directed self-assembly

By blending block copolymer mixtures within the manufacturing facility, the critical size and pitch deviation issues caused by inconsistencies in block copolymer mixtures were resolved, enabling uniform coating and cost-effective directional self-assembly processes that meet the manufacturing requirements of multi-level features.

CN117178346BActive Publication Date: 2026-11-20TOKYO ELECTRON LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280016968.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-22
Filing Date
2022-01-12
Publication Date
2026-11-20
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

In existing directional self-assembly processes, inconsistencies in block copolymer mixtures lead to critical size and pitch deviations, increasing production costs and causing process stagnation. Furthermore, the single film thickness of pre-packaged mixtures results in uneven coating, making it difficult to meet the manufacturing requirements of multi-level features.

Method used

A block copolymer mixture is formed within the manufacturing facility, and the first and second block copolymer liquids are blended on a substrate using a mixer device. Solvent adjustments are made to achieve uniform coating and control of characteristic metrics to meet the target process window.

Benefits of technology

This achieved batch consistency of block copolymer mixtures, improved control over critical size, pitch and microphase separation, ensured uniform coating on the substrate, and reduced cost and time waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117178346B_ABST
    Figure CN117178346B_ABST
Patent Text Reader

Abstract

A method for forming a device includes blending a first liquid comprising a first block copolymer with a second liquid comprising a second block copolymer in a mixer within a manufacturing facility to form a first mixture. The first block copolymer comprises a first homopolymer and a second homopolymer, wherein the first homopolymer has a first mole fraction in the first liquid. The second block copolymer comprises the first homopolymer and the second homopolymer, wherein the first homopolymer has a second mole fraction in the second liquid, the first mole fraction being different from the second mole fraction. The method includes placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims the benefit of U.S. non-provisional application No. 17 / 155,931, filed January 22, 2021, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present invention relates generally to semiconductor processing, and in specific embodiments to systems, tools, and methods for directional self-assembly. Background Technology

[0004] Typically, the fabrication of integrated circuits (ICs) requires the formation of multiple device elements on a semiconductor substrate. Traditionally, ICs are manufactured using optical lithography. Optical lithography forms device elements by: forming a photoresist layer on a substrate, partially exposing the photoresist through a patterned mask, developing the exposed photoresist to define a mask pattern within the photoresist, and then etching the photoresist to form a pattern in the substrate.

[0005] Semiconductor technology is driven by the demand to double circuit density every two years. As circuit density increases, the critical size and pitch of IC device components decrease. Critical size and pitch have already shrunk to the point where optical lithography-based processes use multiple patterning techniques to achieve the required critical size, increasing manufacturing costs. Furthermore, future technology nodes may require even more complex multiple patterning steps.

[0006] Directed self-assembly (DSA) has been identified as an alternative method for forming more densely packed devices. The DSA process is controlled by the molecular weight of the block copolymer mixture, which can theoretically be set to a desired size, smaller than that achievable with optical lithography.

[0007] This is because directional self-assembly allows the formation of small device components using self-assembling block copolymers and guide patterns formed using photolithography. However, the guide patterns are patterned using a coarser photolithography process, while the subsequent directional self-assembly process has the potential to form features with critical dimensions comparable to those achieved using multiple patterning processes.

[0008] However, directional self-assembly has its own advantages and disadvantages. As noted above, the feature size in directional self-assembly processes is determined by the mixture of block copolymers used. More specifically, in typical directional self-assembly processes, the molecular weight of the block copolymer mixture controls the critical size, pitch, and phase (shape) of the formed device element. A single block copolymer mixture can only correspond to a single critical size, pitch, and shape. While this characteristic can be used to develop features that are not easily formed by photolithography, the DSA process also presents its own unique set of challenges. Summary of the Invention

[0009] According to an embodiment of the present invention, a method for forming a device includes blending a first liquid comprising a first block copolymer with a second liquid comprising a second block copolymer in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer having a first mole fraction in the first liquid, the second block copolymer comprising the first homopolymer and the second homopolymer having a second mole fraction in the second liquid, the first mole fraction being different from the second mole fraction; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.

[0010] According to an embodiment of the present invention, a method for forming a device includes blending a first block copolymer and a solvent in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.

[0011] According to an embodiment of the present invention, a method for forming a device includes blending a first liquid comprising a first block copolymer and a second liquid substantially comprising a first homopolymer in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising the first homopolymer and the second homopolymer; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber. Attached Figure Description

[0012] To gain a more complete understanding of the invention and its advantages, reference will now be made to the following description, taken in conjunction with the accompanying drawings, in which:

[0013] Figure 1 A block copolymer coating tool according to an embodiment of this application is shown;

[0014] Figure 2 A block copolymer coating tool according to an embodiment of this application is shown;

[0015] Figures 3A-3E Cross-sectional views of a semiconductor device during various manufacturing stages according to embodiments of this application are shown, wherein Figure 3A The device was shown after the patterned photoresist layer was formed. Figure 3B The device was demonstrated after being coated with a mixture containing blended block copolymers. Figure 3C The device was shown after annealing. Figure 3D The device was demonstrated after selectively removing multiple regions, and... Figure 3E The device is shown after the first pattern of the device elements has been formed;

[0016] Figure 4 This is a flowchart of a directional self-assembly method for forming a first pattern of a device according to an embodiment of this application;

[0017] Figure 5 This is a flowchart of a method for adjusting a first block copolymer mixture in a manufacturing facility to meet target metric requirements, according to embodiments of this application.

[0018] Figures 6A-6B Cross-sectional views of a semiconductor device during various manufacturing stages according to embodiments of this application are shown, wherein Figure 6A The device was demonstrated after coating a second patterned photoresist layer with a second block copolymer mixture, and... Figure 6B The device is shown after the second patterning layer forming the device elements; and

[0019] Figure 7 This is a flowchart of a directional self-assembly method for forming a second pattern of a device element on a first pattern of a device element, according to an embodiment of this application.

[0020] Unless otherwise indicated, corresponding numbers and symbols in different figures generally refer to corresponding parts. The figures are drawn to clearly illustrate relevant aspects of the embodiments, and these figures are not necessarily drawn to scale. Detailed Implementation

[0021] As previously noted, directional self-assembly processes utilize block copolymers. Block copolymer blends are blended by suppliers and pre-packaged in discrete vials for shipment to manufacturing facilities. A drawback of this typical directional self-assembly process is that suppliers of pre-packaged block copolymers are often unaware of the specific process requirements for a given process flow and therefore cannot meet the specific compositional process window required at the manufacturing facility, such as meeting critical size targets for features. Mass production of ICs may require multiple packages of the same block copolymer blend. However, due to quality control issues, multiple vials of the same block copolymer blend, especially from different batches, may have inconsistent molecular weights. Therefore, different packages of the same block copolymer blend from a supplier may contain block copolymers with different compositions and thus produce features with different critical sizes and pitches. For example, in some technologies, a 10% batch-to-batch variation in the molecular weight of a block copolymer blend can cause a critical size change of more than 6% for device components. Such a large deviation can lead to process stalls, where the production line stops until the feature size returns to within the process window. Furthermore, reordering pre-packaged block copolymer blends is costly due to the downtime at the manufacturing facility during the time required to receive new vials.

