Method for producing paper and board
By directly injecting water-soluble polymers in the form of an inverse emulsion reacted in a mixture of alkali metal hydroxides and hypohalides into fiber suspensions, the complexities of polymer solution transport and heating reactions are solved, improving the drainage and dry strength properties of paper or paperboard and simplifying the production process.
Patent Information
- Application Number
- CN202280028578.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-15
- Filing Date
- 2022-04-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-04-13
AI Technical Summary
In the existing technology, the equipment for transporting and dissolving polymer solutions occupies a large area, and the reaction requires heating and temperature control, which makes the process of producing paper or paperboard complicated and inconvenient.
A water-soluble polymer in the form of a reverse emulsion reacts in a mixture of alkali metal hydroxide and hypohalides, and is then directly injected into a fiber suspension, avoiding the material flow scheme and heated reaction medium required in aqueous solution treatment, thus simplifying the operation.
It improves the drainage and dry strength properties of paper or paperboard, expands the application range of polymers, simplifies the production process, and reduces equipment requirements.
Smart Images

Figure BDA0004492953480000111 
Figure BDA0004492953480000112
Abstract
Description
Technical Field
[0001] This invention relates to a method for producing paper or paperboard with improved drainage and processability. More specifically, this invention relates to a method involving the reaction of a water-soluble polymer in the form of a reverse emulsion in a mixture of alkali metal hydroxides and / or alkaline earth metal hydroxides and alkali metal hypohalides and / or alkaline earth metal hypohalides, which is then directly injected into a fiber suspension for the production of paper or paperboard.
[0002] The present invention also relates to paper and paperboard with improved physical properties obtained by this method. Background Technology
[0003] The paper industry has been seeking to optimize its paper or paperboard production methods, particularly in terms of output, productivity, cost reduction, and finished product quality.
[0004] The uses of polymers as dry strength agents, drainage agents, and machinability agents have been described very extensively.
[0005] Drainage performance refers to the ability of the fiber mat to remove or drain the maximum amount of water before the drying section. Improved drainage performance translates to energy savings and increased production capacity.
[0006] Processability refers to optimizing the operation of a paper machine by improving productivity through better drainage on the table, better drying in the press section, reducing breakage through greater loop cleanliness, and reducing deposits.
[0007] JP 2002-212898 describes the use of polymers obtained via Hoffmann degradation reactions in papermaking processes. This document does not describe the addition of polymers in reverse emulsion form during the chemical reaction process.
[0008] WO 2020 / 094960 describes inverse emulsion compositions. EP 2 840 100 Functionalization of polymers.
[0009] Polyvinylamine is known to improve drainage in the papermaking process.
[0010] Polyvinylamine can be obtained by reacting polyacrylamide in a solution of alkali metal hydroxide and / or alkaline earth metal hydroxide and alkali metal hypohalides and / or alkaline earth metal hypohalides, followed by treatment in an acidic medium.
[0011] When the reaction is carried out directly before the product is injected into the fiber suspension to obtain paper or paperboard, only the polyacrylamide in solution reacts with the alkali metal or alkaline earth metal hydroxide and the hypohalides.
[0012] However, this need for polyacrylamide solutions means either transporting them to paper mills or having equipment within the paper mills for dissolving the polymer. In both cases, the footprint of the polymer solution inventory or the dissolving equipment remains substantial.
[0013] Furthermore, this reaction on polyacrylamide requires heating the reaction medium and also requires an exchanger to regulate its temperature at the end of the reaction. Summary of the Invention
[0014] Unexpectedly, the applicant discovered a method involving the reaction of a water-soluble polymer in reverse emulsion form (water-in-oil) in a mixture of hydroxides (alkali metal hydroxides and / or alkaline earth metal hydroxides) and hypohalides (alkali metal hypohalides and / or alkali metal hypohalides), which is then directly injected into a fiber suspension used in the production of paper or paperboard, thereby improving drainage and dry strength properties.
[0015] This method can also avoid the entire logistics process inherent in the handling of water-soluble polymer solutions (transportation or installation of the dissolution unit).
[0016] Furthermore, the method becomes simpler because the reaction medium is homogeneous from the moment the polymer in reverse emulsion form is added to the mixture of alkali metal and / or alkaline earth metal hydroxides and hypohalides, and there is no need to heat the reaction medium or use a heat exchanger.
