A plant polyphenol and polyepoxide copolymer-modified polyester and a method for preparing the same

By introducing plant polyphenols and epoxy copolymers into polyester materials to form a cross-linked structure, the problems of antibacterial properties and processing difficulties of polyester materials in food packaging are solved, thereby improving antibacterial and antioxidant properties and mechanical properties, and expanding its application range.

CN117186596BActive Publication Date: 2026-11-20GUIZHOU WANYE PACKAGING
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311176582.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2026-11-20
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

Existing biodegradable polyester materials lack antibacterial properties and have poor barrier properties in food packaging, and are difficult to process and mold. In addition, traditional additives pose environmental and health risks, and plant polyphenols have poor compatibility with polyester materials, which limits their application in food preservation films.

Method used

By introducing plant polyphenols and epoxy copolymers into polyester materials, a cross-linked structure is formed by the ring-opening reaction of phenolic hydroxyl groups and polyester terminal carboxyl groups, thereby endowing polyester materials with antibacterial, antioxidant and gas barrier properties, and improving compatibility and processing performance by adjusting the molar ratio.

Benefits of technology

It has improved the antibacterial and antioxidant properties of polyester materials, enhanced their mechanical and processing properties, expanded their application in the food packaging field, and used natural additives that are environmentally friendly and harmless.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117186596B_ABST
    Figure CN117186596B_ABST
Patent Text Reader

Abstract

The application discloses a kind of plant polyphenol and polyepoxy copolymer modified polyester and its preparation method, the modified polyester includes polyester, plant polyphenol and polyepoxy copolymer.Its preparation method includes under heating condition, the polyepoxy copolymer is dissolved in organic solvent, under constant temperature condition, the plant polyphenol is added and mixed uniformly, then basic catalyst is added, after nitrogen is passed, constant temperature reaction is carried out;After reaction is finished, it is cooled to room temperature, then dichloromethane and ethanol are added to dissolve reaction product and remove unreacted substance, finally reaction product is precipitated by adding anti-solvent, the precipitate is filtered, dried, and antibacterial and antioxidant functional modified material is obtained;The prepared antibacterial and antioxidant functional modified material is mixed with the polyester in high mixer, and then melt extrusion is carried out to obtain the modified polyester.The modified polyester material has good antibacterial and antioxidant properties, good processing performance, good tensile strength and toughness, and good gas barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a polyester and its preparation method, particularly a polyester modified with plant polyphenols and polyepoxy copolymers and its preparation method. Background Technology

[0002] Fresh fruits and vegetables have a very short shelf life and are prone to mold and rot during transportation and storage, rendering them inedible, causing food waste and food safety issues. Therefore, extending the shelf life of fruits and vegetables through effective methods is crucial. Among the many methods available, plastic wrap is considered an economical and effective solution.

[0003] Biodegradable polyester materials offer significant advantages over traditional non-degradable materials like polypropylene and polyethylene in reducing environmental pollution due to their biodegradability. However, pure polyester films inherently lack antibacterial properties and exhibit low tensile strength and poor barrier properties, limiting their application in food packaging. Therefore, modifying biodegradable polyester materials to impart antibacterial and antioxidant capabilities, and improving their mechanical properties to meet the application requirements of fruit and vegetable preservation films, is an important pathway for the green development of the food preservation packaging sector in the future.

[0004] To produce multifunctional biodegradable polyester food preservation films with antioxidant, antibacterial, and barrier properties, researchers have added essential oils, chitosan, polyphenolic flavonoids, and metal nanoparticles to the films. For example, adding ZnO and ZnO-Ag nanoparticles to a PBAT matrix produces an antibacterial composite film. However, packaging with these metal or metal oxide nanoparticles is harmful to the environment and human health after disposal, and is also expensive and poses a migration risk. To reduce the negative impacts of chemical additives and nanoparticles on humans, films based on natural antibacterial and antioxidant agents, such as curcumin, tea polyphenols, essential oils, and their complexes, are currently a sought-after alternative, as the phenolic hydroxyl groups endow them with powerful antioxidant and antibacterial properties.

[0005] Plant polyphenols are a class of natural active substances widely found in plants. They possess a polyphenolic structure, strong reducing properties, and scavenging activity against free radicals, while also protecting against free radical-induced damage to biomolecules. They exhibit excellent antioxidant, anti-aging, antibacterial, antiviral, anti-inflammatory, and preservative functions. Plant polyphenols are currently widely used in food preservation, pharmaceuticals, and cosmetics. They are now widely applied in the storage and preservation of vegetables, fruits, meat and poultry products, and aquatic products, effectively improving preservation and extending shelf life.

