Synaptic transistor device based on nitroxide radical small molecule and preparation and application thereof
By utilizing the redox properties of nitric oxide radical small molecule materials in synaptic transistor devices, high linearity electronic writing and multi-level switching characteristics were achieved, solving the problem of nonlinear response in traditional transistor devices. This simulates biological synaptic function and can be applied to artificial intelligence and information processing.
Patent Information
- Application Number
- CN202311285064.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-07
AI Technical Summary
Traditional synaptic transistors exhibit nonlinear conductance response under the same peak signal, which affects the convergence speed and classification accuracy of the algorithm, making it difficult to achieve high linearity electronic writing and multi-resistance state modulation, thus limiting their application in artificial neural networks.
By using nitric oxide radical small molecule materials as charge trapping layers and achieving a slow kinetic process under voltage modulation through redox properties, synaptic transistor devices based on nitric oxide radical small molecules are fabricated, including gate electrode, gate insulating layer, P-type semiconductor layer and source/drain electrodes. The slow redox process is used to achieve precise control of channel conductivity.
It achieves high linearity electronic writing and multi-level switching characteristics, and can simulate the excitation and inhibition processes of biological synapses, making it suitable for information processing and storage in the field of artificial intelligence.
Smart Images

Figure CN117202673B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of semiconductor technology and neuromorphic hardware, specifically relating to a synaptic transistor device, and more particularly to a synaptic transistor device based on nitric oxide radical small molecules, its fabrication, and its application. Background Technology
[0002] The advent of the era of artificial intelligence and big data has presented new challenges to current computing hardware and systems. Due to the physical separation of memory and computing units, the traditional von Neumann architecture faces bottlenecks in improving computing power and energy efficiency. Reconfigurable three-terminal synaptic transistors are among the most promising devices for building analog neural networks for neuromorphic computing; however, most synaptic transistors exhibit nonlinear conductance responses under the same peak signals, negatively impacting the convergence speed and classification accuracy of algorithms. This interferes with training efficiency, recognition accuracy, and noise tolerance, thus limiting their application in conventional artificial neural networks (ANNs) and image processing.
[0003] ANNs require simulations of memory non-volatility, multi-resistance state modulation characteristics, large dynamic range, high linearity, and symmetry in weight updates, which contribute to improved computational accuracy. Synapses are the basic units of biological nervous systems, and neuromorphic devices that can simulate biological synaptic behavior have attracted widespread attention. Two-terminal devices, such as memristors, struggle to achieve complex biomimetic functions like data transmission and autonomous learning; therefore, three-terminal synaptic transistors based on ferroelectric and electrolyte gates are receiving increasing attention and research.
[0004] In an electrolyte-gate transistor (EGT) operating in electrochemical doping mode, ions in the electrolyte can migrate to the interface between the semiconductor and the electrolyte under an applied gate electric field and accumulate there, further doping and modulating the channel conductance in a non-volatile manner. Ferroelectric field-effect transistors (FeFETs) are based on the excellent multi-domain polarization switching capability of ferroelectric materials; that is, there is a Coulomb interaction between the polarization of charge carriers and the ferroelectric insulator in the channel, and the polarization state of the ferroelectric material can be changed using the gate voltage. In summary, the reason why these two types of transistor devices can achieve high linearity of conductance change is mainly because a slow kinetic process occurs within these devices that precisely and gradually adjusts the carrier concentration in the channel. In other words, to achieve high linearity of electron writing, synaptic transistor devices need to be able to achieve a slow kinetic process under voltage modulation.
[0005] Nitrogen oxide radicals, characterized by an unpaired electron in their outer shell, can undergo reversible redox reactions by gaining or losing this electron, enabling them to act as fundamental carriers of charge and energy. Nitrogen oxide radical materials have wide applications in electrolyte-containing devices such as electrochemical batteries and OLEDs. However, in solid-state devices without electrolytes, the redox process involves bond breaking and formation, structural framework rearrangement, activation, and moderate delocalization of the unpaired electron at the NO center. The NO bond is considered to possess partial π-bond characteristics and plays a dominant role in electron transfer. Based on this redox property of nitrile oxide radical materials, slow kinetic processes under voltage modulation can be achieved. This means that using such materials to construct synaptic transistor devices could potentially enable precise control of channel conductance, leading to highly linear electron writing, multi-level switching characteristics, and ultimately, simulation of synaptic plasticity. Summary of the Invention
[0006] The purpose of this invention is to provide a synaptic transistor device based on nitric oxide radical small molecules, its fabrication and application. Based on the redox properties of nitric oxide radical small molecule materials, a slow kinetic process under voltage modulation can be achieved, thereby realizing high linearity electronic writing, which can be used for synaptic plasticity function simulation.
