Conductive polymer aqueous solution for photolithography and conductive polymer hydrogel prepared thereby
By simplifying the photolithography process through spin coating, exposure, and development steps of conductive polymer aqueous solution for photolithography, high-resolution conductive polymer hydrogels can be prepared, solving the problems of insufficient resolution and complexity in existing technologies and realizing rapid processing of high-performance conductive polymer hydrogels.
Patent Information
- Application Number
- CN202310320395.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing photolithography technology suffers from insufficient resolution, loss of material properties, and processing complexity when processing conductive polymer hydrogels, making it difficult to achieve high-density integrated applications.
Conductive polymer hydrogels are prepared by using an aqueous solution of conductive polymer for photolithography through spin coating, exposure and development steps, which simplifies the photolithography process and avoids the etching and photoresist removal steps. The conductive polymer aqueous solution is prepared by using a photocurable polymer and a photoinitiator and spin-coated onto a variety of substrates to achieve high-resolution patterning.
High-resolution <20μm conductive polymer hydrogels were achieved, with material conductivity as high as >2000S/m, reducing costs and time, and promoting the development of rapid, high-resolution advanced processing technology for conductive polymer hydrogels.
Smart Images

Figure CN117192894B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photolithography, and in particular to an aqueous solution of a conductive polymer for photolithography and a conductive polymer hydrogel prepared therefrom. Background Technology
[0002] Conductive polymers have been extensively studied due to their combination of lightweight, easy processing, tunable mechanical properties, and excellent electrical conductivity. In particular, conductive polymer hydrogels generated from precursor aqueous solutions combine mechanical properties similar to human tissue, good biocompatibility, and excellent electrical properties, and are widely used in fields such as flexible sensors, electronic skin, wearable and implantable electronic devices.
[0003] Currently, the processing technology of conductive polymer hydrogels mainly relies on inkjet printing (CN201810128796.7), screen printing (CN201910703519.9), and the recently developed 3D printing technology (CN202210882673.9). Although these processing technologies can meet the customized patterning processing of conductive polymer hydrogels, the resolution is generally >50μm, which greatly hinders the high-density integrated application of conductive polymer hydrogels. In contrast, photolithography can obtain high-resolution patterns, but conductive polymers composed of a single component have the following problems during photolithography processing: (1) the combination of conjugated chain segments in conductive polymers produces low-energy orbitals, resulting in redshift of absorption, and the color deepens and absorbance increases with the growth of conjugated chains; (2) the conductive polymer molecular chain segments lack chemical sites for direct reaction, and after exposure and development, high-resolution patterns cannot be obtained through differences in solubility; (3) in traditional photolithography, the etching step will destroy the chemical structure of conductive polymers, resulting in a decrease in properties such as conductivity.
[0004] Based on this, the development of conductive polymer aqueous solutions for photolithography and the conductive polymer hydrogels prepared therefrom can further fill advanced processing technologies for conductive polymers, promote high-density processing and integration of conductive hydrogels, and their application in many fields such as flexible electronics and biomedical engineering. Summary of the Invention
[0005] To address the aforementioned problems in existing technologies, this invention provides a conductive polymer aqueous solution for photolithography and the conductive polymer hydrogel prepared therefrom. This technology eliminates the need for photoresist, reducing conventional steps such as etching and photoresist removal, simplifying the photolithography process and shortening its time consumption. Simultaneously, the conductive polymer aqueous solution is low-cost, and the prepared conductive polymer hydrogel exhibits high pattern resolution and excellent electrical and mechanical properties, making it promising for applications in flexible electronics, biomedical engineering, and other fields.
[0006] The technical solution of the present invention is as follows:
[0007] The first objective of this invention is to provide a method for preparing an aqueous solution of an electropolymer for photolithography, comprising the following steps:
[0008] (1) Dissolve 1-1.3% of the conductive polymer in water to prepare an aqueous solution of the conductive polymer;
[0009] (2) Add 1-2% of photocurable polymer to the conductive polymer solution obtained in step (1), stir and homogenize at room temperature to obtain a conductive polymer mixed solution.