[0017] "Alkali" refers to an alkali metal, preferably lithium, sodium, or potassium. "Alkali metal hydroxide" refers to a hydroxide (OH) of at least one alkali metal. - For example, NaOH, KOH, or NaOH + KOH. This also applies to alkaline earth metal hydroxides.
[0018] "Alkaline earth" refers to alkaline earth metals, preferably calcium or magnesium.
[0019] Hypohalides are oxygen-containing anions, such as hypochlorite (ClO). - .
[0020] "Alkali metal hypohalides" refers to a hypohalide of at least one alkali metal and at least one hypohalide, such as NaOCl, KOBr, or NaOCl+KOBr. The same applies to alkaline earth metal hypohalides.
[0021] Finally, because the molecular weight range of water-soluble polymers in reverse emulsion form is very wide, the method of the present invention allows for an expansion of the current range of drainage agents and dry strength agents compared to similar methods using polyacrylamide in aqueous solution form.
[0022] More specifically, the present invention relates to a method for producing paper or paperboard from a fiber suspension, the method comprising the following steps:
[0023] a) Injecting polymer P2 into a fiber suspension (advantageously a suspension of cellulose fibers),
[0024] b) Forming paper or paperboard.
[0025] c) Dry the paper or cardboard.
[0026] Prior to step a), polymer P2 is prepared from a water-soluble polymer P1 in the form of a reverse emulsion, wherein P1 is a water-soluble polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
[0027] The polymer P2 is obtained by reaction Re, which comprises adding a water-soluble polymer P1 in the form of a reverse emulsion to an aqueous solution M1 of: (i) an alkali metal hydroxide or an alkaline earth metal hydroxide or a mixture thereof, and (ii) an alkali metal hypohalide or an alkaline earth metal hypohalide or a mixture thereof.
[0028] After adding the water-soluble polymer P1 in the form of a reverse emulsion, the reaction time of Re is from 10 seconds to 5 hours.
[0029] Advantageously, step a) is carried out within a time frame not exceeding 24 hours from the start of reaction Re, that is, from the addition of the water-soluble polymer P1 in the form of a reverse emulsion to the aqueous solution M1.
[0030] In the subsequent parts of the specification and in the claims, all references to "gt" are valid. -1 or kg.t -1 The polymer dosages indicated are given as the weight of the polymer per tonne of dry matter. Dry matter is a dry extract obtained after evaporation of water from a fiber suspension used in methods of producing paper or paperboard. Dry matter is typically based on cellulose fibers and fillers, and advantageously consists of cellulose fibers and fillers. The term "cellulose fiber" includes any cellulose entity, including fibers, fine fibers, microfibers, or nanofibers. Fiber suspension is understood to refer to a concentrated or diluted slurry based on water and cellulose fibers. Concentrated slurries (thick slurries) with a dry matter mass concentration typically greater than 1%, or even greater than 3%, are located upstream of a mixing pump (fan pump). Diluted slurries (thin slurries) with a dry matter mass concentration typically less than 1% are located downstream of a mixing pump.
[0031] The term "polymer" refers to homopolymers and copolymers of at least two different monomers.
[0032] Amphoteric polymers are polymers containing both cationic and anionic charges, preferably with anionic charges being equal in number to cationic charges.
[0033] As used herein, the term "water-soluble polymer" refers to a polymer that, when stirred at 25°C for 4 hours and at a concentration of 20 g / L... -1 When a polymer is dissolved in deionized water at a concentration of [amount], it produces an aqueous solution without insoluble particles.
[0034] The numerical range includes a lower limit and an upper limit. Therefore, the numerical ranges "0.1 to 1.0" and "0.1 to 1" include the values 0.1 and 1.0.
[0035] The water-soluble polymer P1 is a polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile. Preferably, polymer P1 contains at least 50 mol% of at least one of these nonionic monomers.
[0036] The polymer P1 may also contain anionic and / or cationic and / or zwitterionic monomers. Advantageously, polymer P1 does not contain nonionic monomers not selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
[0037] The anionic monomer is preferably selected from the group consisting of: monomers having a carboxylic acid functional group and their salts, including acrylic acid, methacrylic acid, itaconic acid, and maleic acid; monomers having a sulfonic acid functional group and their salts; including acrylamide tert-butyl sulfonic acid (ATBS), allyl sulfonic acid, and methyl allyl sulfonic acid and their salts; and monomers having a phosphonic acid functional group and their salts.
