / min) 15 MDO stretch roll temperature (F) 215-245 MDO stretch ratio Approximately 5-6.5:1 Temperature in the stretching zone of the tenter frame (F) 230-260 TDO stretch ratio Approximately 5-5.5:1
[0480] All the basic membrane structures in Table 4 (basic membrane structures numbered 1-15) were successfully converted into BOPE membrane structures (BOPE membrane structures numbered 1-15), and the selected properties of these biaxially oriented multilayer membrane structures are given in Table 6.
[0481] Table 6
[0482] Properties of BOPE multilayer films
[0483]
[0484]
[0485] As can be seen from the data provided in Table 6, when the biaxially oriented membrane structure has a core layer comprising a composition of ethylene copolymer and nucleated polyethylene homopolymer, the membrane structure exhibits very good haze and transparency: haze less than 15% and transparency greater than 80%. It is noteworthy that good haze and transparency are maintained even when the core layer contains very small amounts of the nucleated polyethylene homopolymer composition (e.g., when the core layer contains a blend of at least 95% by weight of ethylene copolymer and no more than 5% by weight of the nucleated polyethylene homopolymer composition; see BOPE membrane numbers 6, 7, 8, 9, 14, and 15). For membrane structures with different materials in the first and second adjacent layers (e.g., the surface layer), good haze and transparency values can be maintained as long as the core layer contains a composition of ethylene copolymer and nucleated polyethylene homopolymer. For comparison, when the core layer contains only unnucleated ethylene copolymers (membranes 1, 2 and 11), or blends of ethylene copolymers with unnucleated polyethylene homopolymers (membranes 10), or blends of ethylene copolymers with nucleated ethylene copolymers (membranes 13), one or both of the haze and transparency of the BOPE membrane structure are negatively affected.
[0486] The non-restrictive embodiments disclosed herein include the following:
[0487] Implementation Scheme A. A biaxially oriented polyethylene film structure, comprising:
[0488] Core layer;
[0489] The first adjacent layer, which is adjacent to the first side of the core layer; and
[0490] The second adjacent layer is adjacent to the second side of the core layer;
[0491] The core layer includes:
[0492] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0493] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition;
[0494] The polyethylene homopolymer composition contains a nucleating agent or a mixture of nucleating agents; and
[0495] The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
[0496] Implementation Scheme B. The biaxially oriented polyethylene film structure of Implementation Scheme A, wherein the density of the polyethylene homopolymer composition is 0.952 to 0.975 g / cm³. 3 .
[0497] Implementation Scheme C. The biaxially oriented polyethylene film structure of Implementation Scheme A or B, wherein the melt index of the polyethylene homopolymer composition is 0.5 to 5.0 g / 10 min.
[0498] Implementation Scheme D. A biaxially oriented polyethylene film structure of Implementation Scheme A, B, or C, wherein the polyethylene homopolymer composition comprises:
[0499] i) 5 to 70% by weight of the product has a density of 0.950 to 0.975 g / cm³. 3 The first ethylene homopolymer; and
[0500] ii) 95 to 30% by weight of a density of 0.950 to 0.975 g / cm³ 3 The second ethylene homopolymer, wherein the ratio of the melt index I2 of the second ethylene homopolymer to the melt index I2 of the first ethylene homopolymer is at least 10.
[0501] Implementation Scheme E. A biaxially oriented polyethylene film structure of Implementation Scheme A, B, C, or D, wherein the density of the first polyethylene is 0.941 to 0.962 g / cm³. 3 .
[0502] Implementation scheme F. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D or E, wherein the melt index of the first polyethylene is 0.5 to 5.0 g / 10 min.
[0503] Implementation scheme G. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E or F, wherein the first polyethylene has a molecular weight distribution of 3.0 to 20.0.
[0504] Implementation scheme H. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E or F, wherein the first polyethylene has a molecular weight distribution of 8.5 to 20.0.
[0505] Implementation Scheme I. A biaxially oriented polyethylene film structure of Implementation Scheme A, B, C, D, E, F, G or H, wherein the first polyethylene has a Z-average molecular weight Mz of at least 500,000 g / mol.