[0010] (3) Add 0.01-0.078% photoinitiator to the conductive polymer mixed solution obtained in step (2), mix evenly, and obtain the conductive polymer aqueous solution for photolithography.
[0011] Preferably, the conductive polymer in step (1) is one or more of poly(3,4-dioxanethiophene): polystyrene sulfonate, polyaniline-poly(4-styrene sulfonate), poly(3,4-ethylenedioxanethiophene): dextran sulfate, and poly(6-(thiophene-3-yl)hexane-1-sulfonate).
[0012] Preferably, the photocurable polymer in step (2) is one of polyvinyl alcohol-styrene pyridinium salt, sulfonic acid type polyurethane acrylate, non-isocyanate polyurethane acrylate, and silicone-containing polyurethane acrylate.
[0013] Preferably, the photoinitiator in step (3) is one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, ethyl 2,4,6-trimethylbenzoylphosphonate, and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
[0014] A second objective of this invention is to provide a method for preparing conductive polymer hydrogels using photolithography, comprising the following steps:
[0015] (1) Spin-coating the conductive polymer aqueous solution onto a substrate and then air-drying it naturally to obtain a film with a thickness of 100-180 nm;
[0016] (2) A chromium mask is placed on the thin film for exposure;
[0017] (3) After exposure, place the sample in deionized water at room temperature for 5-10 minutes to develop, and a patterned conductive polymer hydrogel is obtained.
[0018] Preferably, in step (1), the substrate is one of the following: clean glass, polyethylene terephthalate film, polyethylene film, polydimethylsiloxane film, polyimide film, polyester film, paper, and pigskin.
[0019] Preferably, in step (1), the spin coating conditions are: rotating at a speed of 600-800 r / min for 15-30 s, and then rotating at a speed of 1000-1500 r / min for 30-40 s.
[0020] Preferably, in step (2), the exposure conditions are: 100-150 mW cm⁻¹ at a 365 nm ultraviolet wavelength. -2 Expose at a constant intensity for 1-2 minutes.
[0021] Preferably, in step (3), after development, a post-treatment step is further included. The post-treatment method is to immerse the conductive polymer hydrogel formed after development in a 0.01 mol / L post-treatment aqueous solution for 1-2 hours. In one embodiment of the present invention, the post-treatment aqueous solution is an aqueous solution of sodium chloride, potassium chloride, calcium chloride, magnesium chloride, ferric chloride, methanol, polyethylene glycol, hydrochloric acid, or sulfuric acid.
[0022] The beneficial technical effects of this invention are as follows:
[0023] (1) A conductive polymer aqueous solution for photolithography was prepared using conductive polymer, photocurable polymer, photoinitiator, etc. The solution can be spin-coated onto a variety of substrates and high-performance patterned conductive polymer hydrogels can be prepared by photolithography. The photolithography resolution is <20μm and the material conductivity is as high as >2000S / m. It is expected to be used in flexible electronics, biomedical engineering and other fields.
[0024] (2) Compared with traditional photolithography processes, the photolithography process in this invention does not require the use of photoresist, greatly simplifies the photolithography process, reduces material and equipment costs, shortens processing time, and promotes the development of rapid and high-resolution advanced processing technology for conductive polymer hydrogels. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the photolithography conductive polymer hydrogel process in this invention;
[0026] Figure 2 Here is a simplified structural formula for the conductive polymer used in this invention;
[0027] Figure 3 Here is the simplified structural formula of the photocurable polymer used in this invention;
[0028] Figure 4 The following are the thin films obtained by spin-coating and air-drying at room temperature on different substrates using photolithographic conductive polymer aqueous solutions in this invention: polyester film (a), polyethylene terephthalate film (b), polyethylene film (c), and glass (d).