[0006] However, due to the large number of hydrophilic phenolic hydroxyl groups in natural plant phenols, their compatibility with hydrophobic polymer materials is poor. When added alone, they cannot be uniformly dispersed in the polymer matrix. In addition, plant polyphenols themselves contain a large number of benzene ring structures, which are highly rigid. Direct physical blending with polyester materials does not enhance their properties but may even further degrade them. Furthermore, polyester materials such as PET have slow crystallization rates and are difficult to process, while PLA and PGA have poor toughness and poor processability, making them impossible to process directly without modification. Therefore, there are few reports on the use of plant polyphenols for polyester material modification through blending, and even those that exist suffer from poor compatibility and difficult processing.

[0007] In other words, the application of the antioxidant and antibacterial activities of plant polyphenols to polyester food contact materials without damaging or further reducing the processing difficulty of polyester materials and improving their mechanical properties is in line with current policy guidance and market demand from both practical application needs and environmental protection requirements, and has great market prospects. Summary of the Invention

[0008] The purpose of this invention is to provide a polyester modified with plant polyphenols and epoxy copolymers, and a method for preparing the same. On one hand, the epoxy groups exhibit high reactivity, forming a cross-linked structure through ring-opening reactions between phenolic hydroxyl groups and the terminal carboxyl groups of the polyester, thus endowing the polyester material with high rigidity, heat resistance, and weather resistance. On the other hand, the introduction of phenolic hydroxyl groups into the polyphenol material provides the polyester material with additional antibacterial, antioxidant, and gas barrier properties, offering unique properties not found in existing polyester materials. These unique properties will give it broad application prospects.

[0009] The technical solution of the present invention is a polyester modified with plant polyphenols and epoxy copolymers, comprising polyester, plant polyphenols and epoxy copolymers.

[0010] In a preferred embodiment, the aforementioned polyester modified with plant polyphenols and epoxy copolymers has the following mixing ratio: by weight, it comprises 80-99.9 parts polyester and 0.1-20 parts plant polyphenols and epoxy copolymers in total; wherein the molar ratio of hydroxyl groups in the plant polyphenols to epoxy groups in the epoxy copolymers is 1:0.01-1:50.

[0011] In a preferred embodiment, the aforementioned plant polyphenol and polyepoxy copolymer modified polyester is a petroleum-based polyester and / or a bio-based polyester.

[0012] In a preferred embodiment, the aforementioned plant polyphenol and epoxy copolymer-modified polyester, wherein the petroleum-based polyester is one or any combination of polyethylene terephthalate, polyethylene terephthalate-1,4-cyclohexanediol, polyethylene terephthalate-1,4-cyclohexanediol, polyethylene naphthalate, polybutylene succinate, polycyclohexamethylene terephthalate, polypropylene terephthalate, or polycarbonate; and the bio-based polyester is one or any combination of polylactic acid, polyhydroxyalkanoate, polybutylene succinate, 2,5-furandicarboxylate, polycaprolactone, or polybutylene adipate-butylene terephthalate.

[0013] In a preferred embodiment, the aforementioned polyester modified with plant polyphenols and epoxy copolymers includes plant polyphenols such as anthocyanins, catechins, quercetin, lauryl gallate, ellagic acid, arbutin, quercetin, curcumin, resveratrol, tocopherol, kaempferol, baicalin, luteolin, apigenin, robinin, and rhamnoside.

[0014] In a preferred embodiment, the aforementioned polyester modified with plant polyphenols and epoxy copolymers, wherein the general structural formula of the epoxy copolymers is as follows:

[0015]

[0016] in, Each can be independently one of the following structures:

[0017]

[0018] R4 is either H or CH3;

[0019] R4 is either H or CH3;

[0020] z is 2-20, x and y are 10-300, and n is 1-8000.

[0021] A method for preparing the aforementioned plant polyphenol and epoxy copolymer modified polyester includes the following steps:

[0022] (1) Under heating conditions, the polyepoxy copolymer is dissolved in an organic solvent, the plant polyphenol is added under constant temperature conditions and mixed evenly, then an alkaline catalyst is added, nitrogen gas is introduced, and the reaction is carried out at a constant temperature.

[0023] (2) After the reaction is completed, cool to room temperature, then add dichloromethane and ethanol to dissolve the reaction product and remove unreacted substances. Finally, add the antisolvent to precipitate the reaction product, filter and dry the precipitate to obtain the antibacterial and antioxidant modified material.

[0024] (3) The antibacterial and antioxidant modified material obtained in step (2) is mixed with the polyester in a high-speed mixer and then melt-extruded to obtain the modified polyester.

[0025] In a preferred embodiment, the aforementioned method for preparing polyester modified with plant polyphenols and epoxy copolymers, wherein the organic solvent is one or any combination of acetonitrile, dioxane, dimethyl sulfoxide, acetone, ethyl acetate, n-butyl acetate, methylcyclohexane, or ethanol.