[0038] Typically, the anionic monomer of polymer P1 has an alkali metal, alkaline earth metal, or ammonium (preferably quaternary ammonium) as a counterion.
[0039] The cationic monomer is preferably selected from the group consisting of: quaternized or salted dimethylaminoethyl acrylate (ADAME), quaternized or salted dimethylaminoethyl methacrylate (MADAME), diallyl dimethyl ammonium chloride (DADMAC), acrylamidopropyl trimethyl ammonium chloride (APTAC), and methacrylamidopropyl trimethyl ammonium chloride (MAPTAC).
[0040] Advantageously, the cationic monomer of polymer P1 has a halide ion (preferably chloride ion) as a counterion.
[0041] The zwitterionic monomer is preferably selected from the group consisting of: sulfobetaine monomers, such as sulfopropyl dimethylammonium ethyl methacrylate, sulfopropyl dimethylammonium propyl methacrylamide, or sulfopropyl-2-vinylpyridine; phosphate betaine monomers, such as ethyltrimethylammonium phosphate ethyl methacrylate; and carboxybetaine monomers.
[0042] Preferably, the water-soluble polymer P1 is a homopolymer or copolymer of acrylamide or methacrylamide.
[0043] Polymer P1 can be linear, structured, or crosslinked. Structured crosslinking agents are particularly selected from sodium allyl sulfonate, sodium methyl allyl sulfonate, sodium methyl allyl disulfonate, methylenebisacrylamide, triallylamine, and triallyl ammonium chloride.
[0044] The structuring of polymer P1 can also be achieved using at least one polyfunctional compound containing at least three heteroatoms selected from N, S, O, and P, and each heteroatom having at least one mobile hydrogen atom. Such polyfunctional compounds can be, in particular, polyethyleneimine or polyamine.
[0045] The reaction Re is carried out by adding a reverse emulsion of the water-soluble polymer P1 to an aqueous solution M1. Preferably, the reverse emulsion (water-in-oil emulsion) comprises:
[0046] -Contains at least an aqueous phase of polymer P1,
[0047] - oil phase,
[0048] - At least one emulsifier and at least one phase reverser.
[0049] The oil phase can be mineral oil, vegetable oil, synthetic oil, or a mixture of several of these oils.
[0050] Examples of mineral oils are those containing saturated hydrocarbons of the aliphatic, cyclothenic, alkanes, isoalkanes, cycloparaffinic, or naphthyl type.
[0051] Examples of synthetic oils are hydrogenated polydecene or hydrogenated polyisobutylene, and esters such as octyl stearate or butyl oleate. (Exxon's) The product line is a perfect fit.
[0052] Typically, the weight ratio of the aqueous phase to the oil phase in a reverse emulsion is preferably between 50 / 50 and 90 / 10. This ratio includes the weights of the different components of the emulsion, particularly the water-soluble polymer P1.
[0053] The water-in-oil emulsion preferably contains 15 to 40% by weight of oil, 20 to 55% by weight of water, and 15 to 50% by weight of polymer P1, the percentages being expressed relative to the total weight of the reverse emulsion of polymer P1.
[0054] In this invention, the term "emulsifier" refers to a reagent capable of emulsifying water in oil, while "reversing agent" is a reagent capable of emulsifying oil in water. More precisely, reversing agents are considered surfactants with an HLB of 10 or greater, and emulsifiers are considered surfactants with an HLB of strictly less than 10.
[0055] The hydrophilic-lipophilic balance (HLB) of a compound is a measure of its degree of hydrophilicity or lipophilicity, determined by calculating molecular values in different regions, as described by Griffin in 1949 (Griffin, WC, Classification of Surface-Active Agents by HLB, Journal of the Society of Cosmetic Chemists, 1949, 1, pp. 311-326).
[0056] In this invention, we employ the Griffin method, which is based on the calculated values of molecular chemical groups. Griffin specifies a dimensionless number between 0 and 20 to provide solubility information in water and oil. Substances with an HLB value of 10 are distributed between the two phases, such that the hydrophilic groups (molecular weight Mh) extend completely into the water, while the hydrophobic hydrocarbon groups (molecular weight Mp) are adsorbed in the non-aqueous phase.