[0029] Figure 5 The ultraviolet transmittance at different positions of the spin-coated film in Example 1 of this invention;
[0030] Figure 6 This refers to the photocurable polymer double bond conversion rate membrane used in Examples 1 and 2 of this invention;
[0031] Figure 7 These are optical micrographs from the present invention. (a) and (b) have a resolution of 50 μm, and (c) and (d) have a resolution of 15 μm. Detailed Implementation
[0032] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0033] Example 1
[0034] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0035] (1) Disperse 50 mg PEDOT:PSS, 50 mg polyvinyl alcohol-styrene pyridinium salt, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0036] (2) The solution in step (1) is dropped onto a clean glass substrate. The substrate is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 120 nm.
[0037] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0038] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0039] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L sodium chloride aqueous solution for 1 hour before conductivity testing.
[0040] Example 2:
[0041] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0042] (1) Disperse 50 mg PANI-PSS, 50 mg polyvinyl alcohol-styrene pyridinium salt, and 1.2 mg of 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0043] (2) The solution in step (1) above is drop-coated onto a clean polyethylene terephthalate film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 128 nm.
[0044] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 100 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0045] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0046] (5) Drop the solution from step (1) onto a cleaned polyethylene terephthalate film, air dry at room temperature, and then apply a 100mW cm⁻¹ pressure coating. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L potassium chloride aqueous solution for 1 hour before conductivity testing.
[0047] Example 3:
[0048] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0049] (1) Disperse 50 mg PEDOT:DS, 50 mg polyvinyl alcohol-styrene pyridinium salt, and 1.2 mg 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0050] (2) The solution in step (1) above is dropped onto a clean polyethylene film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 135 nm.
[0051] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0052] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0053] (5) Apply the solution from step (1) above onto a cleaned polyethylene film, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L calcium chloride aqueous solution for 1 hour before conductivity testing.
[0054] Example 4:
[0055] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0056] (1) Disperse 50 mg PTHS, 50 mg polyvinyl alcohol-styrene pyridinium salt, and 1.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0057] (2) The solution in step (1) above is dropped onto the cleaned polydimethylsiloxane film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 130 nm.
[0058] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 145 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0059] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0060] (5) Drop the solution from step (1) onto a cleaned polydimethylsiloxane film, air dry at room temperature, and then apply a 145mW cm⁻¹ coating. -2 The light source was fixed in an ultraviolet box with a wavelength of 365nm for 2 minutes, and after development with deionized water, the conductivity was tested.
[0061] Example 5
[0062] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0063] (1) Disperse 50 mg PEDOT:PSS, 50 mg sulfonic acid polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0064] (2) The solution in step (1) above is dropped onto the cleaned polyimide film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 120 nm.
[0065] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0066] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop it and obtain the preset pattern on the mask.
[0067] (5) Drop the solution from step (1) onto the cleaned polyimide film, air dry at room temperature, and then apply a 125mW / cm² strength coating. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L sodium chloride aqueous solution for 1 hour before conductivity testing.
[0068] Example 6:
[0069] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0070] (1) Disperse 50 mg PANI-PSS, 50 mg sulfonic acid polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0071] (2) The solution in step (1) above is dropped onto a clean polyester film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 128 nm.
[0072] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0073] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0074] (5) Drop the solution from step (1) onto a cleaned polyester film, air dry at room temperature, and then apply a 125mW cm⁻¹ coating. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L potassium chloride aqueous solution for 1 hour before conductivity testing.
[0075] Example 7:
[0076] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0077] (1) Disperse 50 mg PEDOT:DS, 50 mg sulfonic acid polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0078] (2) The solution in step (1) above is dropped onto clean paper. The paper is first spread by rotating at 600 r / min for 20 seconds on a spin coater, and then thinned by rotating at 1000 r / min for 40 seconds. After that, it is air-dried at room temperature to obtain a uniform film of 135 nm.
