A method for forming a Mg-9.2Gd-3.2Y-2Zn-0.4 Zr alloy

By combining CMT arc additive manufacturing equipment and liquid nitrogen spray gun cooling equipment, the cracking and residual stress problems of Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy in the arc additive forming process were solved, realizing crack-free and low residual stress forming, thus improving product quality and application range.

CN117182251BActive Publication Date: 2026-11-24ZHONGBEI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311313387.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2026-11-24
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

The Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy is prone to cracking during arc additive manufacturing, which is difficult to improve with traditional processes. Furthermore, the traditional substrate water cooling method is not suitable for large parts, resulting in cracks and high residual stress during the molding process.

Method used

By using CMT arc additive manufacturing equipment combined with liquid nitrogen spray gun cooling equipment, heat is dissipated below the molding layer through liquid nitrogen spraying, heat accumulation is controlled, internal stress introduced by thermal expansion and contraction is eliminated, and molding with no cracks and low residual stress is achieved.

Benefits of technology

It improves product yield, expands the application scenarios of rare earth magnesium alloys, saves rare earth and magnesium metal resources, and has a simple process, low cost, and is suitable for various process parameters and deposition rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117182251B_ABST
    Figure CN117182251B_ABST
Patent Text Reader

Abstract

This invention discloses a forming method for a Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy, belonging to the field of metal material forming technology. The process includes the following steps: (1) cleaning and treating the raw materials; (2) installing the equipment; and (3) arc forming. This method is a way to achieve arc additive forming of rare earth magnesium alloys, used to solve the problem of cracking during the forming process and reduce the residual stress of the parts. Using this method can improve the yield rate of products, expand the application scenarios and scale of rare earth magnesium alloys, and save rare earth and magnesium metal resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material forming technology, specifically relating to a process method for forming a crack-free, low residual stress Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy using CMT electric arc additive manufacturing equipment and liquid nitrogen spray gun cooling equipment. Background Technology

[0002] Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy is a magnesium-based alloy composed of elements such as magnesium (Mg), gadolinium (Gd), ytterbium (Y), zinc (Zn), and zirconium (Zr). Due to its high strength, high heat resistance, high corrosion resistance, and fine grain size, this alloy is widely used in the aerospace and automotive industries. However, because of its high coefficient of thermal expansion, the arc additive manufacturing process involves extremely complex thermodynamic cycles, making it highly susceptible to cracking during the forming process. Traditional methods of adjusting process parameters are insufficient to mitigate this cracking tendency, hindering its application in various fields. Therefore, a new forming process is needed to prevent cracking during the forming process. Due to the effects of heat accumulation, the material undergoes overall expansion and contraction during forming, introducing significant stress. Therefore, forming crack-free parts with low residual stress requires controlling heat accumulation during the forming process. Eliminating heat accumulation can limit the residual stress effect of the formed layer to within two layers. Traditional substrate water cooling methods are not suitable for molding large parts. When the number of molding layers is too high, the substrate's influence on heat dissipation for the part decreases. Therefore, this paper uses liquid nitrogen spraying to dissipate heat in the additive manufacturing area below the molding layers. Because liquid nitrogen has an extremely low temperature, it can carry away a large amount of heat during the molding process, preventing heat transfer to the lower additive manufacturing areas and thus avoiding internal stress caused by the overall thermal expansion and contraction of the molding area. This method can be used to mold Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy parts with cracks and low residual stress. Summary of the Invention

[0003] The purpose of this invention is to provide a process method for forming crack-free, low-residual-stress Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloys using CMT arc additive manufacturing equipment and liquid nitrogen spray gun cooling equipment. This method is a way to achieve arc additive manufacturing of rare earth magnesium alloys, solving the problem of cracking during part forming and reducing residual stress in the parts. Using this method can improve product yield, expand the application scenarios and scale of rare earth magnesium alloys, and conserve rare earth and magnesium metal resources.