[0026] In a preferred embodiment, the aforementioned method for preparing polyester modified with plant polyphenols and epoxy copolymers, wherein the alkaline catalyst is one of potassium hydroxide, sodium hydroxide, potassium carbonate, potassium alkoxide, sodium alkoxide, or triethylamine; and the antisolvent is petroleum ether.

[0027] In a preferred embodiment, the aforementioned method for preparing polyester modified with plant polyphenols and epoxy copolymers, wherein the volume-to-mass ratio of the alkaline catalyst to the epoxy copolymer is 10-13 ml:10 g; the heating temperature is 60-100 °C; and the reaction time is 4-10 h.

[0028] Beneficial effects of the present invention

[0029] This invention incorporates plant polyphenols with strong antibacterial and antioxidant functions into polyester materials, giving the polyester materials strong antibacterial and antioxidant properties, and making them promising for use in packaging materials for vegetables and fruits, livestock and poultry meat and their products, aquatic products, or pharmaceuticals.

[0030] The method of the present invention improves the compatibility of polyester and plant polyphenols. At the same time, through graft modification of polyepoxy copolymers, the polyester material has better processing and molding performance, lower molding difficulty, better tensile strength and toughness, and better gas barrier properties.

[0031] The principle of this invention is as follows: a functional modifier for polyester materials with antibacterial and antioxidant properties is prepared by grafting a polyepoxy copolymer onto natural plant polyphenols with antibacterial and antioxidant activities through a catalytic reaction. By controlling the molar ratio of plant polyphenols and polyepoxy copolymers during the reaction, the functional modifier can simultaneously retain the epoxy functional groups of the polyepoxy copolymer and the phenolic hydroxyl groups of the plant polyphenols. The epoxy functional groups in the modifier can undergo chain extension reactions with the terminal hydroxyl or carboxyl groups of the polyester material, improving the performance of the polyester itself. At the same time, since the polyepoxy copolymer itself has excellent compatibility with the polyester material, this process naturally improves the compatibility between the plant polyphenols and the polyester material, resulting in better dispersion of the plant polyphenols in the polyester and better mechanical properties of the polyester material.

[0032] On the other hand, the phenolic hydroxyl groups in the modifier can donate hydrogen atoms, giving the polyester composite material antibacterial and antioxidant properties. By increasing the reaction with peroxy free radicals, stable phenoxy free radicals are generated, so that the unpaired single electrons on the oxygen atom can interact with the electron cloud on the benzene ring, producing a conjugation effect, thereby reducing the energy of the free radical and interrupting the chain reaction of lipid peroxidation.

[0033] In other words, this invention enables polyester composite materials to simultaneously possess antibacterial and antioxidant properties, while improving the mechanical and processing properties of polyester. Furthermore, since plant polyphenols are derived from plants, animals, or microorganisms in nature, they are renewable, environmentally friendly, and will not harm the human body, making them more suitable for polyester packaging that comes into direct contact with food or pharmaceuticals, and polyester fibers that come into direct contact with human skin. Moreover, even with extremely low addition levels, the invention enables functional modification of polyester materials, further expanding the application areas of polyester materials and enhancing product competitiveness.

[0034] To demonstrate the beneficial effects of this invention, the applicant provided the following experiments:

[0035] 1. Sample preparation

[0036] Following the method described in Example 1, a polyepoxy copolymer (ADR-4468)-quercetin (QR) graft polymer, denoted as A-QR, was prepared. Simultaneously, following the method described in Example 1, a modified polyester, denoted as PBAT / A-QR, was prepared. The following experiments were conducted using the sample prepared in this example.

[0037] 2. Structural characterization

[0038] The spectra of ADR-4468, A-QR, and QR are as follows: Figure 1 As shown, due to the presence of multiple phenolic hydroxyl groups on quercetin, A-QR at 3265 cm⁻¹ -1 There is a large, broad peak at the (OH stretching vibration) site, and the characteristic peak of quercetin is at 1662 cm⁻¹. -1 (C=O tensile vibration), 1360–1316 cm -1 (C-OH bending vibration) and 1161 cm -1 (COC tensile vibration). ADR-4468 at 3061–2921 cm⁻¹ -1 (CH tensile vibration), 1730cm -1 (C=O stretching vibration of the ester carbonyl group) and 915-845 cm⁻¹ -1(Under the stretching vibration of the epoxy group). The synthesized polymer A-QR exhibits the same OH, C=O, and COC characteristic peaks as quercetin, as well as the same CH, C=C, and epoxy group characteristic peaks of the ester carbonyl group as ADR-4468. Furthermore, a C-OH characteristic peak appears on A-QR, which is a novel characteristic peak of the epoxy ring-opening reaction between the phenolic hydroxyl and epoxy groups. In summary, this indicates that ADR-4468 was successfully grafted onto quercetin.