[0022] Another drawback of directional self-assembly is that each feature with different critical dimensions uses a separate block copolymer blend. This is expensive and time-consuming if multiple layers or features are to be fabricated using directional self-assembly in conventional semiconductor manufacturing processes. This is because for each feature that must be patterned at different feature sizes, a different block copolymer composition must be used, and this block copolymer must be delivered to the manufacturing facility. This can lead to significant bottlenecks and increase the costs associated with managing multiple pre-packaged block copolymer blends. For example, using multiple pre-packaged bottles can become expensive due to the complexity associated with purchasing, scheduling, storage, and tooling requirements related to using different bottles.

[0023] Another drawback of directional self-assembly is that the pre-packaged block copolymer mixtures have a single film thickness, which can lead to uneven filling patterns on the substrate when the mixture is applied. In other words, each pre-packaged block copolymer mixture has a predetermined film thickness that it can achieve. Therefore, if the pre-packaged block copolymer mixture has a film thickness less than the target thickness, the pattern of the device elements will not be properly filled. Consequently, even for features with the same critical dimensions, the same bottle may not be used due to differences in the thickness of the patterned substrate layer.

[0024] Embodiments of the present invention advantageously avoid the aforementioned problems by forming block copolymer mixtures within a manufacturing facility. This allows for batch-to-batch consistency, improved control over characteristic metrics such as critical size, pitch, microphase separation, surface roughness, and local critical size uniformity, and control over pattern fill density to ensure uniform coating on the substrate. This disclosure describes embodiments of a method for blending block copolymer mixtures in an in-line mixer within a processing tool (such as a coating tool within a manufacturing facility), which enables cost-effective fabrication of ICs using directional self-assembly processes.

[0025] According to an embodiment of the present invention, in Figure 1 and Figure 2 The image shows coating tools within a manufacturing facility. Several example embodiments of methods for forming semiconductor devices using coating tools are described in more detail in Figures 3-7.

[0026] Figure 1 A block copolymer coating tool according to an embodiment of this application is shown.

[0027] like Figure 1 As shown, the block copolymer coating tool includes a first mixer apparatus 100 and a processing tool 124 in which a semiconductor substrate 120 is processed. The processing tool 124 includes a processing chamber 122 and a substrate holder 121 configured to support the semiconductor substrate 120 during processing. The blended block copolymer mixture is coated onto the main surface of the semiconductor substrate 120 by injecting a blended block copolymer mixture from the first mixer apparatus 100 through a nozzle 118 of the processing tool 124. For example, the nozzle 118 may be a flat flange nozzle, a solids flow nozzle, or any other nozzle known to those skilled in the art.

[0028] The substrate holder 121 can be configured to rotate during the coating process. In some embodiments, the processing chamber 122 includes an outlet for any excess fluid and may also be connected to a pressure system to maintain a target pressure within the processing chamber 122. For some applications, the processing chamber 122 may also include a gas inlet, such as for pumping inert gas into the processing chamber 122.

[0029] refer to Figure 1The first mixer device 100 includes a first supply tank 102 and a second supply tank 104, which are coupled to a mixer 114 including a mixing chamber 112. Although only two sources are shown being mixed, in various embodiments, more than two fluid sources may be mixed in the mixer 114. The first supply tank 102 and the second supply tank 104 each contain a first liquid and a second liquid, respectively. In various embodiments, the first supply tank 102 and the second supply tank 104 are made of ceramic, glass, stainless steel, or any other material, depending on the corrosive properties of the first and second liquids used.

[0030] In various embodiments, the first liquid comprises a first block copolymer comprising a first homopolymer (-AA-…AA-) and a second homopolymer (-BB-…BB-). Thus, the first homopolymer is a polymer of a first monomer (A), and the second homopolymer is a polymer of a second monomer (B). When the first homopolymer is mixed with the second homopolymer (B), a block copolymer ((-AB-)-(-AB-)-…(-AB-)-(-AB-)-) is formed. Examples of homopolymers include methyl methacrylate, styrene, dimethylsiloxane, ethylene oxide, butadiene, vinylpyridine, isoprene, lactic acid, etc.

[0031] In various embodiments, the first homopolymer has a first mole fraction in the first liquid. The second liquid comprises a second block copolymer, which comprises the first homopolymer and the second homopolymer. The first homopolymer has a second mole fraction in the second liquid. Therefore, although both the first and second liquids have the same polymer, the first mole fraction differs from the second mole fraction.

[0032] In one or more embodiments, the first homopolymer is a polystyrene block comprising repeating styrene units and the second homopolymer is a polymethyl methacrylate block comprising repeating methyl methacrylate units. The first homopolymer and the second homopolymer together form poly(styrene-b-methyl methacrylate), i.e., repeating styrene-b-methyl methacrylate units, which is a block copolymer. Therefore, both the first liquid and the second liquid comprise poly(styrene-b-methyl methacrylate) with different molecular weights. The first liquid and the second liquid are described herein by way of example only. Other types of liquids may be used by those skilled in the art.

[0033] In various embodiments, the first mole fraction in the first liquid can be in the range of 10% to 90% and the second mole fraction in the second liquid can be in the range of 10% to 90%, as long as the first mole fraction and the second mole fraction are different.

[0034] In various embodiments, the first mixer device 100 may be gravity-driven with few intermediate components, or may include a pump and valve system for controlling fluid flow. Therefore, in some embodiments, the first mixer device 100 optionally includes a first pump 106a, a second pump 106b, and a third pump 106c; a first shut-off valve 108a, a second shut-off valve 108b, and a third shut-off valve 108c; a first flow meter 110a, a second flow meter 110b, and a third flow meter 110c.

[0035] The first supply tank 102 and the second supply tank 104 are both connected to the first pump 106a and the second pump 106b. The first pump 106a and the second pump 106b are respectively connected to the first shut-off valve 108a and the second shut-off valve 108b, which are further connected to the mixer 114. The mixer 114 is connected to the processing tool 124 via an optional third pump 106c connected to the third shut-off valve 108c and the third flow meter 110c.

[0036] like Figure 1 As shown, mixer 114 can be arranged within mixing chamber 112. As an example, mixer 114 can be designed as described in the following application serial number: 62 / 839,917, filed April 29, 2019, which is incorporated herein by reference. In some embodiments, mixer 114 can be a planetary mixer, a static mixer, or any other mixer known to those skilled in the art capable of blending liquid mixtures.