[0007] The technical solution of the present invention is as follows: a synaptic transistor device based on nitric oxide radical small molecules, comprising a gate electrode, a gate insulating layer, a P-type semiconductor layer and source / drain electrodes arranged in sequence, wherein a charge trapping layer is provided between the gate insulating layer and the P-type semiconductor layer, and the charge trapping layer is prepared from a nitric oxide radical small molecule material.
[0008] Furthermore, the nitrogen oxide radical small molecule material is 3-[2-(2-iodoacetamido)acetamido](PROXYL), 2,2,6,6-tetramethylpiperidine oxide (TEMPO), nitrogen oxide radical piperidinol, or phenoxy radical.
[0009] Furthermore, the charge trapping layer has a thickness of 5-50 nm.
[0010] Furthermore, the P-type semiconductor layer is made of P-type organic semiconductor or P-type inorganic semiconductor material. Preferably, it can be made of pentaphenyl, bis(2,3-B:2′,3′-F)thiophene[3,2-B]thiophene (DNTT), 2,7-dioctyl[1]benzothiophene[3,2-b][1]benzothiophene (C8-BTBT), zinc selenide (ZnSe) or zinc sulfide (ZnS). The thickness of the P-type semiconductor layer is 1 to 200 nm.
[0011] Furthermore, the thickness of the source and drain electrodes is 20-200 nm, the source and drain electrodes are coplanar, and a channel structure is formed between the source and drain electrodes, wherein the ratio of the channel width W to the channel length L is 10-30, preferably 10.
[0012] Furthermore, the thickness of the gate insulating layer is 5–300 nm.
[0013] The fabrication method of the above-mentioned synaptic transistor device based on nitrile oxide radical small molecules is as follows:
[0014] 1) Obtain a charge-trapping layer solution by dissolving nitric oxide radical small molecule materials in an organic solvent;
[0015] 2) The substrate with the gate electrode and the gate insulating layer is pretreated. The gate electrode can be any one of conductive metals, oxides and nitrides such as Al, Au, Pt, ITO, TaN, highly doped silicon or graphene. The gate insulating layer covers the entire surface of the gate electrode, isolating the contact between the gate electrode and the charge trapping layer, which can effectively reduce the gate leakage current. The material used for the gate insulating layer can be dielectric materials such as alumina, silicon dioxide, hafnium oxide, polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVDF) and its derivatives.
[0016] 3) Charge trapping layer films are prepared on pretreated substrates using physical or chemical methods. Specifically, solution methods such as spin-coating, sol-gel, spray, silk-screen printing, and inkjet printing, or techniques such as thermal evaporation, magnetron sputtering, electron beam evaporation, and atomic layer deposition (ALD) can be used.
[0017] 4) P-type semiconductor layers are prepared on charge trapping layer films by physical or chemical methods. Specifically, solution methods such as spin-coating, sol-gel, spray, silk-screen printing, and inkjet printing, or techniques such as thermal evaporation, magnetron sputtering, electron beam evaporation, and atomic layer deposition (ALD) can be used.
[0018] 5) Source and drain electrodes are fabricated on the P-type semiconductor layer by physical or chemical deposition methods. The source and drain electrode materials can be any one of conductive metals, oxides and nitrides such as Al, Au, Pt, ITO, TaN, highly doped silicon or graphene. Specifically, they can be fabricated by thermal evaporation, magnetron sputtering, electron beam evaporation or atomic layer deposition (ALD).
[0019] Further, in step 1), the organic solvent is 1,2-dichloroethane, toluene, or chlorobenzene, and the concentration of the charge trapping layer solution is 0.1 mg / mL to 10 mg / mL. Preferably, toluene is the organic solvent used to prepare the charge trapping layer solution.
[0020] Furthermore, in step 3), the charge trapping layer film is prepared by spin coating at a speed of 500-6000 rpm.
[0021] The above-mentioned method for controlling the synaptic transistor device based on nitrile and oxygen radical small molecules is as follows: set the device current level at 10 -12 A~10 -3 Within the range of A, the device is used as the initial state, and a linear change process is achieved by applying a fixed voltage.