[0079] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0080] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0081] (5) Apply the solution from step (1) above onto clean paper, let it air dry at room temperature, and then apply a 125mWcm solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L calcium chloride aqueous solution for 1 hour before conductivity testing.
[0082] Example 8:
[0083] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0084] (1) Disperse 50 mg PTHS, 50 mg sulfonic acid polyurethane acrylate, and 1.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0085] (2) The solution in step (1) above is dropped onto clean pigskin. The solution is first spread in a cyclic manner by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 130 nm.
[0086] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 145 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0087] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0088] (5) Apply the solution from step (1) above to the cleaned pigskin, let it air dry at room temperature, and then apply a 145mWcm solution. -2 The light source was fixed in an ultraviolet box with a wavelength of 365nm for 2 minutes, and after development with deionized water, the conductivity was tested.
[0089] Example 9
[0090] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0091] (1) Disperse 50 mg PEDOT:PSS, 50 mg non-isocyanate polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0092] (2) The solution in step (1) is dropped onto a clean glass substrate. The substrate is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 120 nm.
[0093] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0094] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0095] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L sodium chloride aqueous solution for 1 hour before conductivity testing.
[0096] Example 10:
[0097] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0098] (1) Disperse 50 mg PANI-PSS, 50 mg non-isocyanate polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0099] (2) The solution in step (1) above is dropped onto a clean polyethylene film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 128 nm.
[0100] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0101] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0102] (5) Apply the solution from step (1) above onto a cleaned polyethylene film, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L potassium chloride aqueous solution for 1 hour before conductivity testing.
[0103] Example 11:
[0104] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0105] (1) Disperse 50 mg PEDOT:DS, 50 mg non-isocyanate polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0106] (2) The solution in step (1) above is dropped onto a clean glass substrate. The substrate is first rotated at 600 r / min for 20 s to spread it, and then rotated at 1000 r / min for 40 s to thin it. After that, it is air-dried at room temperature to obtain a uniform film of 135 nm.
[0107] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0108] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0109] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 10 minutes, developed with deionized water, and then immersed in a 0.01mol / L ethylene glycol aqueous solution for 1 hour before conductivity testing.
[0110] Example 12:
[0111] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0112] (1) Disperse 50 mg PTHS, 50 mg silicone polyurethane acrylate and 1.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0113] (2) The solution in step (1) above is dropped onto the cleaned polydimethylsiloxane film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 130 nm.
[0114] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 145 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0115] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop it and obtain the preset pattern on the mask.
[0116] (5) Drop the solution from step (1) onto a cleaned polydimethylsiloxane film, air dry at room temperature, and then apply a 125 mW cm⁻¹ coating. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 10 minutes, developed with deionized water, and then immersed in a 0.01mol / L hydrochloric acid aqueous solution for 1 hour before conductivity testing.
[0117] Example 13
[0118] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0119] (1) Disperse 50 mg PEDOT:PSS, 50 mg silicone polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0120] (2) The solution in step (1) above is dropped onto clean paper. The paper is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 120 nm.
[0121] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0122] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop it and obtain the preset pattern on the mask.
[0123] (5) Apply the solution from step (1) above onto clean paper, let it air dry at room temperature, and then apply a 100mWcm solution. -2 The light source was fixed in an ultraviolet box with a wavelength of 365nm for 2 minutes, and after development with deionized water, the conductivity was tested.
[0124] Example 14:
[0125] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0126] (1) Disperse 50 mg PANI-PSS, 50 mg silicone polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0127] (2) The solution in step (1) is dropped onto a clean glass substrate. The substrate is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 128 nm.
[0128] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0129] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop, and obtain the preset pattern on the mask.
[0130] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L potassium chloride aqueous solution for 1 hour before conductivity testing.
