A preparation method of a cross-shaped microstructure laser-induced graphene flexible strain sensor

The graphene flexible strain sensor prepared by grid-shaped laser scanning solves the problem of isotropic strain sensing when laser-induced graphene sensors bend in different directions, improving the sensor's sensitivity and stability, and making it suitable for scenarios requiring isotropic bending.

CN117190842BActive Publication Date: 2026-11-24ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311027168.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2026-11-24
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

Existing laser-induced graphene sensors cannot achieve isotropic strain sensing when subjected to bending in different directions, which limits their application in the field of flexible sensors.

Method used

A PI film was prepared using an in-plane grid-shaped laser scanning method and specific laser parameters. The personalized pattern was designed using the C4D software built into the ultraviolet laser cutting machine, and a grid-shaped microstructure laser-induced graphene flexible strain sensor was prepared.

Benefits of technology

It achieves isotropic strain sensing during lateral and longitudinal bending, improving the sensor's sensitivity and stability, and is suitable for special scenarios requiring isotropic bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117190842B_ABST
    Figure CN117190842B_ABST
Patent Text Reader

Abstract

This invention discloses a method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor. By scanning the prepared PI film with an in-plane grid-shaped laser scanning method and specific laser parameters, laser-induced graphene with high carbonization degree is obtained, making the material isotropic when facing lateral and longitudinal bending, and making it easier to quantify external strain. Finally, the laser-induced pattern is customized and cut using the C4D software built into the ultraviolet laser cutting machine, showing unique advantages in sensor fabrication.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of advanced materials preparation and processing, and relates to a method for preparing a laser-induced graphene flexible strain sensor with a grid-shaped microstructure. Background Technology

[0002] In recent years, graphene, as an emerging two-dimensional material, has received widespread attention from scientific research and application fields worldwide. Graphene is an important member of the carbon nanomaterial family. Due to its unique physical properties, such as high surface area, high conductivity, good mechanical strength, and stability, it has shown broad application prospects in electronic devices, energy storage, and electrochemical catalysis.

[0003] Among these, the surface morphology of graphene is a key technical aspect. Because laser-induced graphene materials are very thin, their surface morphology has a significant impact on their performance. In the preparation of laser-induced graphene, linear laser scanning technology is used, resulting in surface morphologies of both horizontal and vertical structures.

[0004] In the process of realizing this invention, the inventors discovered that the existing technology has at least the following problems: In the application of laser-induced graphene functionalization, both horizontal and vertical structures can exhibit excellent resistance strain function when bent in the direction perpendicular to the laser scan. However, when bent along the direction of the laser scan, the relative strain of its resistance is only half that of tangential bending, meaning that isotropic strain sensing cannot be achieved. This is an obvious obstacle to studying the ability of laser-induced graphene to sense strain from external sources in different directions. This property of laser-induced graphene is often used in the field of flexible sensors, which also hinders the research and development of flexible sensors in my country. Therefore, it is urgent to invent a laser-induced graphene material that can have isotropic strain sensing when bent in different directions. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor. By scanning the prepared PI film with an in-plane grid-shaped laser scanning method and specific laser parameters, laser-induced graphene with high carbonization is obtained, making the material isotropic when facing lateral and longitudinal bending, and easier to quantify external strain. Finally, the laser-induced pattern is customized and cut using the C4D software built into an ultraviolet laser cutting machine, demonstrating unique advantages in sensor fabrication.

[0006] To achieve the above-mentioned technical objectives, the technical solution adopted by the present invention is as follows:

[0007] A method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor, characterized by comprising the following steps:

[0008] Step 1: Preparation of the required PI film: Cut the PI film to the required size, then clean the surface with acetone, rinse with ultrapure water and dry to remove stains and dust from the PI film surface; Select a silicone pad with a thickness of 2-4 mm, wipe it clean with anhydrous ethanol, drop anhydrous ethanol on the upper surface, attach the PI film with a thickness of 40-60 μm to the silicone pad, press firmly to squeeze out the excess ethanol, and make the PI film adhere tightly to the silicone pad with the lubricant ethanol;

[0009] Step 2: Laser-induced graphene preparation: Place the prepared sample below the lens of an ultraviolet laser and mark its position with red light. Set the laser parameters: pulse frequency adjustable from 100 to 140 kHz, pulse width 1 to 3 μs, scanning speed 20 to 40 mm / s, scanning interval adjustable from 0.005 to 0.1 mm, and scanning method consisting of one horizontal scan followed by one vertical scan in the plane.