[0037] The first mixer device 100 may further include an electronic flow control system 115, for example, for controlling various aspects of fluid flow. The electronic flow control system 115 includes a controller 116 and various memories, input / output devices, analog-to-digital converters, and other hardware and software as known to those skilled in the art. For example, the controller may include a processor, a microprocessor, or any other type of controller known in the art. Furthermore, the electronic flow control system 115 includes sensors such as flow sensors, temperature sensors, etc.

[0038] The electronic flow control system 115 is connected to the first pump 106a, the second pump 106b, the third pump 106c, the first shut-off valve 108a, the second shut-off valve 108b, the third shut-off valve 108c, the first flow meter 110a, the second flow meter 110b, the third flow meter 110c, the mixer 112, and other components such as processing tools. More specifically, measurement data from the first flow meter 110a, the second flow meter 110b, and the third flow meter 110c can be received at the electronic flow control system 115, while control signals generated at the controller 116 can be sent to the first pump 106a, the second pump 106b, the third pump 106c, the first shut-off valve 108a, the second shut-off valve 108b, and the third shut-off valve 108c.

[0039] The electronic flow control system 115 can receive measurement or metrological data from sensor 103, as well as process information including process formulation / metrics 105 (such as a target process window). Sensor 103 can include various types of sensors, including but not limited to optical sensors (such as cameras, lasers, light, reflectometers, spectrometers, etc.), capacitive sensors, ultrasonic sensors, gas sensors, temperature sensors for monitoring liquid temperature, or other sensors that can monitor the blending process and the first liquid, the second liquid, and the first mixture of the blend. The electronic flow control system 115 can receive additional data input by the user, including but not limited to the first liquid in the first supply tank 102, the second liquid in the second supply tank 104, the target volume of the first mixture, and the required mixing time. In one example embodiment, a mass spectrometer can be used to periodically determine the composition of the first and second liquids. In one example embodiment, one or more optical sensors can be used to periodically determine the opacity of the first and second liquids, which can help determine the validity of the composition.

[0040] Based on data from various sensors 103 and process formulation / measurement 105, controller 116 generates control signals to activate the first pump 106a and the second pump 106b and deactivate the first shut-off valve 108a and the second shut-off valve 108b, thereby dispensing the first and second liquids into mixer 114. The first pump 106a, the second pump 106b, and the third pump 106c may comprise any centrifugal pump or any positive displacement pump capable of pumping liquid block copolymers, as known to those skilled in the art. The first shut-off valve 108a, the second shut-off valve 108b, and the third shut-off valve 108c may comprise an electrically operated diaphragm valve, an electrically operated angle seat valve, or any other valve known to those skilled in the art.

[0041] As the first and second liquids flow from the first supply tank 102 and the second supply tank 104, the controller 116 continuously or periodically monitors the first flow meter 110a and the second flow meter 110b to track the volume of each liquid dispensed into the mixer 114. For example, the first flow meter 110a, the second flow meter 110b, and the third flow meter 110c may include a volumetric flow meter (which can directly provide the volume of the dispensed liquid without additional calculations) or any other flow meter known to those skilled in the art.

[0042] Once the controller 116 determines, based on data provided by the first flow meter 110a and various sensors 103, and the process formulation / measurement 105, that the target volume of the first liquid has been allocated, the controller 116 generates a control signal to activate the first shut-off valve 108a and shut down the first pump 106a. Similarly, when the controller 116 determines, based on data provided by the second flow meter 110b and various sensors 103, and the process formulation / measurement 105, that the target volume of the second liquid has been allocated, the controller 116 (CTLR) generates a control signal to activate the second shut-off valve 108b and shut down the second pump 106b.

[0043] After the first and second liquids are dispensed into the mixer 114, the controller 116 generates a control signal based on the received data to turn on the mixer 114 for a period of time, and the mixer 114 mixes the first liquid and the second liquid to form a first mixture.

[0044] In various embodiments, mixer 114 may include a storage tank in which the blended liquid (i.e., the first mixture) is stored. However, in some embodiments, the first mixture may be injected directly into nozzle 118 of the processing tool without any separate storage tank. In some embodiments, nozzle 118 and storage tank may be integrated together, for example, in a plenum leading to processing chamber 122.

[0045] After mixing, controller 116 generates a control signal to start an optional third pump 106c and deactivate the third shut-off valve 108c so as to inject the first mixture into nozzle 118 and coat the semiconductor substrate 120 with the first mixture in processing chamber 122.

[0046] In an alternative embodiment, to achieve a more uniform fill density on the semiconductor substrate, the second liquid may contain a solvent using the method described above. In some embodiments, a solvent may be added to improve metrics such as surface roughness and other characteristics. In various embodiments, the solvent may be propylene glycol monomethyl ether acetate, toluene, or any other solvent known in the art that can be mixed with the block copolymer mixture. In other embodiments, the solvent may be added from a third supply tank in addition to the second liquid containing the second block copolymer from the second supply tank 104.

[0047] In another alternative embodiment, the second liquid may comprise essentially a first homopolymer or essentially a second homopolymer. In such an embodiment, the first or second homopolymer can help fine-tune parameters such as the critical size or pitch of the feature to be patterned.

[0048] Figure 2 A block copolymer coating tool according to an embodiment of this application is shown.

[0049] like Figure 2 As shown, the coating tool includes a second mixer apparatus 200 and a processing tool 124 in which the semiconductor substrate 120 is processed. The second mixer apparatus 200 may include any number of supply containers ranging from 1, 2, 3, ... N, which are poured into the mixer 114 to form a first mixture of block copolymers coated onto the semiconductor substrate 120 through nozzles 118. A first supply container 1 is configured to contain a first liquid, a second supply container 2 is configured to contain a second liquid, and correspondingly, an nth supply container N is configured to contain an nth liquid. For example, based on the corrosive properties of the liquids, the supply containers may be made of ceramic, glass, stainless steel, or any other material known to those skilled in the art.

[0050] In various embodiments, the first mixture comprises a first liquid contained in a first supply container 1 and a second liquid contained in a second supply container 2. As described above, the first liquid contained in the first supply container 1 may be a first homopolymer and a second homopolymer, wherein the first homopolymer has a first mole fraction in the first liquid. As described above, the second liquid contained in the second supply container 2 may be a first homopolymer and a second homopolymer, wherein the first homopolymer has a second mole fraction in the second liquid.

[0051] The liquid valves of multiple supply containers 1-N can be opened electronically or by the user, allowing multiple liquids to be mixed in mixer 114, as described above. Figure 1 The aforementioned process is used to form a first mixture. Figure 1In the same manner shown, mixer 114 is connected to processing tool 124 via a third pump 106c connected to a third shut-off valve 108c and a third flow meter 110c. The first mixture to be blended may be contained in a storage tank within the second mixer device 200 or processing tool 124.

[0052] At the end of mixing, the user deactivates the third shut-off valve 108c and activates the third pump 106c to inject the first mixture into the nozzle 118 and coat the semiconductor substrate 120 with the first mixture within the processing chamber 122. As the first mixture exits the mixer 114, it flows through the third flow meter 110c, and the user continuously or periodically monitors the volume reading of the third flow meter 110c. Then, once the third flow meter 110c indicates that the desired volume of the first mixture has been dispensed, the user deactivates the third pump 106c and activates the third shut-off valve 108c.