[0506] Implementation Scheme J. A biaxially oriented polyethylene film structure of Implementation Scheme A, B, C, D, E, F, G, H or I, wherein the polyethylene homopolymer composition contains 100 to 3,000 ppm (based on the weight of the polyethylene homopolymer composition) of a nucleating agent or a mixture of nucleating agents.
[0507] Implementation scheme K. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E, F, G, H, I or J, wherein the nucleating agent or mixture of nucleating agents comprises a salt of dicarboxylic acid.
[0508] Implementation scheme L. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E, F, G, H, I, J or K, wherein the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE).
[0509] Implementation scheme M. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E, F, G, H, I, J, K, or L, wherein the core layer comprises:
[0510] i) 70 to 99.5% by weight of the first polyethylene; and
[0511] ii) 0.5 to 30% by weight of second polyethylene.
[0512] Implementation scheme N. A biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E, F, G, H, I, J, K, or L, wherein the core layer comprises:
[0513] i) 90 to 99.5% by weight of the first polyethylene; and
[0514] ii) 0.5 to 10% by weight of the second polyethylene.
[0515] Implementation scheme O. Biaxially oriented polyethylene film structure of implementation schemes A, B, C, D, E, F, G, H, I, J, K, L, M or N, with a haze value of less than 15%.
[0516] Implementation scheme P. A biaxially oriented polyethylene film structure of implementation scheme A, B, C, D, E, F, G, H, I, J, K, L, M, N or O, with a transparency value greater than 80%.
[0517] Implementation scheme Q. A biaxially oriented polyethylene film structure of implementation scheme A, B, C, D, E, F, G, H, I, J, K, L, M, N, O or P, wherein the first adjacent layer and the second adjacent layer are surface layers.
[0518] Implementation scheme R. A biaxially oriented polyethylene film structure, comprising:
[0519] Core layer;
[0520] The first adjacent layer, which is adjacent to the first side of the core layer; and
[0521] The second adjacent layer is adjacent to the second side of the core layer;
[0522] The core layer includes:
[0523] i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a density greater than 0.940 g / cm³. 3 ethylene copolymers; and
[0524] ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene;
[0525] The high-density polyethylene therein comprises a nucleating agent or a mixture of nucleating agents; and
[0526] The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene; and
[0527] The haze value of the biaxially oriented polyethylene film structure is less than 15%.
[0528] Implementation S. The biaxially oriented polyethylene film structure of implementation S and implementation R, wherein the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE).
[0529] Implementation scheme T. Implementation scheme R or S biaxially oriented polyethylene film structure, wherein the core layer comprises:
[0530] i) 70 to 99.5% by weight of the first polyethylene; and
[0531] ii) 0.5 to 30% by weight of second polyethylene.
[0532] Implementation scheme U. Implementation scheme R or S biaxially oriented polyethylene film structure, wherein the core layer comprises:
[0533] i) 90 to 99.5% by weight of the first polyethylene; and
[0534] ii) 0.5 to 10% by weight of the second polyethylene.
[0535] Implementation scheme V. A biaxially oriented polyethylene film structure of implementation scheme R, S, T or U, with a transparency value greater than 80%.
[0536] Implementation scheme W. A biaxially oriented polyethylene film structure of implementation scheme R, S, T, U or V, wherein the first adjacent layer and the second adjacent layer are surface layers.
[0537] Industrial applicability
[0538] A biaxially oriented polyethylene (BOPE) film structure comprising at least three layers is provided. BOPE film structures exhibit good optical properties and recyclability, making them suitable for a variety of packaging applications.
Claims
1. A biaxially oriented polyethylene film structure, comprising: Core layer; The first adjacent layer is adjacent to the first side of the core layer; and The second adjacent layer is adjacent to the second side of the core layer; The core layer includes: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a molecular weight distribution of 8.5 to 20.0, a Z-average molecular weight Mz of at least 500,000 g / mol, and a molecular weight greater than 0.940 g / cm³. 3 ethylene copolymers of a certain density; and ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 A polyethylene homopolymer composition; The polyethylene homopolymer composition contains a nucleating agent or a mixture of nucleating agents; and The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than that of the first polyethylene.
2. The biaxially oriented polyethylene film structure of claim 1, wherein the density of the polyethylene homopolymer composition is 0.952 to 0.975 g / cm³. 3 .