[0010] Step 3: Cut out the required pattern: Using the C4D software built into the UV laser cutter, the laser-induced pattern can be customized and LIG can be prepared by one-click marking. The prepared patterned LIG can then be cut off from the entire PI substrate using the cutting mode.

[0011] Preferably, the silicone pad in step one has a thickness of 2-4 mm and the PI film has a thickness of 40-60 μm.

[0012] Preferably, the laser parameters in step two are set as follows: the pulse wave frequency is adjustable from 100 to 140 kHz, the pulse width is 1 to 3 μs, the scanning speed is 20 to 40 mm / s, and the scanning spacing is adjustable from 0.005 to 0.1 mm.

[0013] Specifically, the laser scanning method in step two is a grid-like scanning (first horizontal then vertical or first vertical then horizontal).

[0014] Preferably, the laser cutting parameters of the ultraviolet laser cutting machine in step three are: pulse wave frequency of 15-25kHz, pulse width of 0.3-0.7μs, scanning speed of 10-30mm / s, and processing times of 1-10 times, with the aim of cutting out patterned laser-induced graphene.

[0015] The beneficial effects of this invention are:

[0016] Compared to chemical vapor deposition and hydrothermal methods, the laser-induced graphene processing method used in this invention can be carried out at room temperature without any solvents and is inexpensive. This method of laser ablation of PI avoids complex wet chemical methods and can directly prepare patterned structures, laying a solid foundation for the widespread application of graphene in the field of sensors.

[0017] The present invention uses a grid-shaped laser scanning method to prepare graphene with a special morphology. Studies have found that compared with the conventional straight-line structure, the grid-shaped structure has a higher degree of carbonization and forms more π-conjugated bonds, which is beneficial to enhance electron transport in graphene, improve conductivity, further enhance the order and regularity of its porous structure, and improve the material sensitivity and stability.

[0018] The present invention uses a grid-shaped laser scanning method to prepare its special morphology. Studies have found that, in terms of bending performance, the grid shape obtained by scanning twice, in the horizontal and vertical directions, is more isotropic than the conventional straight shape. This is helpful for the application of the sensor in special scenarios that require isotropic bending. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the specific embodiments of the present invention, the accompanying drawings used in the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0020] Figure 1 Here is a SEM image of the grid-shaped laser-induced graphene prepared in Example 1;

[0021] Figure 2 This is a magnified SEM image of the grid-shaped laser-induced graphene prepared in Example 1;

[0022] Figure 3 This is an optical microscope image of the grid-shaped laser-induced graphene prepared in Example 1;

[0023] Figure 4 This is a photograph of the Raman spectrum of the laser-induced graphene in the grid pattern prepared in Example 1;

[0024] Figure 5 These are the resistance response curves of the grid-shaped laser-induced graphene flexible strain sensor prepared in Example 1 when bent along the coaxial and tangential directions;

[0025] Figure 6 These are the resistance response curves of the laser-induced graphene flexible strain sensor with a linear structure prepared in Example 2, when bent along the longitudinal and tangential directions.

[0026] Comparison of the sensing performance of laser-induced graphene materials under bending strain;

[0027] Figure 7 Here are SEM images of the transverse scanning laser-induced graphene material prepared in Example 2;

[0028] Figure 8 This is a SEM image of the longitudinally scanned laser-induced graphene material prepared in Example 3. Detailed Implementation

[0029] The present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Other embodiments obtained by those skilled in the art within the scope of the embodiments of the present invention without inventive effort are all within the protection scope of the present invention.

[0030] Example 1

[0031] 1. A method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor, characterized by comprising the following steps:

[0032] Step 1: Preparation of the required PI film: Cut the PI film to the required size, then clean the surface with acetone, rinse with ultrapure water, and dry to remove stains and dust from the PI film surface. Select a silicone pad with a thickness of 2-4 mm, wipe it clean with anhydrous ethanol, drop anhydrous ethanol onto the upper surface, and attach the 40-60 μm thick PI film to the silicone pad. Press firmly to squeeze out the excess ethanol, allowing the PI film to adhere tightly to the silicone pad through the lubricant ethanol.

[0033] Step 2: Preparation using laser with specific parameters: Place the prepared sample below the lens of the ultraviolet laser and mark its position with red light. Set the laser parameters: pulse frequency adjustable from 100 to 140 kHz, pulse width from 1 to 3 μs, scanning speed from 20 to 40 mm / s, scanning interval adjustable from 0.005 to 0.1 mm, and scanning method as a grid scan (horizontal first, then vertical).