[0053] In various embodiments, the semiconductor substrate 120 may undergo a curing process in the processing tool 124 or in different tools.

[0054] In other embodiments, the first mixture may include a third liquid in addition to the first and second liquids, the third liquid comprising substantially the first homopolymer, substantially the second homopolymer, or a solvent added from the third supply tank 3. The first homopolymer, the second homopolymer, and the solvent are not described again and may be similar to the solvents described above, for example, regarding... Figure 1 .

[0055] In other embodiments, the first mixture may comprise a third liquid, which is substantially composed of the first homopolymer, from the third supply tank 3, and a fourth liquid, which is substantially composed of the second homopolymer, from the fourth supply tank 4, in addition to the first and second liquids.

[0056] As mentioned above, the first mixture is blended to form device features of a semiconductor device using a directional self-assembly (DSA) process.

[0057] Although not explicitly described, this embodiment may also include an electronic control system coupled to various sensors and data sources to continuously monitor and control the blending process, as described above. Figure 1 The above and use the following Figure 5 The flowchart.

[0058] Figures 3A-3E Cross-sectional views of a semiconductor device during various manufacturing stages according to embodiments of this application are shown, wherein Figure 3A The device was shown after the patterned photoresist layer was formed. Figure 3B The device was demonstrated after being coated with a mixture containing blended block copolymers. Figure 3C The device was shown after annealing. Figure 3D The device was demonstrated after selectively removing multiple regions, and... Figure 3E The device is shown after the first pattern of the device elements has been formed.

[0059] refer to Figure 3A A first patterned photoresist layer 308 is formed on the semiconductor substrate 120. This process can be performed at any stage of device fabrication (such as fin formation, gate formation, metal lines, contact plugs, vias, etc.).

[0060] The semiconductor substrate 120 includes a semiconductor body 320 supporting a first patterned layer 306, on which a first patterned photoresist layer 308 is formed. The semiconductor body 320 may be a bulk substrate such as a bulk silicon substrate, a silicon-on-insulator substrate, a silicon carbide substrate, a gallium arsenide substrate, or a hybrid substrate such as gallium nitride on silicon and other heteroepitaxial substrates, or any other configuration and material known to those skilled in the art.

[0061] The first patterning layer 306 can be a layer for forming device features, or it can be an intermediate layer for subsequently forming device features. An example of such an intermediate layer can be a hard mask layer used for subsequent patterning of features in the underlying layer. In various embodiments, depending on the features manufactured at this manufacturing stage, the first patterning layer 306 can be an insulating layer, a conductive layer, or a semiconductor layer.

[0062] As is known to those skilled in the art, embodiments of the present invention take into account the presence of other intermediate layers. For example, an antireflective coating 307 may be formed prior to the formation of the first patterned photoresist layer 308. In one embodiment, the antireflective coating (ARC) film may comprise a silicon antireflective coating. In some embodiments, the antireflective coating 307 may comprise an organic ARC layer, a metal ARC layer, a metal oxide ARC layer, or a titanium nitride ARC layer. The antireflective coating 307 must also prevent interaction between the forming, oriented self-assembling material (i.e., the first or second homopolymer chains present in the first mixture being deposited, as described below) and the underlying first patterned layer 306.

[0063] In various embodiments, the first patterned photoresist layer 308 serves as a first DSA template because the features below are aligned with the first patterned photoresist layer 308. The first patterned photoresist layer 308 may comprise positive, negative, or mixed photoresist. In one embodiment, the first patterned photoresist layer 308 is formed by spin-coating a resist material onto a first patterned layer 306, baking the resist material to form photoresist, exposing the photoresist using photolithography, and developing the exposed photoresist.

[0064] The first patterned photoresist layer 308 has thus formed an opening with a specific width 302 and a critical dimension 304 defined during the photolithography process. Advantageously, the specific width 302 and the critical dimension 304 are much larger than the features being formed, and therefore these features can be formed using a lower resolution (and thus lower cost) photolithography process.

[0065] refer to Figure 3B The first mixture 310, blended in mixer 114 within the same manufacturing facility, is coated onto the first patterned photoresist layer 308 via first mixer equipment 100 or second mixer equipment 200, as described above. Figure 1 and Figure 2 A more detailed discussion is needed. For clarity, Figure 3B-3E The filling of adjacent openings in the first patterned photoresist layer 308 is not shown. The first mixture 310 is coated on the first patterned photoresist layer 308 and fills the openings between the patterns in the first patterned photoresist layer 308.

[0066] In one embodiment, the first mixture 310 has a first liquid comprising a first block copolymer liquid and a second liquid comprising a second block copolymer liquid in a first ratio. In another embodiment, the first mixture 310 is a mixture of the first block copolymer liquid and a solvent, such as... Figure 1 Or as described in 2. In yet another embodiment, the first mixture 310 is a mixture of a first block copolymer liquid and a homopolymer, such as Figure 1 Or as described in 2. Therefore, in various embodiments, the first mixture 310 has a first block copolymer liquid that is blended with one or more of the second block copolymer liquid, solvent, or homopolymer, such as... Figure 1 Or as described in section 2.

[0067] refer to Figure 3C Annealing the semiconductor substrate 120 causes the first and second homopolymers present in the first mixture 310 to separate and form a first plurality of regions 312 and a second plurality of regions 314, which alternate between each homopolymer and are aligned with the first patterned photoresist layer 308. The first plurality of regions 312 correspond to the first homopolymer and the second plurality of regions 314 correspond to the second homopolymer. In various embodiments, the pitch between adjacent first plurality of regions 312 or adjacent second plurality of regions 314 can vary between 10 nm and 100 nm, thereby enabling the formation of structures below the resolution limits of the photolithography process used to pattern the first patterned photoresist layer 308.

[0068] Annealing may include furnace annealing, lamp-based annealing, rapid thermal annealing, or any other annealing method known to those skilled in the art. In various embodiments, annealing may be performed between 100°C and 700°C, and in one embodiment between 200°C and 400°C.

[0069] As is known to those skilled in the art, the chemical composition of a block copolymer can be adjusted by changing the composition and molar fraction of the homopolymer to control the type of phase separation after annealing. During annealing, the homopolymer undergoes microphase separation, forming repeating patterns or periodic structures. The type of pattern can be spheres (or vice versa) of the first homopolymer embedded in a matrix of the second homopolymer, hexagonal close-packed cylinders (or vice versa) of the first homopolymer embedded in a matrix of the second homopolymer, helices, or alternating layers of the first and second homopolymers. In these possible structures, from a photolithographic perspective, lines can be formed from alternating layers, while hexagonal close-packed cylinders can be used to form an array of contact holes. In the illustrations described herein, the first plurality of regions 312 and the second plurality of regions 314 are selected to be formed in a layered shape. However, in other embodiments, the first plurality of regions 312 and the second plurality of regions 314 can be selected to form cylinders of the first plurality of regions 312 within the second plurality of regions 314 (or vice versa).