3. The biaxially oriented polyethylene film structure of claim 1, wherein the melt index of the polyethylene homopolymer composition is 0.5 to 5.0 g / 10 min.
4. The biaxially oriented polyethylene film structure of claim 1, wherein the polyethylene homopolymer composition comprises: i) 5 to 70% by weight of a density of 0.950 to 0.975 g / cm³ 3 The first ethylene homopolymer; and ii) 95 to 30% by weight of a density of 0.950 to 0.975 g / cm³ 3 The second ethylene homopolymer, wherein the ratio of the melt index I2 of the second ethylene homopolymer to the melt index I2 of the first ethylene homopolymer is at least 10.
5. The biaxially oriented polyethylene film structure of claim 1, wherein the density of the first polyethylene is 0.941 to 0.962 g / cm³. 3 .
6. The biaxially oriented polyethylene film structure of claim 1, wherein the melt index of the first polyethylene is 0.5 to 5.0 g / 10 min.
7. The biaxially oriented polyethylene film structure of claim 1, wherein the polyethylene homopolymer composition comprises 100 to 3,000 ppm (based on the weight of the polyethylene homopolymer composition) of a nucleating agent or a mixture of nucleating agents.
8. The biaxially oriented polyethylene film structure of claim 1, wherein the nucleating agent or mixture of nucleating agents comprises a dicarboxylic acid salt.
9. The biaxially oriented polyethylene film structure of claim 1, wherein the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE).
10. The biaxially oriented polyethylene film structure of claim 1, wherein the core layer comprises: i) 70 to 99.5% by weight of the first polyethylene; and ii) 0.5 to 30% by weight of second polyethylene.
11. The biaxially oriented polyethylene film structure of claim 1, wherein the core layer comprises: i) 90 to 99.5% by weight of the first polyethylene; and ii) 0.5 to 10% by weight of second polyethylene.
12. The biaxially oriented polyethylene film structure of claim 1, wherein the haze value is less than 15%.
13. The biaxially oriented polyethylene film structure of claim 1, wherein the transparency value is greater than 80%.
14. The biaxially oriented polyethylene film structure of claim 1, wherein the first adjacent layer and the second adjacent layer are surface layers.
15. A biaxially oriented polyethylene film structure, comprising: Core layer; The first adjacent layer is adjacent to the first side of the core layer; and The second adjacent layer is adjacent to the second side of the core layer; The core layer includes: i) 50 to 99.5% by weight of a first polyethylene, wherein the first polyethylene has a molecular weight distribution of 8.5 to 20.0, a Z-average molecular weight Mz of at least 500,000 g / mol, and a molecular weight greater than 0.940 g / cm³. 3 ethylene copolymers of a certain density; and ii) 0.5 to 50% by weight of a second polyethylene, wherein the second polyethylene has a density of at least 0.950 g / cm³. 3 High-density polyethylene; The high-density polyethylene therein comprises a nucleating agent or a mixture of nucleating agents; and The first adjacent layer and the second adjacent layer each contain at least 50% by weight of a third polyethylene, wherein the density of the third polyethylene is lower than the density of the first polyethylene; and The haze value of the biaxially oriented polyethylene film structure is less than 15%.
16. The biaxially oriented polyethylene film structure of claim 15, wherein the third polyethylene is selected from linear low-density polyethylene (LLDPE) and medium-density polyethylene (MDPE).
17. The biaxially oriented polyethylene film structure of claim 15, wherein the core layer comprises: i) 70 to 99.5% by weight of the first polyethylene; and ii) 0.5 to 30% by weight of second polyethylene.
18. The biaxially oriented polyethylene film structure of claim 15, wherein the core layer comprises: i) 90 to 99.5% by weight of the first polyethylene; and ii) 0.5 to 10% by weight of second polyethylene.
19. The biaxially oriented polyethylene film structure of claim 15, wherein the transparency value is greater than 80%.
20. The biaxially oriented polyethylene film structure of claim 15, wherein the first adjacent layer and the second adjacent layer are surface layers.
Citation Information
Patent Citations
High density homopolymer blends
US20060047078A1
Barrier film for food packaging
US20080118749A1
Barrier film for food packaging
US20130225743A1
Crystalline synthetic resin composition
US5342868A
Soft films having enhanced physical properties
US5376439A