[0057] A substance with a total molecular weight of M has a hydrophilic portion with a molecular weight of Mh, and its HLB value is HLB = 20 (Mh / M).
[0058] The reverse emulsion containing polymer P1 advantageously contains 0.1% to 10% by weight of at least one emulsifier, the percentage being expressed by weight relative to the weight of the emulsion. The emulsifier is advantageously selected from sorbitol esters, polyethoxylated sorbitol esters, polyethoxylated fatty acids, polyethoxylated fatty alcohols, polyesters with an average molecular weight of 1000-3000 Daltons obtained by condensation of poly(isobutylene)succinic acid or its anhydride and polyethylene glycol, block copolymers with an average molecular weight of 2500-3500 Daltons obtained by condensation of hydroxystearic acid and polyethylene glycol, ethoxylated fatty amines, derivatives of dialkylolamides, copolymers of stearyl methacrylate, and mixtures of these emulsifiers.
[0059] The reversed emulsion containing polymer P1 advantageously contains 0.1 to 10% by weight of at least one reverser, the percentage being expressed as a weight relative to the emulsion weight. This reverser is advantageously selected from ethoxylated nonylphenol (preferably having 4 to 10 ethoxy groups), ethoxylated / propoxylated alcohols (preferably having ethoxy / propoxy groups containing 12 to 25 carbon atoms); ethoxylated tridecyl alcohol, polyethoxylated fatty acids, poly(ethoxylated / propoxylated) fatty alcohols; ethoxylated sorbitol esters; polyethoxylated sorbitol laurate; polyethoxylated castor oil; heptaoxyethylated lauryl alcohol. alcohol); polyethoxylated dehydrated sorbitan monostearate; polyethoxylated alkylphenol hexadecyl ether; polyethylene oxide alkyl aryl ether; N-hexadecyl-N-ethylmorpholine ethyl sulfate; sodium dodecyl sulfate; condensation products of fatty alcohols and ethylene oxide; condensation products of alkylphenols and ethylene oxide; condensation products of fatty amines and 5 molar equivalents or more of ethylene oxide; ethoxylated tristyrylphenol; condensation products of ethylene oxide and partially esterified polyols having aliphatic chains and their anhydrous forms; amine oxides; alkyl polyglycosides; glucamides; phosphate esters; alkylbenzene sulfonic acids and their salts; water-soluble surfactant polymers; and mixtures of many of these antiphase agents.
[0060] The water-in-oil emulsion according to the invention can be prepared by any method known to those skilled in the art. Typically, an aqueous solution containing monomers and emulsifiers is emulsified in an oil phase. Polymerization is then carried out by adding a free radical initiator. Reference can be made to redox pairs, with oxidants including cumene hydroperoxide, tert-butyl hydroxyperoxide, or persulfate, and reducing agents including sodium sulfite, sodium metabisulfite, and moiré salts. Azo compounds, such as hydrochlorides of 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2-amidinylpropane), can also be used.
[0061] Typically, polymerization is carried out at isothermal, adiabatic, or controlled temperatures. Thus, the temperature is advantageously kept constant, typically between 10°C and 60°C (isothermal), or the temperature is allowed to rise naturally (adiabatic), in which case the reaction typically begins at a temperature below 10°C and ends at a temperature typically above 50°C, or finally, the temperature rise is controlled so as to have a temperature profile between that of the isothermal and adiabatic profiles.
[0062] Typically, the antiphase agent is added at the end of the polymerization reaction, preferably at a temperature below 50°C.
[0063] The reaction Re involves adding a reverse emulsion of polymer P1 to an aqueous solution M1 of the following substances: (i) alkali metal hydroxides and / or alkaline earth metal hydroxides, (ii) alkali metal hypohalides and / or alkaline earth metal hypohalides, and then reacting Re for 10 seconds to 5 hours to form polymer P2.
[0064] Advantageously, the aqueous solution M1 is an aqueous solution of soda (sodium hydroxide) and sodium hypochlorite.
[0065] Advantageously, the reaction time of polymer P1 in aqueous solution M1 of hypohalide and hydroxide is from 10 seconds to 180 minutes.