[0070] Furthermore, one of the homopolymers has a higher affinity for the first patterned photoresist layer 308 and is formed to contact the sidewalls of the first patterned photoresist layer 308. In this example illustration, the first plurality of regions 312 are preferentially formed on the sidewalls of the first patterned photoresist layer 308.

[0071] refer to Figure 3D Selectively removing one of the first plurality of regions 312 or the second plurality of regions 314 forms a first etch mask in the first patterned photoresist layer 308. In various embodiments, the first plurality of regions 312 corresponding to the first homopolymer are removed, and the second plurality of regions 314 corresponding to the second homopolymer form the first etch mask in the first patterned photoresist layer 308. In alternative embodiments, the second plurality of regions 314 corresponding to the second homopolymer may be selectively removed, and the first plurality of regions 312 corresponding to the first homopolymer may form the first etch mask.

[0072] The removal of the first plurality of regions 312 or the second plurality of regions 314 can be performed using wet or dry chemical methods. For example, dry oxygen plasma can be used to remove polymethyl methacrylate. If the selectivity of this etching process is poor, some of the second plurality of regions 314 will be removed simultaneously with the removal of the first plurality of regions 312. In some embodiments, this can be used to advantageously reduce the critical size of the remaining second plurality of regions 314. However, in some embodiments, lateral etching of the second plurality of regions 314 may not be preferred because it may be difficult to control the vertical properties of the sidewall profile required for patterning the layer 306 to be patterned in the next step.

[0073] refer to Figure 3E Using a first etch mask, a first pattern of device elements 316 having a first critical dimension 318 and a first pitch 321 is formed in the patterned layer 306. In this case, the first patterned photoresist layer 308 is removed before etching. Of course, if multiple trenches are formed in the patterned layer 306, the first patterned photoresist layer 308 can be removed after patterning the patterned layer 306. As is known to those skilled in the art, anisotropic reactive ion etching processes can be used to pattern the patterned layer 306. After patterning the patterned layer 306, any remaining second plurality of regions 314 are also removed.

[0074] As previously described, the first critical dimension 318 and the first pitch 321 formed are based on a first ratio of the liquids blended in the first mixture, for example, the ratio of the first block copolymer to the second block copolymer or the ratio of the first block copolymer to the homopolymer. The first patterned photoresist layer 308 and the etch mask formed by the second plurality of elements are removed.

[0075] Figure 4 This is a flowchart of a first oriented self-assembly method for forming a first pattern of a device element according to an embodiment of this disclosure.

[0076] In frame 402, a first patterned photoresist layer 308 is formed on the first patterned layer 306 formed on the semiconductor substrate 120. This first patterned photoresist layer 308 can be used as follows: Figure 3A The terms and conditions described and shown form the basis of this.

[0077] As shown in box 404 below and about Figure 3B The description describes coating a first patterned photoresist layer 308 with a first mixture 310. (About...) Figure 1 and 2The formation of the first mixture 310 is described. In various embodiments, as discussed above, the first mixture 310 is a combination of two or more of a first block copolymer, a second block copolymer, a solvent, and a homopolymer blended using a first mixer apparatus 100 or a second mixer apparatus 200. Advantageously, the blending of the first mixture 310 and the coating of the first mixture 310 onto the semiconductor substrate 120 occur in the same manufacturing facility. Furthermore, this blending can occur very close to the time interval of the coating process to avoid chemical degradation due to long-term storage.

[0078] Next, refer to box 406 and about Figure 3C The substrate is annealed to form a first plurality of regions 312 and a second plurality of regions 314.

[0079] As shown in box 408 below and about Figure 3D Description: Selectively remove a first plurality of regions 312 to form a first etch mask.

[0080] As shown in box 410 below and about Figure 3E The description states that after removing any remaining first patterned photoresist layer, a first pattern of device element 316 is formed using a first etch mask.

[0081] As mentioned above, the advantage of blending block copolymers in a manufacturing facility is that if the metric of the first pattern formation does not meet the target metric, the blended block copolymer mixture can be adjusted in the manufacturing facility instead of ordering a new mixture from the supplier.

[0082] Figure 5 This is a flowchart of a method for adjusting a first block copolymer mixture within a manufacturing facility to meet target metric requirements.

[0083] As shown in box 502, a block copolymer (BCP) mixture, such as first mixture 310, is blended within a manufacturing facility using either a first mixer device 100 or a second mixer device 200, as described above. Figure 1 and Figure 2 As described above, in various embodiments, the first mixture 310 is a combination of two or more of a first block copolymer, a second block copolymer, a solvent, and a homopolymer blended using a first mixer device 100 or a second mixer device 200.

[0084] It is conceivable that during production or process development, the characteristics of the pattern or blend may not fall within the desired target window. This could ultimately lead to a loss of product yield, and therefore the embodiments disclosed herein envision that the measurements taken in boxes 503 and 506 are actively or periodically monitored and provided to, for example... Figure 1The process control of the electronic flow control system 115 described herein.

[0085] As shown below in box 503, the blended block copolymer mixture, the first liquid, or the second liquid can be metered using various metering tools (including sensors, such as those related to...). Figure 1 The sensor 103 described above is used for analysis. Alternatively, or additionally, for the above measurements in block 503, as shown below in block 504, the semiconductor substrate 120 is coated with the first mixture 310 and a pattern of device elements 316 is formed on the semiconductor substrate 120, as described above. Figures 3A-3E As described in section 4. In this case, the measurement of the pattern of device element 316 is performed. In another embodiment, the pattern of the second plurality of regions 314 is measured before the device element 316 is formed. Thus, in various embodiments, the measured metrics may be the critical dimension of device element 316 / second plurality of regions 314, the width of device element 316 / second plurality of regions 314 (the dimension orthogonal to the critical dimension), the height or depth of device element 316 / second plurality of regions 314, the distance between adjacent elements (i.e., the pitch of device element 316 / second plurality of regions 314), the surface roughness of device element 316 / second plurality of regions 314, the local critical dimension uniformity of device element 316 / second plurality of regions 314, the linewidth variation of device element 316 / second plurality of regions 314, the sidewall angle of device element 316 / second plurality of regions 314, the microphase structure, or any other metric. These metrological measurements can be performed using in-line tools for non-destructive testing such as optical metrology tools such as scatterometers, or other metrological tools that can be used for destructive testing such as optical or electron microscopes.

[0086] Compare the measured metric with the target metric or target process window, for example, from Figure 5 The process formulation / measurement described in [the document] is obtained from 105. For example, this can be achieved in [the following]. Figure 1 This is completed within the electronic control system described herein. If the measured metric is the same as the target metric or within the process window, no changes are made to the blend or the process at this point. If the measured metric differs from the target metric or is outside the process window, the process continues to step 510 and proceeds according to... Figure 1 or Figure 2 To generate new or modified formulations for block copolymer blends. New blends may vary any process parameters, such as the flow rate and / or pressure of the first or second liquid, temperature, and other parameters.