[0131] Example 15:
[0132] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0133] (1) Disperse 50 mg PEDOT:DS, 50 mg silicone polyurethane acrylate, and 1.2 mg 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone evenly in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0134] (2) The solution in step (1) above is drop-coated onto a clean polyethylene terephthalate film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 135 nm.
[0135] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 125 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0136] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop it and obtain the preset pattern on the mask.
[0137] (5) Drop the solution from step (1) onto a cleaned polyethylene terephthalate film, air dry at room temperature, and then apply a 100mW cm⁻¹ pressure coating. -2 The light source was fixed in an ultraviolet box with a wavelength of 365nm for 2 minutes, and after development with deionized water, the conductivity was tested.
[0138] Example 16:
[0139] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0140] (1) Disperse 50 mg PTHS, 50 mg silicone polyurethane acrylate and 1.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in 5 ml of deionized water to prepare a conductive polymer mixed solution with a concentration of 2.02 wt%.
[0141] (2) The solution in step (1) is drop-coated onto a clean polyester film. The film is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 130 nm.
[0142] (3) Place a chromium mask on the thin film obtained in step (2) above, and apply a pressure of 145 mW / cm². -2 A UV chamber with a light source wavelength of 365nm was used for 1 minute.
[0143] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 5 minutes to develop it and obtain the preset pattern on the mask.
[0144] (5) Drop the solution from step (1) onto a cleaned polyester film, air dry at room temperature, and then apply a 125mW cm⁻¹ coating. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 10 minutes, developed with deionized water, and then immersed in a 0.01mol / L sodium chloride aqueous solution for 1 hour before conductivity testing.
[0145] Example 17:
[0146] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0147] (1) Disperse 27.5 mg PEDOT:PSS, 27.5 mg PANI-PSS, 80 mg polyvinyl alcohol-styrene pyridinium salt, and 3.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in deionized water to prepare a conductive polymer mixed solution with a concentration of 2.76 wt%.
[0148] (2) The solution in step (1) above is dropped onto a clean glass substrate. The substrate is first rotated at 600 r / min for 20 s to spread it, and then rotated at 1000 r / min for 40 s to thin it. After that, it is air-dried at room temperature to obtain a uniform film of 150 nm.
[0149] (3) Place the thin film obtained in step (2) under a chromium mask and heat it with a strength of 100 mW / cm². -2 Curing in a UV box with a light source wavelength of 365nm for 1 minute;
[0150] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 7 minutes to develop, and obtain the preset pattern on the mask.
[0151] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 100mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L ethylene glycol aqueous solution for 1 hour before conductivity testing.
[0152] Example 18:
[0153] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0154] (1) Disperse 27.5 mg PEDOT:DS, 27.5 mg PANI-PSS, 80 mg sulfonic acid type polyurethane acrylate, and 3.2 mg ethyl 2,4,6-trimethylbenzoylphosphonate in deionized water to prepare a conductive polymer mixed solution with a concentration of 2.76 wt%.
[0155] (2) The solution in step (1) above is dropped onto the cleaned pigskin. First, it is rotated at 600 r / min for 20 s to spread it in a circular motion, and then rotated at 1000 r / min for 40 s to thin it. Then it is air-dried at room temperature to obtain a uniform film of 145 nm.
[0156] (3) Place the thin film obtained in step (2) under a chromium mask and heat it with a strength of 100 mW / cm². -2 Curing in a UV box with a light source wavelength of 365nm for 1 minute;
[0157] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 6 minutes to develop, and obtain the preset pattern on the mask.
[0158] (5) Apply the solution from step (1) above to the cleaned pigskin, let it air dry at room temperature, and then apply a 125mWcm solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 10 minutes, developed with deionized water, and then immersed in a 0.01mol / L potassium chloride aqueous solution for 1 hour before conductivity testing was performed.
[0159] Example 19:
[0160] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0161] (1) Disperse 27.5 mg PEDOT:DS, 27.5 mg PTHS, 80 mg non-isocyanate polyurethane acrylate, and 3.2 mg 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone evenly in deionized water to prepare a conductive polymer mixed solution with a concentration of 2.76 wt%.