[0066] The reaction Re is advantageously carried out at temperatures between 10°C and 30°C, and more advantageously between 20°C and 25°C.
[0067] Preferably, for reaction Re, the coefficient α = (moles of alkali metal and / or alkaline earth metal) hypohalides / (moles of nonionic monomers of polymer P1, such as acrylamide, methacrylamide, N,N-dimethylacrylamide, acrylonitrile or mixtures thereof) is 0.1 to 1.0, and the coefficient β = (moles of alkali metal and / or alkaline earth metal) hydroxides / (moles of alkali metal and / or alkaline earth metal) hypohalides is 0.5 to 4.0.
[0068] For reaction Re, polymer P1 is preferably added to aqueous solution M1 in an amount of 0.1 to 20% by weight, more preferably 0.3 to 10% by weight, and even more preferably 0.5 to 3.0% by weight, relative to the weight of aqueous solution M1.
[0069] Advantageously, at the end of reaction Re and before its injection into the fiber suspension, polymer P2 can be functionalized with a compound containing at least one aldehyde functional group to produce polymer P3, for example by adding a compound containing at least one aldehyde functional group. Preferably, the compound containing at least one aldehyde functional group is glyoxal.
[0070] Preferably, before injecting the fiber suspension, the pH of the reaction mixture containing polymer P2 obtained from reaction Re can be adjusted to 0.5 to 7.5, more preferably 1.0 to 3.0, by adding acid. Those skilled in the art know how to adjust the pH of this type of reaction medium. pH adjustment is advantageously carried out without the formation of polymer P3.
[0071] According to a preferred embodiment, after homogenizing the fiber suspension in a dilution pump (fan pump), polymer P2 (or P3) is introduced into white water and / or slurry and / or a mixture formed by white water and slurry.
[0072] Advantageously, polymer P2 (or P3) can also be introduced in the papermaking process at the forming wire, for example by spraying or applying in the form of foam, or at the sizing machine (coating machine).
[0073] Advantageously, 0.1 to 10 kg.t is added to the fiber suspension. -1 Preferably, the dosage is 0.2 to 5.0 kg / t. -1 The polymer P2 (or P3).
[0074] Fiber suspensions may include various cellulose fibers that can be used: virgin fibers, regenerated fibers, chemical pulps, mechanical pulps, microfibrillated cellulose, or nanofibrillated cellulose. Fiber suspensions also include the use of these different cellulose fibers and all types of fillers, such as TiO2, CaCO3 (crushed or precipitated), kaolin, organic fillers, and mixtures thereof.
[0075] Polymer P2 or P3 can be combined with other products for use in papermaking processes, such as inorganic or organic coagulants, dry strength agents, wet strength agents, natural polymers such as starch or carboxymethyl cellulose (CMC), inorganic microparticles such as bentonite microparticles and colloidal silica microparticles, and organic polymers of any ionic type (nonionic, cationic, anionic, or amphoteric) and which may be (but are not limited to) linear, branched, crosslinked, hydrophobic, or associated.
[0076] The following examples illustrate the present invention, but do not limit its scope. Detailed Implementation
[0077] Programs used for application testing:
[0078] a) Type of slurry used
[0079] Recycled fiber pulp: Wet pulp is obtained by disintegrating the dry pulp to achieve a final water concentration of 1% by weight. This is a neutral pH pulp composed of 100% recycled paperboard fibers.
[0080] b) Drainage performance assessment (DDA)
[0081] The DDA ("Dynamic Drainage Analyzer") automatically measures the time (in seconds) required for vacuum removal of fiber suspension deposited on fabric. The polymer is added to the wet slurry (0.6 L of 1.0 wt% slurry) in the DDA cylinder under stirring at 1000 rpm.
[0082] -T=0s: Stirring slurry
[0083] -T = 20s: Add polymer
[0084] -T=30s: Stop stirring and apply at 200mbar (1bar=10mbar). 5 Vacuum drainage for 70 seconds under pressure (Pa).
[0085] The pressure under the fabric is recorded as a function of time. When all water has been removed from the fiber pad, air passes through the pad, causing a sudden change in the slope of the curve representing the pressure under the fabric as a function of time. The time (in seconds) recorded at the point of this slope change corresponds to the drainage time. The shorter the time, the better the vacuum drainage effect.