[0004] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A forming method for a Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy includes the following steps: Step 1: Cleaning and processing the raw materials (1) The Mg-9.2Gd-3.2Y-2Zn-0.4Zr wt% alloy wire and the substrate were placed in a mixed solution of anhydrous ethanol, nitric acid and picric acid and heated for ultrasonic cleaning. (2) The cleaned filament and substrate are placed in anhydrous ethanol for heated ultrasonic cleaning; (3) Place the cleaned filament and substrate into a drying oven to dry; Step 2, Install the equipment (1) Install a copper plate of the same size as the substrate between the base and the substrate, and connect the four corners of the substrate to the copper plate and the base; (2) Install the filament into the equipment and set the pressure between the rollers of the filament feeding mechanism and the pressure of the filament output roller of the gun head; (3) Install the liquid nitrogen nozzles on both sides of the welding torch, with the nozzle height matching the height of the welding torch head, and the convergence point of the two nozzles below the welding torch; Step 3, Arc forming (1) Use software to perform three-dimensional modeling, slice the three-dimensional model and set the interlayer thickness, perform path planning, and set the overlap rate, welding speed and interlayer cooling time. (2) Import the program into the welding torch remote control and perform a pre-run to control the distance between the welding torch head and the substrate; (3) Select appropriate process parameters, including wire feeding speed, voltage, current, protective gas speed, arc ignition energy ratio, and arc extinguishing energy ratio; (4) Adjust the flow rate of the liquid nitrogen spray gun; (5) Open the liquid nitrogen spray gun to test run the first layer of the program. After completing the planned path, turn on the welding protection and start additive manufacturing.

[0005] Furthermore, in step one (1), the volume ratio of the anhydrous ethanol, nitric acid and picric acid is 18:1:1, the washing time is 30-60 min, and the heating temperature is 40-50℃.

[0006] Furthermore, in step one (2), the heating temperature is 50-60℃ and the time is 15-30min.

[0007] Furthermore, in step one (3), the drying oven is set at 50-60°C for 10-15 minutes.

[0008] Furthermore, in step two (1), the thickness of the copper plate and the substrate is 10-30mm.

[0009] Furthermore, in step two (2), the pressure between the rollers of the wire feeding mechanism is 150-200N, and the pressure of the wire exit roller of the gun head is 100-150N.

[0010] Furthermore, in step two (3), the convergence point of the two nozzles of the wire is located 20mm below the welding gun, and the welding gun is at a 60° angle to the horizontal plane.

[0011] Furthermore, in step three (1), the interlayer thickness is 2.4-2.7 mm, the path is planned as a serpentine reciprocating cycle, the overlap rate is 30-50%, the welding speed is 8-13 mm / s, and the interlayer cooling time is 20-30 s.

[0012] Furthermore, in step three (2), the distance between the welding torch head and the substrate is 10 times the diameter of the welding wire.

[0013] Furthermore, in step three (3), the wire feeding speed is 6-14 m / min, the voltage is 11-13 V, the current is 80-160 A, the protective gas speed is 10-400 L / min, the arc starting energy ratio is 100-130%, and the arc extinguishing energy ratio is 60-100%.

[0014] Furthermore, in step three (4), the flow rate of the liquid nitrogen spray gun is 5-25 L / min.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The present invention has a simple process, low cost, and obvious effect.

[0016] 2. The liquid nitrogen basin used in this invention can greatly increase the liquid phase cooling rate during the molding process, thereby refining the grains and improving the hardness, tensile strength, plasticity, and friction and wear performance of the molded parts.

[0017] 3. Since this invention does not involve adjusting process parameters, it can be applied to a wider working window, facilitating additive manufacturing with various process parameters and deposition rates.

[0018] 4. This invention can be modified into any robotic arm-type additive manufacturing equipment. The modification is simple and the effect is significant.