[0087] In various embodiments, if the target metric is a critical size or pitch, and the measured critical size or pitch does not meet the target metric, the first mixture can be further blended with a third liquid comprising substantially a first homopolymer or substantially a second homopolymer to form an adjusted second mixture having a new critical size or pitch.

[0088] In an alternative embodiment, if the target metric is a critical size or pitch, and the measured critical size or pitch does not meet the target metric, the first mixture may be further blended with a third liquid that substantially contains a first homopolymer and a fourth liquid that substantially contains a second homopolymer to form an adjusted second mixture having a new critical size or pitch.

[0089] In an alternative embodiment, if the target metric is surface roughness and the measured surface roughness does not meet the target surface roughness, the first mixture can be further blended with a third liquid containing a solvent to form a new mixture with an improved film thickness. For example, the solvent may include propylene glycol monomethyl ether acetate, toluene, or any other solvent known in the art that alters the film thickness of block copolymers.

[0090] In alternative embodiments, the microphase of the first mixture may be unsuitable. For example, the microphase may be hexagonal rather than layered. In such cases, the first mixture may be further blended with a third liquid comprising substantially a first homopolymer or substantially a second homopolymer to change the phase of the blend from hexagonal to layered and vice versa. In various embodiments, as previously described, the phase can be varied between close-packed cylinders, hexagons, and layers by changing the composition of the homopolymer in the block copolymer.

[0091] The new mixtures used for blending or modification of new process formulations repeat the processes in boxes 502 to 508.

[0092] As mentioned above, another advantage of the disclosed invention is that it allows for the fabrication of multilayer IC device elements with different critical dimensions, pitches, and / or shapes on the same semiconductor substrate by blending multiple block copolymer mixtures corresponding to each successive layer of the device element within a manufacturing facility.

[0093] Figures 6A-6B Cross-sectional views of a semiconductor device during various manufacturing stages according to embodiments of this application are shown, wherein Figure 6A The device was demonstrated after coating a second patterned photoresist layer with a second block copolymer mixture, and... Figure 6B The device is shown after the second patterning layer is formed to form the device elements. Figure 7 It is used to form Figures 6A-6B The flowchart shows the second DSA method for the second layer of the device element in the manufacturing process.

[0094] In this embodiment, blends with different compositions are formed using the same supply containers previously used for patterning device elements at different process steps. Advantageously, different critical dimensions can be achieved using the same mixing equipment without having to change the supply containers.

[0095] Therefore, this embodiment is from Figure 3E Continue. Now refer to Figure 6A And box 702, for example, in Figure 3E An interlayer dielectric layer 606 is formed on the device element 316 formed in the process. The interlayer dielectric layer 606 may comprise multiple layers and may comprise SiO2, SION, Si3N4, glass (such as borosilicate glass, organosilicon glass), low-k dielectric material, or any other interlayer dielectric known to those skilled in the art.

[0096] Next, a second patterned layer 608 is formed on the interlayer dielectric layer 606 (frame 704) and may also include a dielectric layer, a conductive layer or a semiconductor layer, depending on the features formed.

[0097] Next, a second patterned photoresist layer is formed on the second patterned layer 608 (frame 706). For example... Figure 6A As shown, a second patterned photoresist layer 610 is formed on the second patterned layer 608. The second patterned photoresist layer 610 may contain the same material as the first patterned photoresist layer 308 and may be formed in the same manner, such as... Figure 3A As shown in the diagram, the second patterned photoresist layer 610 is patterned with a second specific pitch 602 and a second specific critical dimension 604. The second patterned photoresist layer 610 serves as a second DSA template.

[0098] The second patterned photoresist layer 610 (frame 708) is coated with the second mixture. The second mixture has the same properties as... Figure 3B The second mixture has a different composition than the first mixture used. In one embodiment, the second mixture has a second ratio of a first liquid containing a first block copolymer liquid and a second liquid containing a second block copolymer liquid. The second ratio is selected to achieve a target second critical size of the patterned features, while the first ratio is selected to achieve different target first critical sizes of the patterned features. Similar to the first mixture, in various embodiments, the second mixture has a first block copolymer liquid blended with one or more of the second block copolymer liquid, solvent, or homopolymer, such as... Figure 1 Or as described in 2. Similar to the first mixture, the second mixture is then coated onto the second patterned photoresist layer 610 via a first mixer device 100 or a second mixer device.

[0099] Reference box 710, by annealing the substrate to induce microphase separation (e.g., similar to...). Figure 3D Then one of the phase regions is removed to form the second etch mask 612.

[0100] refer to Figure 6B Using a second etch mask 612, a second pattern (box 712) is formed of device element 616 having a second critical dimension 618 and a second pitch 620. The formed second critical dimension 618 and second pitch 620 are based on a second ratio of the first liquid to the second liquid in the second mixture. The second patterned photoresist layer 610 and the second etch mask 612 are then removed (box 714).

[0101] In various embodiments, a first DSA process is used to form a first pattern of the gate line and a second DSA process is used to form a second pattern of metal lines on the gate line. In alternative embodiments, a first DSA process is used to form a first pattern of the gate line and a second DSA process is used to form a second pattern of contact holes within the gate line.

[0102] Advantageously, such as using Figures 3A-3E And then Figures 6A-6B As discussed in the described embodiments, two different patterns with different critical dimensions and pitches can be formed using a common supply tank source. This advantage expands rapidly if more levels utilize a directional self-assembly process, as additional patterns with other critical dimensions can be manufactured using the same number of supply tanks / liquids.

[0103] Examples of embodiments are described below.

[0104] Example 1. A method for forming a device includes blending a first liquid comprising a first block copolymer with a second liquid comprising a second block copolymer in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer having a first mole fraction in the first liquid, the second block copolymer comprising the first homopolymer and the second homopolymer having a second mole fraction in the second liquid, the first mole fraction being different from the second mole fraction; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.

[0105] Example 2. The method of Example 1, further comprising: forming a patterned photoresist layer on a layer to be patterned disposed on the substrate, wherein coating the substrate with the first mixture includes coating the patterned photoresist layer with the first mixture; annealing to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer; selectively removing the first plurality of regions to form an etch mask aligned with the patterned photoresist layer, the etch mask comprising the second plurality of regions; and using the etch mask to form a pattern in the layer to be patterned.

[0106] Example 3. The method as described in either Example 1 or 2, further comprising removing the patterned photoresist layer and removing the second plurality of regions after the pattern has been formed.