[0039] The NMR hydrogen spectra of QR, ADR-4468, and A-QR are as follows: Figure 2 As shown in the report, quercetin (QR) exhibits five proton peaks at δ = 7.72 (2'-H), 7.62 (6'-H), 6.88 (5'-H), 6.38 (8-H), and 6.17 ppm (6-H). The proton signal at δ = 12.36 ppm corresponds to 5-OH, δ = 10.61 ppm corresponds to 7-OH, and δ = 9.22 ppm corresponds to 3-OH, 4'-OH, and 3'-OH. ADR-4468 exhibits a proton peak signal belonging to styrene at δ = 7.09 ppm, and the remaining proton peaks of the other two structural units of ADR-446 also appear in the range of δ = 0-4 ppm. A-QR shows five QR proton peaks in the range of δ = 6-7 ppm, while also showing the proton peak signal of ADR-4468, indicating that quercetin was successfully grafted onto ADR-4468. The proton signals of quercetin disappeared at δ = 10.61 and 9.22 ppm, retaining only the proton signal at δ = 12.36 ppm, indicating a weakening of the proton peak signal intensity in ADR-4468. This suggests that the positions of 7-OH, 3-OH, 4'-OH, and 3'-OH in quercetin react with ADR. The grafting efficiency of quercetin was calculated by integrating the proton peaks of the styrene unit in ADR-4468, yielding a grafting efficiency of 85%.

[0040] The results of titration analysis of products A-QR and QR using ADR-4468 are shown in Table 1. The results indicate that the phenolic hydroxyl groups of quercetin react with the epoxy groups of ADR-4468, while retaining both the phenolic hydroxyl groups of quercetin and the epoxy groups of ADR-4468, which can improve the processing properties of the polymer and the antibacterial properties of the packaging film.

[0041] Table 1

[0042]

[0043]

[0044] 3. Antibacterial properties

[0045] To evaluate the antibacterial properties of quercetin QR-grafted ring-polyepoxy copolymer ADR-4468, the antibacterial properties of A-QR were determined in vitro using foodborne bacteria Staphylococcus aureus and Escherichia coli; the results are as follows. Figure 3 As shown in the figure, modifying the structure of quercetin (QR) can enhance its antibacterial activity against certain bacteria compared to quercetin (QR) itself. Studies have shown that quercetin and quercetin derivatives inhibit Gram-positive bacteria more effectively than Gram-negative bacteria, and the difference in antibacterial activity between Gram-positive and Gram-negative bacteria may be due to differences in bacterial cell membrane composition, with antibacterial activity primarily determined by structural hydroxyl groups, consistent with the results of this study. Using ADR-4468 and QR as control groups, it was found that ADR-446 had no inhibitory effect on either type of bacteria, while QR showed better antibacterial efficacy, demonstrating that QR plays a major antibacterial role in the A-QR group. The results are as follows... Figure 3 As shown, A-QR exhibits good antibacterial activity against both Staphylococcus aureus and Escherichia coli, but its antibacterial effect against Staphylococcus aureus is stronger than that against Escherichia coli. Quercetin also shows antibacterial activity against both bacteria, with better antibacterial activity against Staphylococcus aureus than against Escherichia coli. ADR-4468 shows no antibacterial activity against either of these bacteria. However, compared to pure quercetin, the grafted ADR-4468 product A-QR shows a relatively lower antibacterial activity against Staphylococcus aureus, but still retains good antibacterial activity, while its antibacterial activity against Escherichia coli is enhanced.

[0046] Pathogens such as Staphylococcus aureus and Escherichia coli are associated with the spoilage of fruits and vegetables. The antibacterial activity of PBAT / A-QR composite membranes against Staphylococcus aureus and Escherichia coli is as follows: Figure 4 As shown in Table 2, the inhibition diameters are also shown. In vitro antibacterial tests indicated that the antibacterial activity of the membrane increased with increasing A-QR concentration. Using pure PBAT membrane as a control, the results showed that PBAT lacked antibacterial properties, and A-QR was responsible for the antibacterial effect of the PBAT / A-QR combination. Therefore, adding A-QR to antibacterial food packaging films can reduce the spoilage rate of fruits and vegetables.