[0162] (2) The solution in step (1) above is drop-coated onto the cleaned polydimethylsiloxane film. The coating method is as follows: first, rotate at a speed of 600 r / min for 20 s to spread it in a circular motion, then rotate at a speed of 1000 r / min for 40 s to thin it, and then air dry at room temperature to obtain a uniform film of 155 nm.
[0163] (3) Place the thin film obtained in step (2) under a chromium mask and heat it with a strength of 125 mW / cm². -2 Curing in a UV box with a light source wavelength of 365nm for 1 minute;
[0164] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 6 minutes to develop, and obtain the preset pattern on the mask.
[0165] (5) Drop the solution from step (1) onto a cleaned polydimethylsiloxane film, air dry at room temperature, and then apply a 125 mW / cm² pressure coating. -2 The light source was fixed in an ultraviolet box with a wavelength of 365nm for 2 minutes, and after development with deionized water, the conductivity was tested.
[0166] Example 20:
[0167] A method for preparing conductive polymer hydrogels using photolithography includes the following steps:
[0168] (1) Disperse 30 mg PTHS, 30 mg PANI-PSS, 80 mg silicone polyurethane acrylate and 1.6 mg ethyl 2,4,6-trimethylbenzoylphosphonate in deionized water to prepare a conductive polymer mixed solution with a concentration of 2.83 wt%.
[0169] (2) The solution in step (1) is drop-coated onto a clean glass substrate. First, it is rotated at 600 r / min for 20 s to spread it in a circular motion, and then rotated at 1000 r / min for 40 s to thin it. After that, it is air-dried at room temperature to obtain a uniform film of 160 nm.
[0170] (3) Place the thin film obtained in step (2) under a chromium mask and heat it with a strength of 125 mW / cm². -2 Curing in a UV box with a light source wavelength of 365nm for 1 minute;
[0171] (4) Place the film selectively exposed in step (3) above in deionized water at room temperature for 6 minutes to develop, and obtain the preset pattern on the mask.
[0172] (5) Drop the solution from step (1) onto a clean glass substrate, allow it to air dry at room temperature, and then apply a 125mW cm⁻¹ solution. -2 The sample was placed in a UV box with a light source wavelength of 365nm for 2 minutes, developed with deionized water, and then immersed in a 0.01mol / L hydrochloric acid aqueous solution for 1 hour before conductivity testing was performed.
[0173] Comparative Example 1
[0174] (1) Disperse 50mg PEDOT:PSS and 50mg sulfonic acid type waterborne polyurethane acrylate evenly in deionized water to prepare a conductive polymer mixed solution with a concentration of 2wt%.
[0175] (2) The solution in step (1) is dropped onto a clean glass substrate. The substrate is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 115 nm.
[0176] (3) Place the film from step (2) above in a 125mW / cm² intensity zone. -2 The sample was cured in a UV chamber with a light source wavelength of 365nm for 1 minute, and then developed in deionized water for 5 minutes. It was found that the unexposed area and the exposed area were dispersed in the deionized water.
[0177] Comparative Example 2
[0178] (1) Disperse 50 mg PEDOT:PSS and 1.2 mg 2-hydroxy-2-methyl-1-phenyl-1-propanone evenly in deionized water to prepare a conductive polymer mixed solution with a concentration of 1.02 wt%.
[0179] (2) The solution in step (1) is dropped onto a clean glass substrate. The substrate is first spread by rotating at 600 r / min for 20 s on a spin coater, and then thinned by rotating at 1000 r / min for 40 s. After that, it is air-dried at room temperature to obtain a uniform film of 100 nm.
[0180] (3) The film from step (2) was placed in an ultraviolet box with an intensity of 125mW cm-2 and a light source wavelength of 365nm for 1 min to cure, and then developed in deionized water for 5 min. It was found that the unexposed area and the exposed area were dispersed in the deionized water.