[0022] The synaptic transistor device based on nitroxide radical small molecules fabricated in this application can simulate biological synaptic processes and effectively regulate excitation and inhibition plasticity. To simulate synaptic function, the transistor uses an external input signal as stimulation, with the gate electrode acting as the synaptic front end and the channel and source / drain electrodes playing the roles of the synaptic back end. By real-time adjustment of the source / drain current levels, signal transmission is regulated, which is equivalent to simulating the weighting process in a synapse. The transistor exhibits performance characteristics similar to biological synapses, allowing the use of a fixed voltage to simulate the excitation and inhibition functions of biological synapses. Therefore, this synaptic transistor can be used for biological synapse simulation and can assist in information processing and storage in the field of artificial intelligence.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] 1. This application uses nitrile radical materials as the charge trapping layer of synaptic transistor devices. Based on the redox properties of such materials, a slow dynamic process under voltage modulation can be realized. The slow oxidation dynamic process under voltage modulation can be used to achieve fine control of channel conductivity, thereby realizing high linearity of electronic writing at the device level and achieving the characteristic of linearly increasing electronic storage window, which provides the possibility for high-precision neuromorphic computing.
[0025] 2. Unlike traditional synaptic transistor devices based on P-type organic semiconductors, which have difficulty achieving forward voltage writing in the absence of light, the synaptic transistor device based on nitrile radical small molecules disclosed in this application can achieve fine control of channel conductivity by utilizing the kinetic process of slow oxidation under the absence of light, thereby achieving high linearity writing.
[0026] 3. The synaptic transistor device based on nitric oxide radical small molecules provided in this application has high linear writing capability, so it is expected to be applied to network frameworks for self-learning, information processing, environmental perception, computing and storage. Using electronic devices to simulate biological synapses is crucial for the development of artificial intelligence. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of a synaptic transistor device fabricated based on nitric oxide radical small molecules; wherein, 1-gate electrode, 2-gate insulating layer, 3-charge trapping layer, 4-P-type semiconductor layer, 5-source drain electrode;
[0028] Figure 2 The continuous current-voltage hysteresis curves were obtained by applying a scanning voltage to the synaptic transistor device based on nitrile radical small molecules prepared in Example 1.
[0029] Figure 3 The PSC curves are obtained by applying different pulse durations to the synaptic transistor device based on nitrile radical small molecules obtained in Example 1 under a fixed pulse.
[0030] Figure 4 It is a long-term enhancement / suppression (LTP-LTD) method that applies positive and negative voltage modulation to the synaptic transistor device based on nitrile radical small molecules obtained in Example 1.
[0031] Figure 5 This is a local diagram showing the linear increase of the LTP stage in the synaptic transistor device based on nitrile radical small molecules obtained in Example 1;
[0032] Figure 6 This is the hysteresis curve of the synaptic transistor device prepared in Example 2 under dark conditions;
[0033] Figure 7 The hysteresis curve of the synaptic transistor device prepared in Comparative Example 1 under dark conditions;
[0034] Figure 8 The curves are multi-pulse curves obtained by applying a fixed voltage modulation to the synaptic transistor devices prepared in Example 1, Example 2, and Comparative Example 1. Detailed Implementation
[0035] The technical solution of the present invention will be further described below with reference to the accompanying drawings, but it is not limited thereto. Any modifications or equivalent substitutions to the technical solution of the present invention that do not depart from the spirit and scope of the technical solution of the present invention should be covered within the protection scope of the present invention.
[0036] The synaptic transistor device fabricated in this application is designed through a layer-by-layer stacking method. The device includes a five-layer structure, which, from bottom to top, consists of a substrate, a gate electrode, a gate insulating layer, a charge trapping layer, a P-type semiconductor layer, and source / drain electrodes. Figure 1 In the fabrication process, a charge trapping layer is first prepared on the gate electrode and the gate insulating layer material. The charge trapping layer material is a nitric oxide free radical small molecule material. Then, a P-type semiconductor layer is prepared on the charge trapping layer. Finally, the source and drain electrodes are prepared on the P-type semiconductor layer.
[0037] Transistors are commonly used to simulate synaptic function, where the gate electrode acts as the synaptic front end, and the channel and source / drain electrodes act as the synaptic back end. By applying a stimulus to the gate electrode, the transistor's operating current acts as the synaptic weight for signal transmission. In other words, transistors can simulate the excitation and inhibition processes of biological synapses.