[0047] Table 2

[0048]

[0049]

[0050] 4. Application of PBAT / A-QR film in food packaging

[0051] Strawberries, lacking a hard outer shell for protection, are prone to mold and rot due to microbial invasion; bananas soften and rot more easily due to the large amount of ethylene they produce, resulting in a shorter shelf life; flat mushrooms, a common edible mushroom, are prone to water loss and rot, requiring a longer shelf life; apples oxidize and lose moisture rapidly after being cut, making storage difficult. In this study, we chose to test our antibacterial and antioxidant preservation film on these four fruits and vegetables.

[0052] like Figure 5 As shown, strawberries in PBAT film became soft and moldy after 5 days of storage, while strawberries in the 0.6% A-QR and 1% A-QR groups remained fresh. Bananas showed varying degrees of decay after 5 days of storage, but the control group showed greater decay and decayed faster during storage (as shown in the photo on day 3). Mushrooms in the control group became darker in color, decayed more, and lost more water after 7 days of storage, while mushrooms in the two A-QR groups remained unchanged in color, did not decay, and also lost water. In fresh-cut apple packaging, the PBAT control group showed severe browning, while the two groups containing A-QR showed minimal browning and minimal weight loss. These results indicate that the introduction of A-QR expands the application range of PBAT materials and improves their performance. PBAT / A-QR preservation film can extend the shelf life of various fruits and vegetables, and its effect is universally applicable. Attached Figure Description

[0053] Appendix Figure 1 Infrared spectra of ADR-4468, A-QR, and QR;

[0054] Appendix Figure 2 The proton spectra of ADR-4468, A-QR, and QR are shown.

[0055] Appendix Figure 3 The graphs show the antimicrobial properties of ADR-4468, A-QR, and QR.

[0056] Appendix Figure 4 Graphs showing the antibacterial properties of different concentrations of PBAT / ADR-4468 and PBAT;

[0057] Appendix Figure 5 The image shows the preservation effect of PBAT / A-QR composite film on fruits and vegetables.

[0058] Appendix Figure 6 The infrared spectrum of the product of Example 2;

[0059] Appendix Figure 7 The infrared spectrum of the product of Example 3;

[0060] Appendix Figure 8 The infrared spectrum of the product of Example 4;

[0061] Appendix Figure 9 The diagrams show the blow molding process of the embodiments and comparative examples of the present invention. a is Comparative Example 2, b is Comparative Example 6, c is Example 1, and d is Example 3. Detailed Implementation

[0062] The present invention will be further described below with reference to embodiments, but these embodiments are not intended to limit the scope of the invention.

[0063] Embodiments of the present invention

[0064] Example 1

[0065]

[0066] Step 1: Add 10g of 0.0015mol of commercially available epoxy copolymer (ADR-4468) to a 500mL round-bottom flask, followed by 200mL of acetonitrile and 40mL of ethanol. Stir the epoxy copolymer (ADR-4468) at 60℃ until completely dissolved. Then add 0.033mol of 10g of quercetin and stir until homogeneous. Next, add 11.4mL of triethylamine as a catalyst and react at 60℃ for 4 hours. After the reaction, cool the reaction solution to room temperature. Then add an appropriate amount of dichloromethane and a small amount of ethanol to completely dissolve the product and remove unreacted monomers. Finally, pour the dissolved product into a large amount of petroleum ether. The product will precipitate from the petroleum ether. Dry the precipitate in an oven at 60℃ to constant weight to obtain a powdered solid product, A-QR.

[0067] Step 2: By weight, 0.6 parts of the modifier (quercetin-4468) prepared in Step 1 and 99.5 parts of polybutylene adipate-butylene terephthalate are mixed in a high-speed mixer at 80°C for 10 minutes. The mixture is then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130°C and a screw speed of 200 rpm. After extrusion, the granules are placed in a blown film extruder at a screw speed of 450 rpm and blown at a blown film temperature of 130°C to obtain PBAT / A-QR.

[0068] Example 2

[0069]

[0070] Step 1: Take 0.0006 mol of epoxy copolymer 2 (4 g) into a round-bottom flask, add 30 mL of dimethyl sulfoxide and 6 mL of ethanol as solvents, then add 0.23 mol of tocopherol (10 g), stir the reaction at 70 °C, and after the solid dissolves, add 0.35 g of sodium hydroxide catalyst. After reacting for 6 h, stop the reaction, and after cooling to room temperature, add an appropriate amount of dichloromethane to dissolve the solid product completely. Then pour the product into a large amount of petroleum ether to precipitate the solid product. After discarding the petroleum ether, put the solid product into an oven and dry it at 80 °C to constant weight. A powdered solid product is obtained, which is the product of Example 2. Its infrared characterization is as follows. Figure 6 As shown, 1730cm -1 The peak at 915 cm⁻¹ represents the C=O stretching vibration on the ester group of the polyepoxy copolymer 2. -1 840cm -1 The presence of these two characteristic groups on the product, which are due to the stretching vibration of the epoxy group, indicates that the grafting has been successful.