[0034] Step 3: Cut out the desired pattern: Using the C4D software built into the UV laser cutter, the laser-induced pattern can be customized and LIG can be prepared by one-click marking. The cutting mode is: pulse wave frequency of 15-25kHz, pulse width of 0.3-0.7μs, scanning speed of 10-30mm / s, and processing times of 1-10 times. The prepared patterned LIG is then cut off from the whole PI substrate.

[0035] The above is the core content of this invention: a PI film is prepared by scanning with a planar grid-like laser scanning method and specific laser parameters. Finally, the laser-induced pattern is customized using the C4D software built into the ultraviolet laser cutting machine. This effectively enables the material to have superior strain performance when facing bending in different directions, achieves personalized design, and also exhibits superior performance in sensors.

[0036] Specifically, step one, preparation of the required PI film: cut the PI film to the required size, then clean the surface with acetone, rinse with ultrapure water, and dry to remove stains and dust from the PI film surface. Select a 3μm thick silicone pad, wipe it clean with anhydrous ethanol, drop anhydrous ethanol onto the upper surface, attach the 50μm thick PI film to the silicone pad, press firmly to squeeze out excess ethanol, and use the lubricant ethanol to tightly adhere the PI film to the silicone pad;

[0037] Step 2: Preparation using laser with specific parameters: Place the prepared sample below the lens of the ultraviolet laser and mark its position with red light. Set the laser parameters as follows: pulse frequency of 120Hz, pulse width of 2μs, scanning speed of 30mm / s, scanning interval of 0.01mm, and scanning method of one horizontal scan followed by one vertical scan (grid pattern) in the plane.

[0038] Step 3: Cut out the desired pattern: Using the C4D software built into the UV laser cutter, the laser-induced pattern can be customized and LIG can be prepared by one-click marking. The patterned LIG is cut from the whole PI substrate in a single cutting mode with a pulse wave frequency of 20kHz, a pulse width of 0.5μs, and a scanning speed of 20mm / s.

[0039] Example 2

[0040] A method for fabricating a laser-induced graphene flexible strain sensor in the shape of an "I" is characterized by comprising the following steps:

[0041] Specifically, step one, preparation of the required PI film: cut the PI film to the required size, then clean the surface with acetone, rinse with ultrapure water, and dry to remove stains and dust from the PI film surface. Select a 3μm thick silicone pad, wipe it clean with anhydrous ethanol, drop anhydrous ethanol onto the upper surface, attach the 5μm thick PI film to the silicone pad, press firmly to squeeze out excess ethanol, and use the lubricant ethanol to tightly adhere the PI film to the silicone pad;

[0042] Step 2: Preparation with laser under specific parameters: Place the prepared sample below the lens of an ultraviolet laser, and mark the position of the sample with red light. Set the laser parameters as follows: pulse wave frequency of 120 Hz, pulse width of 2 μs, scanning speed of 30 mm / s, scanning spacing of 0.01 mm, and scanning mode of one horizontal scan in the plane.

[0043] Step 3: Cut out the desired pattern: Conduct personalized design on the laser-induced pattern through the C4D software built into the ultraviolet laser cutting machine, and prepare LIG through one-step marking. The prepared patterned LIG is cut from the entire PI substrate through a single processing mode with a pulse wave frequency of 20 kHz, a pulse width of 0.5 μs, and a scanning speed of 20 mm / s.

[0044] Embodiment 3

[0045] A method for preparing a "丨"-shaped microstructure laser-induced graphene flexible strain sensor, comprising the following steps:

[0046] Specifically, Step 1: Preparation of the required PI film: Cut the PI film into the required size, then clean the surface with acetone, rinse it with ultrapure water and dry it to remove stains, dust, etc. on the surface of the PI film. Select a silicone pad with a thickness of 3 m, wipe it clean with absolute ethanol, drop absolute ethanol on the upper surface, attach the 5 μm-thick PI film to the silicone pad, press firmly to squeeze out excess ethanol, and make the PI film closely adhere to the silicone pad through the action of the lubricant ethanol.

[0047] Step 2: Preparation with laser under specific parameters: Place the prepared sample below the lens of an ultraviolet laser, and mark the position of the sample with red light. Set the laser parameters as follows: pulse wave frequency of 120 Hz, pulse width of 2 μs, scanning speed of 30 mm / s, scanning spacing of 0.01 mm, and scanning mode of one vertical scan in the plane.