[0107] Example 4. The method of any one of Examples 1 to 3, further comprising: forming a first pattern by coating the first mixture; measuring a first critical dimension of a feature of the first pattern; in response to determining that the first critical dimension differs from a target critical dimension, blending the first liquid with the second liquid in the mixer to form a second mixture, the first mixture comprising a first ratio of the first block copolymer and the second block copolymer, the second mixture comprising a second ratio of the first block copolymer and the second block copolymer, the second ratio differing from the first ratio; coating another substrate with the second mixture; and forming a second pattern by coating the second mixture, wherein a second critical dimension of a feature of the second pattern satisfies a target critical dimension.

[0108] Example 5. The method of any one of Examples 1 to 4, further comprising: blending the first liquid with the second liquid in the mixer to form a second mixture, the first mixture comprising a first ratio of the first block copolymer and the second block copolymer, the second mixture comprising a second ratio of the first block copolymer and the second block copolymer, the second ratio being different from the first ratio; and coating the substrate with the second mixture.

[0109] Example 6. The method of any one of Examples 1 to 5, further comprising: forming a first pattern by using a first oriented self-assembly process based on the first mixture; and forming a second pattern by using a second oriented self-assembly process based on the second mixture, wherein a first critical dimension of a feature of the first pattern is different from a second critical dimension of a feature of the second pattern.

[0110] Example 7. The method as described in any one of Examples 1 to 6, wherein the first directional self-assembly process includes: forming a first patterned photoresist layer on a first patterned layer disposed on the substrate, wherein coating the substrate with the first mixture includes coating the first patterned photoresist layer with the first mixture; annealing to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer; selectively removing the first plurality of regions to form a first etch mask aligned with the first patterned photoresist layer, the first etch mask comprising the second plurality of regions; and using the first etch mask on the first patterned layer. The first pattern is formed in the substrate; and the second orientation self-assembly process includes forming a second patterned photoresist layer on a second patterned layer disposed on the substrate, wherein coating the substrate with the second mixture includes coating the second patterned photoresist layer with the second mixture, annealing to form a third plurality of regions containing the first homopolymer and a fourth plurality of regions containing the second homopolymer, selectively removing the third plurality of regions to form a second etch mask aligned with the second patterned photoresist layer, the second etch mask containing the fourth plurality of regions, and using the second etch mask to form a second pattern in the second patterned layer.

[0111] Example 8. The method as described in any one of Examples 1 to 7, wherein the first pattern is a pattern for gate lines, and wherein the second pattern is a pattern for metal lines on those gate lines.

[0112] Example 9. The method as described in any one of Examples 1 to 8, wherein the first pattern is a pattern for gate lines, and wherein the second pattern is a pattern for forming contact holes in these gate lines.

[0113] Example 10. The method of any one of Examples 1 to 9, wherein coating the substrate comprises: rotating the substrate holder together with the substrate; and injecting the first mixture through a nozzle connected to the mixer, the nozzle being directed toward the substrate so as to coat the substrate with the first mixture.

[0114] Example 11. The method as described in any one of Examples 1 to 10, wherein, during the blending process, the method further comprises adding a third liquid substantially comprising the first homopolymer to form the first mixture.

[0115] Example 12. The method as described in any one of Examples 1 to 11, wherein, during the blending process, the method further includes adding a fourth liquid substantially comprising the second homopolymer to form the first mixture.

[0116] Example 13. A method for forming a device includes blending a first block copolymer and a solvent in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.

[0117] Example 14. The method of Example 13, further comprising: forming a first pattern from the coating of the first mixture; measuring a first metric of a characteristic of the first pattern; in response to determining that the first metric differs from a target metric, blending the first block copolymer with the solvent in the mixer to form a second mixture, the first mixture comprising a first ratio of the first block copolymer to the solvent, the second mixture comprising a second ratio of the first block copolymer to the solvent, the second ratio differing from the first ratio; coating another substrate with the second mixture; and forming a second pattern from the coating of the second mixture, wherein a second metric of a characteristic of the second pattern satisfies the target metric.

[0118] Example 15. The method as described in one of Examples 13 or 14, wherein the first metric, the second metric, and the target metric are measurements of surface roughness.

[0119] Example 16. The method of any one of Examples 13 to 15, further comprising: forming a patterned photoresist layer disposed on the substrate, wherein coating the substrate with the first mixture includes coating the patterned photoresist layer with the first mixture while delivering a solvent to the first mixture; annealing to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer; selectively removing the first plurality of regions to form an etch mask aligned with the patterned photoresist layer, the etch mask comprising the second plurality of regions; and using the etch mask to form a pattern in the layer to be patterned.

[0120] Example 17. A method for forming a device includes blending a first liquid comprising a first block copolymer and a second liquid substantially comprising a first homopolymer in a mixer within a manufacturing facility to form a first mixture, the first block copolymer comprising the first homopolymer and the second homopolymer; placing a substrate on a substrate holder in a processing chamber within the manufacturing facility; and coating the substrate with the first mixture in the processing chamber.

[0121] Example 18. The method as described in Example 17, wherein, during the blending process, the method further includes adding a third liquid substantially comprising the first homopolymer to form the first mixture.

[0122] Example 19. The method as described in one of Examples 17 or 18, wherein, during the blending process, the method further comprises adding a third liquid substantially comprising a solvent to form the first mixture.

[0123] Example 20. The method of any one of Examples 17 to 19, further comprising: forming a first pattern from the coating of the first mixture; measuring a first critical dimension of a feature of the first pattern; in response to determining that the first critical dimension differs from a target critical dimension, mixing the first liquid with the second liquid in the mixer to form a second mixture, the first mixture comprising a first ratio of the first liquid to the second liquid, the second mixture comprising a second ratio of the first liquid to the second liquid, the second ratio differing from the first ratio; coating another substrate with the second mixture; and forming a second pattern from the coating of the second mixture, wherein a second critical dimension of a feature of the second pattern satisfies the target critical dimension.

[0124] Although the invention has been described with reference to illustrative embodiments, this description is not intended to be limiting. Various modifications and combinations thereof will be apparent to those skilled in the art from the specification, illustrative embodiments, and other embodiments of the invention. Therefore, the appended claims are intended to cover any such modifications or embodiments.

Claims

1. A method for forming a device, the method comprising: In a mixer within a manufacturing facility, a first liquid comprising a first block copolymer is blended with a second liquid comprising a second block copolymer to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer having a first mole fraction in the first liquid, the second block copolymer comprising the first homopolymer and the second homopolymer having a second mole fraction in the second liquid, the first mole fraction being different from the second mole fraction; The substrate is placed on a substrate holder in the processing chamber within the manufacturing facility; The substrate is coated with the first mixture in the processing chamber; Measure the mass of the first mixture; The coating of the first mixture forms a first pattern, and the measurement of the first pattern is taken. as well as The measurements of the first mixture and the first pattern are periodically monitored, and if the measured measurements differ from the target measurements or are outside the process window, a new or modified formulation for the block copolymer mixture is generated.