[0071] Step 2: By weight, mix 1 part of the modifier prepared in Step 1 (product of Example 2) and 99 parts of polybutylene adipate-butylene terephthalate (PBAT) in a high-speed mixer at 80°C for 10 minutes. Extrude and granulate the mixture in a twin-screw extruder at a melt extrusion temperature of 110-130°C. The screw speed is 200 rpm. After extrusion, granulate the resulting material and place it in a blown film extruder at a screw speed of 450 rpm. Blow-mold the material at a blown film temperature of 130°C to form a film, i.e., the PBAT / Product of Example 2.

[0072] Example 3

[0073]

[0074] Step 1: Take 0.0015 mol of epoxy copolymer 3 (10 g) into a round-bottom flask, add 20 mL of ethyl acetate and 4 mL of ethanol as solvents, then add 0.03 mol of gallic acid laurate (10 g), stir the reaction at 60 °C, and after the solid melts, add 1.66 g of catalyst K2CO3. After reacting for 4 h, stop the reaction, and after cooling to room temperature, add an appropriate amount of dichloromethane to dissolve the solid product completely. Then pour the product into a large amount of petroleum ether to precipitate the solid product. After discarding the petroleum ether, put the solid product into an oven and dry it at 60 °C to constant weight. A powdered solid product is obtained, which is the product of Example 3. Its infrared characterization is as follows. Figure 7 As shown, 1730cm -1 The peak at 910 cm⁻¹ represents the C=O stretching vibration of the ester group in the polyepoxy copolymer 3. -1 840cm -1 The presence of these two characteristic groups on the product, which are due to the stretching vibration of the epoxy group, indicates that the grafting has been successful.

[0075] Step 2: By weight, mix 5 parts of the modifier prepared in Step 1 (product of Example 3), 75 parts of polybutylene adipate-butylene terephthalate (PBAT), and 20 parts of polylactic acid (PLA) in a high-speed mixer at 80°C for 10 minutes. Extrude and granulate the mixture in a twin-screw extruder at a melt extrusion temperature of 140-170°C. The screw speed is 200 rpm. After extrusion, granulate the mixture and place the resulting granules into a blown film machine at a screw speed of 450 rpm, blow molding it into a film at a blow molding temperature of 170°C.

[0076] Example 4

[0077]

[0078] Step 1: Take 0.0015 mol of epoxy copolymer 4 (10 g) into a round-bottom flask, add 20 mL of acetonitrile and 4 mL of ethanol as solvents, then add 0.027 mol of curcumin (10 g), stir the reaction at 60 °C, and after the solid melts, add 0.61 g of triethylamine catalyst. After reacting for 8 hours, stop the reaction, and after cooling to room temperature, add an appropriate amount of dichloromethane to dissolve the solid product completely. Then pour the product into a large amount of petroleum ether to precipitate the solid product. After discarding the petroleum ether, put the solid product into an oven and dry it at 60 °C to constant weight. A powdered solid product is obtained, which is the product of Example 4. Its infrared characterization is as follows. Figure 8 As shown, 1730cm -1 The peak at 915 cm⁻¹ represents the C=O stretching vibration on the ester group of the polyepoxy copolymer 4. -1 840cm -1 The peaks represent the stretching vibrations of the epoxy group. The presence of these two characteristic groups on the product indicates that the grafting has been successful.

[0079] Step 2: By weight, 1 part of the modifier prepared in Step 1 (product of Example 4) is mixed with 99 parts of polyethylene terephthalate-1,4-cyclohexanediethanol ester (PETG) in a high-speed mixer at 80°C for 10 minutes. The mixture is then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 160-190°C. The screw speed is 200 rpm. After extrusion, the granules are fed into a blown film extruder at a screw speed of 450 rpm and blown into a film at a blown film temperature of 190°C.

[0080] Comparative Example 1

[0081] 100 parts of polybutylene adipate-butylene terephthalate (PBAT) were dried in a vacuum drying oven at 80°C for 24 hours. The granules were then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130°C. The screw speed was 200 rpm. After extrusion, the granules were fed into a blown film extruder at a screw speed of 450 rpm and blown at a blown film temperature of 130°C.

[0082] Comparative Example 2

[0083] 0.6 parts quercetin and 99.4 parts polybutylene adipate-butylene terephthalate (PBAT) were dried in a vacuum drying oven at 80℃ for 24 hours. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130℃ and a screw speed of 200 rpm. The resulting granules were then fed into a blown film extruder at a screw speed of 450 rpm and blown into a film at a blown film temperature of 130℃.