[0086] c) Performance under DSR (dry strength) application, basis weight 90 g.m - 2
[0087] Collect the required amount of slurry to obtain a weight of 90g.m -2 Paper (sheet).
[0088] Wet slurry is introduced into the barrel of the dynamic paper forming machine and agitation is maintained. Various components of the system are then injected into the slurry in a predetermined sequence. Typically, the contact time between each polymer addition is 30 to 45 seconds.
[0089] The paper forming machine employs an automatic dynamic paper forming process: absorbent paper and forming fabric are placed in the rollers of the dynamic paper forming machine, and then the rollers begin to rotate at 1000 rpm, forming a water wall. The treated pulp is spread on the water wall to form a fiber mat on the forming fabric.
[0090] Once the water is drained, the fiber pad is recycled, pressed at an output pressure of 4 bar, and then dried at 117°C. The resulting paper is left overnight in a room with controlled humidity and temperature (50% relative humidity and 23°C). The dry strength properties of all paper obtained through this process are then measured.
[0091] Bursting strength (bursting index) was measured using a Messier Buchel M 405 bursting strength tester according to standard TAPPI T403 om-02. Results are expressed in kPa or as a percentage of a reference value. (kPa·m) 2 The burst strength index, expressed as / g, is determined by dividing this value by the gram weight of the paper being tested.
[0092] According to standard TAPPI T494 om-01, the breaking length was measured in the longitudinal (machine direction) (DBL SM) and transverse (DBL ST) directions using a test AX traction device. The results are expressed in km or as a percentage of a reference value.
[0093] Test products in application testing:
[0094] Polymer P1
[0095] Synthesis of polymer P1-A
[0096] 310 g of water was introduced into a 1-liter reactor equipped with a mechanical stirrer, thermometer, condenser, and nitrogen immersion rod. The pH of the reaction medium was adjusted to 3.3 using a pH buffer solution (30% by weight NaOH aqueous solution and 75% by weight H3PO4 aqueous solution). The medium was heated using a water bath and maintained at a temperature of 79 to 81 °C. In two consecutive liquid pours, 400 g of 50% acrylamide, 237.8 g of water, and 2.40 g of 100% sodium hypophosphite (liquid pour 1) were added over 180 minutes. In liquid pour 2, 0.48 g of 100% sodium persulfate and 48 g of water were added over 180 minutes. After the liquid pours were completed, the polymer solution was incubated at 80 °C for 120 minutes.
[0097] The resulting polymer P1-A solution had a pH of 5.7, a weight concentration of 20%, and a viscosity of 6000 cps.
[0098] Polymer P1-B: Acrylamide homopolymer in reverse emulsion form is sold by SNF under the trade name: Flopam TM EM230.
[0099] Polymers P1-A (aqueous solution) and P1-B (reverse emulsion) are both homopolymers of acrylamide, and their only difference is their physical form.
[0100] Polymer P2
[0101] Synthesis of polymer P2-A
[0102] A 10% by weight P1-A aqueous solution was prepared by diluting 20g of a 20% by weight P1-A aqueous solution with 20g of water. The polymer solution was then heated to 50°C.
[0103] Based on the reaction coefficients α (0.5) and β (2.0), an aqueous solution of 14.29 g of 14.6% (by weight in water) sodium hypochlorite (NaOCl) and 7.5 g of 30% (by weight in water) soda ash was prepared. The aqueous solution of sodium hypochlorite and soda ash was added to the polymer P1-A solution while it was at 50°C. After reacting for 30 seconds, 138.20 g of water was added. A solution of polymer P2-A with a concentration of 2% by weight was obtained.
[0104] Synthesis of polymer P2-B
[0105] Based on the coefficients α (0.5) and β (2.0) of the reaction Re, an aqueous solution M1 of 3.66 g of 14.6% (by weight in water) sodium hypochlorite (NaOCl) and 1.92 g of 30% (by weight in water) soda ash was prepared. Then 93.60 g of water was added.
[0106] Under ambient temperature and stirring, 3.20 g of polymer P1-B (reverse emulsion) was added to aqueous solution M1. The polymer was stirred in solution M1 for 60 minutes. A solution of polymer P2-B was obtained, with a final polymer weight concentration of 1%.