[0019] 5. This invention can eliminate heat accumulation in each layer, thus maintaining the consistency of the microstructure of each layer of the molded part, thereby ensuring the consistency of the performance of each part. Attached Figure Description

[0020] Figure 1 A diagram of the equipment used in the method of this invention; Figure 2 The Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy part formed in Example 1; Figure 3 The Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy part formed in Example 2; In the figure: 1. Copper substrate; 2. Alloy substrate; 3. Additive forming area; 4. First liquid nitrogen spray gun; 5. Welding gun; 6. Second spray gun. Detailed Implementation

[0021] The technical solution and effects of the present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited thereto.

[0022] The wire material and Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy substrate of this invention were purchased from Henan Tait Magnesium Industry Technology Co., Ltd. Example 1

[0023] A forming method for a Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy includes the following steps: Step 1: Cleaning and processing the raw materials (1) Place the Mg-9.2Gd-3.2Y-2Zn-0.4Zr wt% alloy wire and the substrate in anhydrous ethanol, nitric acid and picric acid solution with a volume ratio of 18:1:1, heat to 40℃ and ultrasonically clean for 60 min; (2) Place the cleaned filament and substrate into a pure anhydrous ethanol solution and heat to 50°C, then ultrasonically clean for 30 minutes. (3) Place the cleaned filament and substrate into a drying oven and dry at 60°C for 10 minutes; Step two, install the equipment, such as Figure 1 As shown, (1) Install a copper substrate 1 of the same size as the alloy substrate 2 between the base and the alloy substrate 2. The thickness is 30mm. Connect the four corners of the alloy substrate 2 to the copper substrate 1 and the base. The upper part of the alloy substrate 2 is the additive manufacturing area, which is used to form alloy parts. (2) Install the filament into the equipment, and set the pressure between the rollers of the filament feeding mechanism to 150N and the pressure of the filament output roller of the gun head to 150N; (3) Install the liquid nitrogen nozzles on both sides of the welding torch 5. The nozzle height is the same as the welding torch head height. The convergence point of the two nozzles is 20mm below the welding torch. The welding torch is at 60° to the horizontal plane. Step 3, Arc forming (1) Use software to perform three-dimensional modeling, slice the three-dimensional model and set the interlayer thickness to 2.4mm, plan the path as a serpentine reciprocating loop, set the overlap rate to 30%, the welding speed to 11mm / s, and the interlayer cooling time to 20s; (2) Import the program into the welding torch remote control and perform a pre-run, controlling the distance between the welding torch head and the substrate to be 1.2cm; (3) Select appropriate process parameters including wire feeding speed of 14m / min, voltage of 13V, current of 160A, protective gas speed of 30L / min, arc ignition energy ratio of 110%, and arc extinguishing energy ratio of 60%; (4) Adjust the liquid nitrogen spray guns, that is, the flow rate of the first liquid nitrogen spray gun 1 and the second liquid nitrogen spray gun 6 is 10L / min; (5) Open the liquid nitrogen spray gun to test run the first layer of the program. After completing the planned path, turn on the welding protection and start additive manufacturing.