[0048] Step 3: Cut out the desired pattern: Conduct personalized design on the laser-induced pattern through the C4D software built into the ultraviolet laser cutting machine, and prepare LIG through one-step marking. The prepared patterned LIG is cut from the entire PI substrate through a single processing mode with a pulse wave frequency of 20 kHz, a pulse width of 0.5 μs, and a scanning speed of 20 mm / s.

[0049] The SEM image of the grid-shaped laser-induced graphene material prepared in Embodiment 1 is shown in Figure 1 and 2 . It can be seen from Figure 1 that the LIG obtained under the grid-shaped scanning mode presents a regular grid-shaped structure, and the prepared material has good uniformity and stability, which meets the expected effects. Figure 3 The grid-like structure can also be clearly seen in optical microscope images.

[0050] The Raman spectrum of the final product prepared in Example 1 using the grid scanning method is shown in the image below. Figure 4 As shown, the Raman spectroscopy results further indicate that when the scanning spacing is 0.1 mm, the ID / IG ratio drops to 0.6 and the I2D / IG ratio is 0.2, proving that the graphene generated under these parameters has the fewest defects and the highest degree of graphitization.

[0051] The experiment also investigated the effect of bending direction on the sensing performance of the LIG sensor. The relative change in resistance of the LIG flexible strain sensor with a linear structure along the bending direction was only half that in the tangential direction. Figure 6 This indicates that the sensing performance of laser-induced LIG exhibits significant differences between axial and tangential bending, with the sensor showing higher sensitivity along the tangential direction. Comparing the sensing performance of the grid-shaped LIG sensor along axial and tangential bending, both axial and tangential directions show a relative resistance change exceeding 8% at a 90° bend, demonstrating that the grid-shaped microstructure LIG obtained through two transverse and longitudinal scans is isotropic in bending test performance. Figure 5 The superiority of the grid-shaped LIG structure design will help the sensor be used in special scenarios that require isotropic bending.

[0052] The SEM image of the laser-induced graphene material prepared in Example 2 is shown below. Figure 7 As shown in the figure, the laser-induced graphene material with obvious stripe structure can be seen. Compared with Example 1, the scanning method in this example is a single horizontal scan, and the conductive pathways are reduced and the degree of carbonization is decreased.

[0053] The SEM image of the laser-induced graphene material prepared in Example 3 is shown below. Figure 8 As shown in the figure, the laser-induced graphene material with obvious stripe structure can be seen. Compared with Example 1, the scanning method in this example is a vertical scan once, and it is observed that the conductive pathway is reduced and the degree of carbonization is reduced.

[0054] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor, characterized in that, Includes the following steps: Step 1: Pretreatment of PI film: Cut the PI film to the required size, then clean the surface with acetone, rinse with ultrapure water and dry; wipe the silicone pad clean with anhydrous ethanol, drop anhydrous ethanol on the upper surface, attach the PI film to the silicone pad, press firmly to squeeze out the excess ethanol, and make the PI film adhere tightly to the silicone pad through the action of ethanol. Step 2: Preparation of laser-induced graphene: The laser-induced pattern is customized using the C4D software built into the UV laser cutter. Then, the pretreated PI film is placed below the UV laser lens. The position of the sample is marked with red light, and the laser scanning parameters are adjusted to prepare laser-induced graphene. The laser scanning method is a grid-like scanning. Step 3: Cutting patterned laser-induced graphene: Adjust the laser cutting parameters and use the C4D software built into the UV laser cutting machine to mark the edges of the prepared laser-induced graphene with one click, and peel the patterned laser-induced graphene off the PI film. The laser parameters for step two are set as follows: pulse frequency of 100~140 kHz, pulse width of 1~3 μs, scanning speed of 20~40 mm / s, and scanning spacing of 0.005~0.1 mm.

2. The method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor as described in claim 1, characterized in that, The silicone pad used in step one has a thickness of 2-4 mm, and the PI film has a thickness of 40-100 μm.

3. The method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor as described in claim 1, characterized in that, The laser scanning method in step two is either horizontal first and then vertical, or vertical first and then horizontal.

4. The method for fabricating a grid-shaped microstructure laser-induced graphene flexible strain sensor as described in claim 1, characterized in that, In step three, the patterned laser-induced graphene is cut using laser cutting parameters of 15-25 kHz pulse frequency, 0.3-0.7 μs pulse width, 10-30 mm / s scanning speed, and 1-10 processing times.