[0107] Application testing
[0108] Drainage performance (DDA)
[0109]
[0110] Table 1: Drainage as a polymer function
[0111] An improvement in drainage was observed when using polymer P2-B compared to polymer P2-A.
[0112] Performance in DSR (Dry Strength) Applications
[0113]
[0114] Table 2: Dry strength as a polymer function
[0115] The bursting resistance was improved by using polymer P2-B. The same trend was observed in the fracture length measurements in both the longitudinal (DBL SM) and transverse (DBL ST) directions.
Claims
1. A method for producing paper or paperboard from a fiber suspension, comprising the following steps: a) Inject polymer P2 into the fiber suspension. b) Forming paper or paperboard, c) Dry the paper or cardboard. Prior to step a), polymer P2 is prepared from a water-soluble polymer P1 in the form of a reverse emulsion, wherein P1 is a water-soluble polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile. The polymer P2 is obtained by reaction Re, which comprises adding a water-soluble polymer P1 in the form of a reverse emulsion to an aqueous solution M1 of: (i) an alkali metal hydroxide or an alkaline earth metal hydroxide or a mixture thereof, and (ii) an alkali metal hypohalide or an alkaline earth metal hypohalide or a mixture thereof. After adding the water-soluble polymer P1 in the form of a reverse emulsion, the reaction time of Re is from 10 seconds to 5 hours.
2. The method according to claim 1, characterized in that... The polymer P1 contains at least 50 mol% of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide and acrylonitrile.
3. The method according to claim 1 or 2, characterized in that... The polymer P1 is a homopolymer or copolymer of acrylamide or methacrylamide.
4. The method according to claim 1 or 2, characterized in that, The reverse emulsion comprises: - Contains at least an aqueous phase of polymer P1. - oil phase, - At least one emulsifier and at least one phase reverser.
5. The method according to claim 4, characterized in that... The reverse emulsion of polymer P1 contains 15 to 40% by weight of oil, 20 to 55% by weight of water, and 15 to 50% by weight of polymer, the percentages being expressed relative to the total weight of the reverse emulsion of polymer P1.
6. The method according to claim 1 or 2, characterized in that... For reaction Re, the coefficient α = moles of hypohalide / moles of nonionic monomer of water-soluble polymer P1 is 0.1 to 1.0, and the coefficient β = moles of hydroxide / moles of hypohalide is 0.5 to 4.
0.
7. The method according to claim 1 or 2, characterized in that... 0.1 to 20% by weight of polymer P1 is added to aqueous solution M1 relative to the weight of aqueous solution M1.
8. The method according to claim 1 or 2, characterized in that... At the end of reaction Re, and before the fiber suspension is injected, polymer P2 is functionalized with a compound containing at least one aldehyde functional group to produce polymer P3.
9. The method according to claim 8, characterized in that... A compound containing at least one aldehyde functional group is glyoxal.
10. The method according to claim 1 or 2, characterized in that... Before being injected into the fiber suspension, the pH of the reaction mixture containing polymer P2 obtained from the reaction Re is adjusted to between 0.5 and 7.5 by adding acid.
11. The method according to claim 1 or 2, characterized in that... After homogenizing the fiber suspension in a dilution pump, polymer P2 is introduced into white water and / or slurry and / or a mixture formed from white water and slurry.
12. The method according to claim 1 or 2, characterized in that... Step a) is carried out within 24 hours from the time the water-soluble polymer P1 in the form of a reverse emulsion is added to the aqueous solution M1.
13. The method according to claim 1 or 2, characterized in that... The aqueous solution M1 is an aqueous solution of sodium hydroxide and sodium hypochlorite.
14. The method according to claim 1 or 2, characterized in that The reaction Re is carried out at a temperature of 10 to 30°C.
15. The method according to claim 1 or 2, characterized in that... Add 0.3 to 10% by weight of polymer P1 to aqueous solution M1 relative to the weight of aqueous solution M1.
Citation Information
Patent Citations
Novel polymeric hydrosuluble complexes and their use
EP2840100A1
Auto-invertible inverse polymer emulsion
WO2020094960A1
Method for freeness improvement
JP2002212898A
Internal additive for papermaking and method for using the same