[0084] Comparative Example 3

[0085] 0.6 parts of epoxy copolymer ADR4468 and 99.4 parts of polybutylene adipate-butylene terephthalate (PBAT) were dried in a vacuum drying oven at 80℃ for 24 hours. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130℃. The screw speed was 200 rpm. After extrusion, the granules were fed into a blown film extruder at a screw speed of 450 rpm and blown at a blown film temperature of 130℃.

[0086] Comparative Example 4

[0087] 0.3 parts quercetin, 0.3 parts epoxy copolymer ADR4468, and 99.4 parts polybutylene adipate-butylene terephthalate (PBAT) were dried in a vacuum drying oven at 80℃ for 24 hours. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130℃ and a screw speed of 200 rpm. The resulting granules were then fed into a blown film extruder at a screw speed of 450 rpm and blown into a film at a blown film temperature of 130℃.

[0088] Comparative Example 5

[0089] 2.5 parts gallic laurate, 2.5 parts epoxy copolymer 3, polybutylene adipate-butylene terephthalate (PBAT), and 20 parts polylactic acid (PLA) were mixed in a high-speed mixer at 80°C for 10 minutes. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 140-170°C. The screw speed was 200 rpm. After extrusion, the granules were granulated and fed into a blown film extruder at a screw speed of 450 rpm, where they were blown into a film at a blown film temperature of 170°C.

[0090] Comparative Example 6

[0091] One part curcumin and 99 parts polyethylene terephthalate-1,4-cyclohexanediol ester (PETG) were mixed in a high-speed mixer at 100°C for 10 minutes. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 160-190°C. The screw speed was 200 rpm. After extrusion, the granules were granulated and fed into a blown film extruder at a screw speed of 450 rpm. The film was blown at a blown film temperature of 190°C.

[0092] Comparative Example 7

[0093] One part epoxy copolymer and 4.99 parts polyethylene terephthalate-1,4-cyclohexanediol ester (PETG) were dried in a vacuum drying oven at 100℃ for 24 hours. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130℃. The screw speed was 200 rpm. After extrusion, the granules were fed into a blown film extruder at a screw speed of 450 rpm and blown into a film at a blown film temperature of 190℃.

[0094] Comparative Example 8

[0095] 0.5 parts curcumin, 0.5 parts epoxy copolymer, and 99 parts polyethylene terephthalate-1,4-cyclohexanediol ester (PETG) were dried in a vacuum drying oven at 100℃ for 24 hours. The mixture was then extruded and granulated in a twin-screw extruder at a melt extrusion temperature of 110-130℃ and a screw speed of 200 rpm. The resulting granules were then fed into a blown film extruder at a screw speed of 450 rpm and blown into a film at a blown film temperature of 190℃.

[0096] The test results of Examples 1-4 and Comparative Examples 1-8 are shown in Table 3. The test standards are as follows: the impact strength of the cantilever beam is tested according to GB / T1843-2008; the tensile strength is tested according to GB / T1040.1-2006; the bending performance is tested (GB / T9341-2000); and the crystallization performance is tested by differential scanning calorimetry.

[0097] Table 3

[0098]

[0099]

[0100] When plant polyphenols are added directly to the polyester matrix, as shown in Comparative Examples 1, 2, and 6, the plant polyphenols do not contribute to the strength of the polyester material; on the contrary, they reduce the strength and elongation at break. Due to the reduction in material properties, the material cannot be endowed with excellent processing properties, as illustrated in the attached figure. Figure 9PETG, as an amorphous polymer, cannot have its crystalline structure altered by adding plant polyphenols and modifiers. When epoxy copolymers are added alone (Comparative Examples 3 and 7), the epoxy copolymers can undergo chain extension reactions with polyester materials, thus appropriately improving the mechanical properties of the polyester materials during processing. When epoxy copolymers and plant polyphenols are added to polyester or polyester alloy materials via physical mixing (Comparative Examples 4 and 5), the phenolic hydroxyl and epoxy groups on the surface of the plant polyphenols do not react under catalysis, resulting in no chemical interaction between them and no composite effect. Therefore, the dispersion performance of the polyphenols cannot be improved, and the material's performance cannot be fundamentally enhanced. Through the embodiments of this invention, it can be seen that after grafting epoxy copolymers with plant polyphenols, a new compound with chemical bonds is formed through molecular interactions between the two, resulting in a superior composite effect. Unlike blending, this method leverages the uniform dispersion of plant polyphenols in the polyester matrix, thereby achieving excellent heterogeneous nucleation effects and improving the mechanical and crystallinity properties of the material.