[0038] Sources of raw materials and reagents used in the examples: Charge trapping layer material was purchased from Sigma Aldrich; P-type semiconductor was purchased from J&K Scientific. Substrates with gate electrodes and gate insulating layers were purchased from Aladdin and used without further purification.
[0039] Example 1: Fabrication of a synaptic transistor device with 2,2,6,6-tetramethylpiperidine oxide (TEMPO) as the charge trapping layer
[0040] I. Environmental Conditions
[0041] In actual preparation, the laboratory temperature is maintained at 10-30℃ and the indoor humidity is maintained at 20-60%.
[0042] II. Substrate Pretreatment
[0043] (1) Cleaning the substrate with gate electrode and gate insulating layer: Clean the substrate with acetone, ethanol and deionized water respectively, and put the substrate into an ultrasonic cleaner with a frequency of 100kHz and a power of 50-90% and ultrasonically vibrate at 0-20℃ for 5-20 minutes.
[0044] (2) After cleaning, use a nitrogen gun to dry the substrate until the surface is dry;
[0045] (3) Place the substrate dried with a nitrogen gun into a drying oven and dry it at 90°C for 60 minutes.
[0046] (4) Place the dried substrate into an ultraviolet ozone cleaner and clean it for 10 minutes.
[0047] III. Preparation of Charge Trapping Layer
[0048] (1) Preparation of charge trapping layer by solution spin coating: Prepare a charge trapping layer solution with 2,2,6,6-tetramethylpiperidine oxide as solute and toluene as solvent, so that the concentration of the prepared solution is 2 mg / mL, and prepare a thin film with a thickness of 20 nm on the gate insulating layer by spin coating at a speed of 4000 rpm.
[0049] (2) After spin coating, annealing is performed on a heating platform, and the temperature is maintained at 120°C for 20 minutes to prepare a charge trapping layer film.
[0050] IV. Fabrication of P-type semiconductor layer
[0051] (1) A P-type semiconductor thin film was prepared by vacuum evaporation as a semiconductor conductive channel;
[0052] (2) Place the thin film prepared in step three into a vacuum evaporation coating equipment, add pentabenzene, and control the vacuum degree at 5×10⁻⁶. -4 pa, to obtain a P-type semiconductor thin film with a thickness of approximately 50 nm;
[0053] (3) Under the premise of maintaining the original vacuum pressure, the P-type semiconductor thin film is annealed for 30 minutes;
[0054] (4) Remove the substrate from the vacuum evaporation coating equipment.
[0055] V. Fabrication of source and drain electrodes
[0056] (1) Place the material obtained in step four into a vacuum evaporation coating equipment, using copper as the metal source;
[0057] (2) Control the vacuum degree of the vacuum evaporation equipment at 5×10 -4 Pa, using a strip pattern mask (the channel width of the mask is W = 1500 μm and the length is L = 150 μm), a copper electrode with a thickness of 80 nm is obtained by evaporating a metal source;
[0058] (3) Under the premise of maintaining the original vacuum pressure, the top electrode film is annealed for 20 minutes;
[0059] (4) Remove the substrate from the vacuum evaporation coating equipment to obtain a synaptic transistor based on nitrogen and oxygen free radical small molecules.
[0060] Relevant performance verification
[0061] 1) Apply scanning voltages of ±10V, ±20V, ±30V, and ±40V to the device to perform hysteresis scanning and obtain the hysteresis curve of the device;
[0062] 2) By applying a voltage of approximately -25V to the fabricated device, a current level of approximately 10 is achieved. -8 The initial state around A;
[0063] 3) After the device is adjusted to the initial state, test the synaptic plasticity: apply an electric current in the same direction for 0.2s to 10s to the device to achieve synaptic plasticity;
[0064] 4) After the device is adjusted to the initial state, test the reconfigurability: apply voltages of opposite polarities (10V and -15V) to obtain the device's LTP / LTD cycle.
[0065] See the verification test results. Figure 2-4 .
[0066] Figure 2 The figure shows the hysteresis curve of the synaptic transistor device prepared in Example 1 under dark conditions. As can be seen from the figure, the memory window of the device increases with the change of the scan range.
[0067] Figure 3 PSC curves of different pulse widths were obtained by applying a fixed voltage pulse to the synaptic transistor device prepared in Example 1. It can be seen that at the beginning, as the pulse time increases, the current level of the device gradually increases relative to the initial state current level.
[0068] Figure 4 The LTP / LTD applied to the synaptic transistor device prepared in Example 1 with positive and negative voltage modulation showed that the device has good reconfigurability.