2. The method of claim 1, further comprising: A patterned photoresist layer is formed on the patterned layer disposed on the substrate, wherein coating the substrate with the first mixture includes coating the patterned photoresist layer with the first mixture; Annealing to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer; The first plurality of regions are selectively removed to form an etch mask aligned with the patterned photoresist layer, the etch mask including the second plurality of regions; as well as The etch mask is used to form a pattern in the layer to be patterned.

3. The method of claim 2, further comprising removing the patterned photoresist layer and removing the second plurality of regions after the pattern has been formed.

4. The method of claim 1, wherein, Measuring the metric of the first pattern includes measuring a first critical dimension of a feature of the first pattern, wherein the method further includes: In response to determining that the first critical size differs from the target critical size, in the mixer, the first liquid is blended with the second liquid to form a second mixture, the first mixture comprising a first ratio of the first block copolymer and the second block copolymer, and the second mixture comprising a second ratio of the first block copolymer and the second block copolymer, the second ratio being different from the first ratio; and The second mixture is used to coat another substrate; and The coating of the second mixture forms a second pattern, wherein the second critical dimension of the features of the second pattern satisfies the target critical dimension.

5. The method of claim 1, further comprising: In the mixer, the first liquid and the second liquid are blended to form a second mixture, the first mixture comprising a first ratio of the first block copolymer and the second block copolymer, and the second mixture comprising a second ratio of the first block copolymer and the second block copolymer, the second ratio being different from the first ratio; and The substrate is coated with the second mixture.

6. The method of claim 5, further comprising: The first pattern is formed by using a first directional self-assembly process based on the first mixture; as well as A second pattern is formed by using a second directional self-assembly process based on the second mixture, wherein a first critical dimension of the features of the first pattern is different from a second critical dimension of the features of the second pattern.

7. The method as described in claim 6, in, The first directional self-assembly process includes: A first patterned photoresist layer is formed on a first patterning layer disposed on the substrate, wherein coating the substrate with the first mixture includes coating the first patterned photoresist layer with the first mixture. Annealing is performed to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer. Selectively removing the first plurality of regions to form a first etch mask aligned with the first patterned photoresist layer, the first etch mask including the second plurality of regions, and The first pattern is formed in the first patterning layer using the first etch mask; and wherein the second directional self-assembly process includes... A second patterned photoresist layer is formed on a second patterned layer disposed on the substrate, wherein coating the substrate with the second mixture includes coating the second patterned photoresist layer with the second mixture. Annealing is performed to form a third plurality of regions comprising the first homopolymer and a fourth plurality of regions comprising the second homopolymer. Selectively removing the third plurality of regions to form a second etch mask aligned with the second patterned photoresist layer, the second etch mask including the fourth plurality of regions, and The second pattern is formed in the second patterning layer using the second etch mask.

8. The method of claim 6, wherein, The first pattern is a pattern for the gate lines, and the second pattern is a pattern for the metal lines on these gate lines.

9. The method of claim 6, wherein, The first pattern is a pattern for gate lines, and the second pattern is a pattern for forming contact holes in these gate lines.

10. The method of claim 1, wherein, Coating the substrate includes: Rotate the substrate holder together with the substrate; and The first mixture is injected through a nozzle connected to the mixer, the nozzle being directed toward the substrate so as to coat the substrate with the first mixture.

11. The method of claim 1, wherein, During the blending process, the method further includes adding a third liquid containing the first homopolymer to form the first mixture.

12. The method of claim 11, wherein, During the blending process, the method further includes adding a fourth liquid containing the second homopolymer to form the first mixture.

13. A method for forming a device, the method comprising: In a mixer within a manufacturing facility, a first block copolymer and a solvent are blended to form a first mixture, the first block copolymer comprising a first homopolymer and a second homopolymer; The substrate is placed on a substrate holder in the processing chamber within the manufacturing facility; The substrate is coated with the first mixture in the processing chamber; Measure the mass of the first mixture; The coating of the first mixture forms a first pattern, and the measurement of the first pattern is taken. as well as The measurements of the first mixture and the first pattern are periodically monitored, and if the measured measurements differ from the target measurements or are outside the process window, a new or modified formulation for the block copolymer mixture is generated.

14. The method of claim 13, wherein, Measuring the first pattern includes measuring a first metric of the features of the first pattern, wherein the method further includes: In response to determining that the first metric differs from the target metric, in the mixer, the first block copolymer is blended with the solvent to form a second mixture, the first mixture comprising a first ratio of the first block copolymer to the solvent, and the second mixture comprising a second ratio of the first block copolymer to the solvent, the second ratio being different from the first ratio; and The second mixture is used to coat another substrate; and The coating of the second mixture forms a second pattern, wherein a second metric of the characteristics of the second pattern satisfies a target metric.

15. The method of claim 14, wherein, The first metric, the second metric, and the target metric are measurements of surface roughness.

16. The method of claim 13, further comprising: A patterned photoresist layer is formed on the patterned layer disposed on the substrate, wherein coating the substrate with the first mixture includes coating the patterned photoresist layer with the first mixture while delivering a solvent to the first mixture; Annealing to form a first plurality of regions comprising the first homopolymer and a second plurality of regions comprising the second homopolymer; The first plurality of regions are selectively removed to form an etch mask aligned with the patterned photoresist layer, the etch mask including the second plurality of regions; as well as The etch mask is used to form a pattern in the layer to be patterned.

17. A method for forming a device, the method comprising: In a mixer within a manufacturing facility, a first liquid comprising a first block copolymer and a second liquid comprising a first homopolymer are blended to form a first mixture, the first block copolymer comprising the first homopolymer and the second homopolymer; The substrate is placed on a substrate holder in the processing chamber within the manufacturing facility; The substrate is coated with the first mixture in the processing chamber; Measure the mass of the first mixture; The coating of the first mixture forms a first pattern, and the measurement of the first pattern is taken. as well as The measurements of the first mixture and the first pattern are periodically monitored, and if the measured measurements differ from the target measurements or are outside the process window, a new or modified formulation for the block copolymer mixture is generated.

18. The method of claim 17, wherein, During the blending process, the method further includes adding a third liquid containing the first homopolymer to form the first mixture.

19. The method of claim 17, wherein, During this blending process, the method further includes adding a third liquid containing a solvent to form the first mixture.

20. The method of claim 17, wherein, Measuring the metric of the first pattern includes measuring a first critical dimension of a feature of the first pattern, wherein the method further includes: In response to determining that the first critical size differs from the target critical size, in the mixer, the first liquid and the second liquid are blended to form a second mixture, the first mixture comprising the first liquid and the second liquid in a first ratio, and the second mixture comprising the first liquid and the second liquid in a second ratio, the second ratio being different from the first ratio; and The second mixture is used to coat another substrate; and The coating of the second mixture forms a second pattern, wherein the second critical dimension of the features of the second pattern satisfies the target critical dimension.

Citation Information

Patent Citations

  • Methods and compositions for forming patterns with isolated or discrete features using block copolymer materials

    US20080299353A1

  • Substrate processing method, computer storage medium, and substrate processing system

    WO2014125965A1