[0101] The antioxidant activity of the embodiments and comparative examples of this invention was tested using DPPH free radical scavenging. First, the film samples of each embodiment and comparative example were cut into small pieces (0.1 g) and mixed with 5 mL of methanol solution. The mixture was sonicated for 20 min, allowed to stand at room temperature for 10 h, and centrifuged at 5000 r / min for 10 min. After centrifugation, 1 mL of the supernatant was mixed with 3 mL of 0.06 mmol / L DPPH methanol solution and allowed to stand in the dark at room temperature for 1 h. The absorbance was measured at 517 nm using a UV spectrophotometer (MAPADA, UV-6300). A mixture of 3 mL of methanol solution and 1 mL of DPPH solution was used as a blank control. The antioxidant capacity of the composite material was determined by comparing the change in the absorption peak intensity of the reaction mixture at 513 nm over 60 minutes, analyzing the free radical scavenging ability of the comparative and embodiment examples. The results are shown in Table 4.

[0102] Table 4

[0103]

[0104] As can be seen from Examples 1-4, the free radical scavenging ability gradually increases with the increase of polyphenol modifier. Although the addition of plant polyphenols has certain antioxidant activity, the processing performance of polyphenol products alone is poor, and products with excellent processing performance cannot be obtained. When epoxy copolymers and plant polyphenols are added to polyester or polyester alloy materials in a physical mixing manner, since there is no chemical reaction between the two, the dispersion performance of polyphenols cannot be improved, and therefore the maximum anti-aging effect of polyphenols cannot be exerted in polyester materials.

[0105] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A polyester modified with plant polyphenols and epoxy copolymers, characterized in that: The mixing ratio of the polyester, plant polyphenols and epoxy copolymer is as follows: by weight, it contains 80-99.9 parts of polyester and 0.1-20 parts of plant polyphenols and epoxy copolymers in total; wherein, the molar ratio of hydroxyl groups in plant polyphenols to epoxy groups in epoxy copolymers is 1:0.01-1:

50. Its preparation method includes the following steps: (1) Under heating conditions, the polyepoxy copolymer is dissolved in an organic solvent, the plant polyphenols are added under constant temperature conditions and mixed evenly, then an alkaline catalyst is added, nitrogen gas is introduced, and the reaction is carried out at a constant temperature. (2) After the reaction is completed, cool to room temperature, then add dichloromethane and ethanol to dissolve the reaction product and remove unreacted substances. Finally, add the antisolvent to precipitate the reaction product, filter and dry the precipitate to obtain the antibacterial and antioxidant modified material. (3) The antibacterial and antioxidant modified material obtained in step (2) is mixed with the polyester in a high-speed mixer and then melt-extruded to obtain the modified polyester. The plant polyphenols are one or more of the following: anthocyanins, catechins, lauryl gallate, ellagic acid, arbutin, quercetin, curcumin, resveratrol, tocopherol, kaempferol, baicalin, luteolin, apigenin, robinin, or rhamnoside. The general structural formula of the polyepoxy copolymer is as follows: in, and Each can be independently one of the following structures: , , , , , or ; R4 is H or CH3; z is 2-20, x and y are 10-300, and n is 1-8000.

2. The polyester modified with plant polyphenols and epoxy copolymers according to claim 1, characterized in that: The polyester is a petroleum-based polyester and / or a bio-based polyester.

3. The polyester modified with plant polyphenols and polyepoxy copolymers according to claim 2, characterized in that: The petroleum-based polyester is one or more of the following: polyethylene terephthalate, polyethylene terephthalate-1,4-cyclohexanediol, polyethylene terephthalate-1,4-cyclohexanediol, polyethylene naphthalate, polybutylene succinate, polycyclohexamethylene terephthalate, polypropylene terephthalate, or polycarbonate; the bio-based polyester is one or more of the following: polylactic acid, polyhydroxyalkanoate, polybutylene succinate, 2,5-furandicarboxylate, polycaprolactone, or polybutylene adipate-butylene terephthalate.

4. The polyester modified with plant polyphenols and polyepoxy copolymers according to claim 1, characterized in that: The organic solvent is one or any combination of acetonitrile, dioxane, dimethyl sulfoxide, acetone, ethyl acetate, n-butyl acetate, methylcyclohexane, or ethanol.

5. The polyester modified with plant polyphenols and polyepoxy copolymers according to claim 1, characterized in that: The alkaline catalyst is one of potassium hydroxide, sodium hydroxide, potassium carbonate, potassium alkoxide, sodium alkoxide, or triethylamine; the antisolvent is petroleum ether.

6. The polyester modified with plant polyphenols and polyepoxy copolymers according to claim 1, characterized in that: The volume-to-mass ratio of the alkaline catalyst to the epoxy copolymer is 10-13 ml: 10 g; the heating temperature is 60-100℃, and the reaction time is 4-10 h.

Citation Information

Patent Citations

  • Preparation method of degradable composite multifunctional packaging film

    CN110105612A