[0069] Figure 5 This is a partial diagram showing the linear increase in the LTP stage of the synaptic transistor device prepared in Example 1. It can be seen that under continuous stimulation with the same voltage, the current increase ΔI generated by each stimulation is the same, confirming the fact of linear writing.
[0070] In summary, the synaptic transistor device prepared in Example 1 can achieve linear write-controlled synaptic characteristics, enabling large-capacity charge storage.
[0071] Example 2: Fabrication of a synaptic transistor device using nitroxide free radical piperidinol as the charge trapping layer material I. Environmental conditions
[0072] In actual preparation, the laboratory temperature is maintained at 10-30℃ and the indoor humidity is maintained at 20%-60%.
[0073] II. Substrate Pretreatment
[0074] (1) Cleaning the substrate with gate electrode and gate insulating layer: Clean the substrate with acetone, ethanol and deionized water respectively, and put the substrate into an ultrasonic cleaner with a frequency of 100kHz and a power of 50-90% and ultrasonically vibrate at 0-20℃ for 5-20 minutes.
[0075] (2) After cleaning, use a nitrogen gun to dry the substrate until the surface is dry;
[0076] (3) Place the substrate dried with a nitrogen gun into a drying oven and dry it at 90°C for 60 minutes.
[0077] (4) Place the dried substrate into an ultraviolet ozone cleaner and clean it for 10 minutes.
[0078] III. Preparation of Charge Trapping Layer
[0079] (1) Charge trapping layer is prepared by solution spin coating: a charge trapping layer solution is prepared with nitric oxide free radical piperidinol as solute and toluene as solvent, so that the concentration of the prepared solution is 2 mg / mL. A thin film with a thickness of 20 nm is prepared on the gate insulating layer by spin coating at a speed of 4000 rpm.
[0080] (2) After spin coating, annealing is performed on a heating platform, and the temperature is maintained at 120°C for 20 minutes to prepare a charge trapping layer film.
[0081] IV. Fabrication of P-type semiconductor layer
[0082] (1) A P-type semiconductor thin film was prepared by vacuum evaporation as a semiconductor conductive channel;
[0083] (2) Place the thin film prepared in step three into a vacuum evaporation coating equipment, add pentabenzene, and control the vacuum degree to 5×10. -4 pa, to obtain a P-type semiconductor thin film with a thickness of approximately 50 nm;
[0084] (3) Under the premise of maintaining the original vacuum pressure, the P-type semiconductor thin film is annealed for 30 minutes;
[0085] (4) Remove the substrate from the vacuum evaporation coating equipment.
[0086] V. Fabrication of source and drain electrodes
[0087] (1) Place the material obtained in step four into a vacuum evaporation coating equipment, using copper as the metal source;
[0088] (2) Control the vacuum degree of the vacuum evaporation equipment at 5×10 -4Pa, using a strip pattern mask (the channel width of the mask is W = 1500 μm and the length is L = 150 μm), a copper electrode with a thickness of 80 nm is obtained by evaporating a metal source;
[0089] (3) Under the premise of maintaining the original vacuum pressure, the top electrode film is annealed for 20 minutes;
[0090] (4) Remove the substrate from the vacuum evaporation coating equipment to obtain a synaptic transistor based on nitrogen and oxygen free radical small molecules.
[0091] Relevant performance verification
[0092] 1) Apply scanning voltages of ±10V, ±20V, ±30V, and ±40V to the device to perform hysteresis scanning and obtain the hysteresis curve of the device;
[0093] 2) After the device is adjusted to the initial state, test the linear change of the conductance: apply a certain voltage (10V, 0.5s) and obtain the linear change of the device conductance;
[0094] Figure 6 The figure shows the hysteresis curve of the synaptic transistor device prepared in Example 2 under dark conditions. As can be seen from the figure, the memory window of the device increases with the change of the scan range.
[0095] Comparative Example 1
[0096] This comparative example uses tetramethylpiperidinol, which has a similar structure to TEMPO but does not contain nitric oxide radicals, as the charge trapping layer material. Except for the preparation process of the charge trapping layer described in step three, the preparation methods of the other structural layers are the same as in Example 2.
[0097] I. Environmental conditions are the same as in Example 2.
[0098] 2. The pretreatment of the substrate is the same as in Example 2.