[0181] The conductivity of the hydrogel in some different embodiments is shown in Table 1.
[0182] Table 1
[0183] Example electrical conductivity Example 1 2890S / m Example 2 2170S / m Example 3 2360S / m Example 4 19S / m Example 5 2130S / m Example 6 2350S / m Example 7 2640S / m Example 8 23S / m Example 9 2250S / m Example 10 2370S / m Example 11 2270S / m Example 12 2760S / m Example 13 24S / m Example 14 2780S / m Example 15 21S / m Example 16 2340S / m Example 17 2410S / m Example 18 2670S / m Example 19 26S / m Example 20 2490S / m
[0184] The above description is merely an example and illustration of the proportional optimization in this invention. The technology in this technical field is not limited to this invention. Any modifications, substitutions, improvements, etc., made within the spirit and principles of the invention should fall within the protection scope of this invention.
Claims
1. An aqueous solution of a conductive polymer for photolithography, characterized in that, The conductive polymer aqueous solution comprises the following raw materials in the following mass percentages: 1-1.3% conductive polymer, 1-2% photocurable polymer, 0.01-0.078% photoinitiator, and the balance being water; The conductive polymer is poly(3,4-dioxanethiophene):polystyrene sulfonate; The photocurable polymer is an aqueous photocurable polymer, and the aqueous photocurable polymer is polyvinyl alcohol-styrene pyridine salt; The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
2. The conductive polymer aqueous solution for photolithography according to claim 1, characterized in that, The photolithographic preparation method of the conductive polymer aqueous solution includes the following technical operation process: (1) Spin-coating an aqueous solution of conductive polymer onto a substrate and then air-drying it to obtain a film with a thickness of 100-180 nm. (2) A chromium mask is placed on the thin film for exposure; (3) After exposure, place it in deionized water at room temperature for 5-10 minutes to develop, and a patterned conductive polymer hydrogel is obtained.
3. The conductive polymer aqueous solution for photolithography according to claim 2, characterized in that, In step (1), the substrate is one of the following: clean glass, polyethylene terephthalate film, polyethylene film, polydimethylsiloxane film, polyimide film, polyester film, paper, and pigskin; the spin coating conditions are: rotating at a speed of 600-800 r / min for 15-30 s, and then rotating at a speed of 1000-1500 r / min for 30-40 s.
4. The conductive polymer aqueous solution for photolithography according to claim 2, characterized in that, In step (2), the exposure conditions are: 100-150 mW / cm² at a UV wavelength of 365 nm. -2 Expose at a constant intensity for 1-2 minutes.
5. The aqueous solution of the conductive polymer for photolithography according to claim 2, characterized in that, In step (3), after development, there is also a post-processing step. The post-processing method is to immerse the conductive polymer hydrogel formed after development in a 0.01 mol / L post-processing aqueous solution for 1-2 hours.
6. The conductive polymer aqueous solution for photolithography according to claim 2, characterized in that, The post-treatment aqueous solution is one of sodium chloride, potassium chloride, calcium chloride, magnesium chloride, ferric chloride, methanol, polyethylene glycol, hydrochloric acid, or sulfuric acid aqueous solution.
7. The conductive polymer aqueous solution for photolithography according to claim 2, characterized in that, The conductive polymer hydrogel prepared from the aqueous solution of the conductive polymer for photolithography has a conductivity >2000 S / m and a pattern resolution <20 μm.
Citation Information
Patent Citations
Preparation method of water-based UV conductive ink
CN108148469A
A method for fabricating a flexible sensor array made of composite conductive polymer
CN110438829B
Stretchable polyaniline composite hydrogel based on ink direct writing 3D printing as well as preparation method and application of stretchable polyaniline composite hydrogel
CN115093581A
Directly photo-patternable, stretchable, electrically conductive polymer
US20200401042A1