[0024] The molded parts are free of cracks. Figure 2 As shown. Example 2

[0025] A forming method for a Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy includes the following steps: Step 1: Cleaning and processing the raw materials (1) Place the Mg-9.2Gd-3.2Y-2Zn-0.4Zr wt% alloy wire and the substrate in anhydrous ethanol, nitric acid and picric acid solution with a volume ratio of 18:1:1, heat to 50℃ and ultrasonically clean for 30 min; (2) Place the cleaned filament and substrate into a pure anhydrous ethanol solution and heat to 50°C, then ultrasonically clean for 30 minutes. (3) Place the cleaned filament and substrate into a drying oven and dry at 50°C for 15 minutes; Step 2, Install the equipment (1) Install a copper plate of the same size as the substrate and with a thickness of 10mm between the base and the substrate, and connect the four corners of the substrate to the copper plate and the base. (2) Install the filament into the equipment, and set the pressure between the rollers of the filament feeding mechanism to 200N and the pressure of the filament output roller of the gun head to 150N; (3) Install the liquid nitrogen nozzles on both sides of the welding torch. The nozzle height is the same as the welding torch head height. The convergence point of the two nozzles is 20mm below the welding torch. The welding torch is at a 60° angle to the horizontal plane. Step 3, Arc forming (1) Use software to perform three-dimensional modeling, slice the three-dimensional model and set the interlayer thickness to 2.55mm, plan the path as a serpentine reciprocating loop, set the overlap rate to 33%, the welding speed to 9mm / s, and the interlayer cooling time to 30s; (2) Import the program into the welding torch remote control and perform a pre-run, controlling the distance between the welding torch head and the substrate to be 1.2cm; (3) Select appropriate process parameters including wire feeding speed of 8m / min, voltage of 11.3V, current of 87A, protective gas speed of 25L / min, arc ignition energy ratio of 120%, and arc extinguishing energy ratio of 70%; (4) Adjust the flow rate of the liquid nitrogen spray gun to 8 L / min; (5) Open the liquid nitrogen spray gun to test run the first layer of the program. After completing the planned path, turn on the welding protection and start additive manufacturing.

[0026] The molded parts are free of cracks. Figure 3 As shown.

[0027] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A forming method for a Mg-9.2Gd-3.2Y-2Zn-0.4Zr alloy, characterized in that, The molding method includes the following steps: Step 1: Cleaning and processing the raw materials (1) Place the Mg-9.2Gd-3.2Y-2Zn-0.4Zr wt% alloy wire and the substrate into a mixed solution of anhydrous ethanol, nitric acid and picric acid with a volume ratio of 18:1:1 and heat to 40-50℃ for ultrasonic cleaning for 30-60 minutes. (2) Place the cleaned filament and substrate into anhydrous ethanol and heat at 50-60℃ for ultrasonic cleaning for 15-30 minutes; (3) Place the cleaned filament and substrate in a drying oven at 50-60℃ and dry for 10-15 minutes; Step 2, Install the equipment (1) Install a copper plate of the same size as the substrate between the base and the substrate, and connect the four corners of the substrate to the copper plate and the base; (2) Install the filament into the equipment, and set the pressure between the rollers of the filament feeding mechanism to 150-200N and the pressure of the filament output roller of the gun head to 100-150N; (3) Install a first liquid nitrogen spray gun and a second liquid nitrogen spray gun on both sides of the welding gun. The nozzle height of the first liquid nitrogen spray gun and the second liquid nitrogen spray gun is the same as the height of the welding gun head. The convergence point of the two nozzles is located 20mm below the welding gun. The welding gun is at a 60° angle to the horizontal plane. Step 3, Arc forming (1) Use software to perform three-dimensional modeling, slice the three-dimensional model and set the interlayer thickness to 2.4-2.7mm, perform path planning, the path planning is a serpentine reciprocating loop, set the overlap rate to 30-50%, the welding speed to 8-13mm / s and the interlayer cooling time to 20-30s; (2) Import the program into the welding gun remote control and perform a pre-run, controlling the distance between the welding gun head and the substrate to be 10 times the diameter of the welding wire; (3) Set the wire feeding speed to 6-14 m / min, the voltage to 11-13 V, the current to 80-160 A, the protective gas speed to 10-400 L / min, the arc ignition energy ratio to 100-130%, and the arc extinguishing energy ratio to 60-100%; (4) Adjust the flow rate of the liquid nitrogen spray gun to 5-25 L / min; (5) Open the liquid nitrogen spray gun to test run the first layer of the program. After completing the planned path, turn on the welding protection and start additive manufacturing.

Citation Information

Patent Citations

  • Simultaneous cooling assisted connection method based on laser additive manufacturing

    CN105414746A

  • Liquid nitrogen follow-up cooling additive manufacturing device and method

    CN111283305A

  • Magnesium alloy electric arc additive manufacturing method assisted by synchronous air cooling

    CN116833526A