[0099] III. Preparation of Charge Trapping Layer
[0100] (1) Charge trapping layer is prepared by solution spin coating: a charge trapping layer solution is prepared with tetramethylpiperidinol as solute and toluene as solvent, so that the concentration of the prepared solution is 2 mg / mL. A thin film with a thickness of 20 nm is prepared on the gate insulating layer by spin coating at a speed of 4000 rpm.
[0101] (2) After spin coating, annealing is performed on a heating platform, and the temperature is maintained at 120°C for 20 minutes to prepare a charge trapping layer film.
[0102] IV. Preparation of the P-type semiconductor layer is the same as in Example 2.
[0103] V. The preparation of source and drain electrodes is the same as in Example 2.
[0104] Figure 7 The figure shows the hysteresis curve of the synaptic transistor device prepared in Comparative Example 1 under dark conditions. As can be seen from the figure, the memory window of the device increases with the change of the scan range.
[0105] Figure 8 The multi-pulse curves of the synaptic transistor devices prepared in Example 1, Example 2, and Comparative Example 1 were obtained by applying a fixed voltage modulation. The device prepared with TEMPO as the charge trapping layer had the best performance, followed by the device prepared with nitroxide radical piperidinol as the charge trapping layer. The device prepared with tetramethylpiperidinol without nitroxide radicals had the worst performance, which shows that the device prepared with nitroxide radicals as the charge trapping layer has high linearity writing characteristics.
[0106] In summary, synaptic transistor devices containing nitrogen and oxygen radicals can achieve linear write-controlled synaptic characteristics, enabling large-capacity charge storage.
[0107] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A synaptic transistor device based on nitrile-oxygen radical small molecules, comprising a gate electrode, a gate insulating layer, a p-type semiconductor layer, and source / drain electrodes arranged sequentially, characterized in that, A charge trapping layer is provided between the gate insulating layer and the P-type semiconductor layer, and the charge trapping layer is prepared from a nitrile radical small molecule material; The nitroxide radical small molecule material is 3-[2-(2-iodoacetamido)acetamido], 2,2,6,6-tetramethylpiperidine oxide, or nitroxide radical piperidinol.
2. The synaptic transistor device based on nitrile-oxygen free radical small molecules as described in claim 1, characterized in that, The charge trapping layer has a thickness of 5-50 nm.
3. The synaptic transistor device based on nitrile-oxygen free radical small molecules as described in claim 1, characterized in that, The P-type semiconductor layer is made of P-type organic semiconductor or P-type inorganic semiconductor material, and the thickness of the P-type semiconductor layer is 1~200 nm.
4. The synaptic transistor device based on nitrile-oxygen free radical small molecules as described in claim 1, characterized in that, The thickness of the source and drain electrodes is 20~200 nm. The source and drain electrodes are arranged in the same plane, and a channel structure is formed between the source and drain electrodes. The ratio of the channel width W to the channel length L is 10~30.
5. The synaptic transistor device based on nitrile-oxygen free radical small molecules as described in claim 1, characterized in that, The thickness of the gate insulating layer is 5~300 nm.
6. The method for fabricating a synaptic transistor device based on nitrile-oxygen radical small molecules as described in any one of claims 1-5, characterized in that, Includes the following steps: 1) Obtain a charge-trapping layer solution by dissolving nitric oxide radical small molecule materials in an organic solvent; 2) Pre-treat the substrate with the gate electrode and gate insulating layer; 3) Prepare a charge trapping layer thin film on a pretreated substrate using physical or chemical methods; 4) Prepare a P-type semiconductor layer on the charge trapping layer thin film using physical or chemical methods; 5) Source and drain electrodes are fabricated on a P-type semiconductor layer by physical or chemical deposition methods.
7. The method for fabricating a synaptic transistor device based on nitrile oxide free radical small molecules as described in claim 6, characterized in that, In step 1), the organic solvent is 1,2-dichloroethane, toluene, or chlorobenzene, and the concentration of the charge trapping layer solution is 0.1 mg / mL to 10 mg / mL.
8. The method for fabricating a synaptic transistor device based on nitrile oxide free radical small molecules as described in claim 6, characterized in that, In step 3), the charge trapping layer film is prepared by spin coating at a speed of 500-6000 rpm.
9. The linear variation control method for synaptic transistor devices based on nitrile-oxygen free radical small molecules as described in any one of claims 1-5, characterized in that, Set the device current level to 10. -12 A~10 -3 Within the range of A, the device is used as the initial state, and a linear change process is achieved by applying a fixed voltage.
Citation Information
Patent Citations
Laminated charge trapping type synaptic transistor and preparation method thereof
CN113871527A