Thin film resistor (TFR) module

By employing high-density plasma ridge removal technology and annealing, the problems of large temperature coefficient of resistance variation and numerous mask layers in TFR modules have been solved, enabling the manufacturing of TFR modules with low temperature coefficient of resistance and fewer mask layers, thereby improving resistance stability and manufacturing efficiency.

CN117204145BActive Publication Date: 2026-11-20MICROCHIP TECHNOLOGY INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280025003.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-01-14
Publication Date
2026-11-20
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Existing TFR modules exhibit high resistance variation and temperature sensitivity, and require multiple mask layers during manufacturing, making it difficult to meet the requirements of integrated circuits for low resistance temperature coefficients and low mask layer counts.

Method used

The vertical ridges of the TFR element are removed or shortened using a high-density plasma (HDP) ridge removal process, combined with annealing, to form a cup-shaped structure with a laterally extended TFR element substrate and sloping sidewalls, reducing the vertical height. The fabrication is carried out using a single mask layer inlay method.

Benefits of technology

This study improves the temperature coefficient of resistance (TCR) characteristics of TFR components, reduces dependence on component width, and reduces the number of mask layers in the manufacturing process, thereby improving resistance stability and manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117204145B_ABST
    Figure CN117204145B_ABST
Patent Text Reader

Abstract

A damascene method for fabricating a thin film resistor (TFR) module is provided. A pair of heads are formed spaced apart from one another. A dielectric region is deposited on the pair of heads and an opening extending over both heads is formed in the dielectric region. A TFR layer is deposited on the dielectric region and extends into the opening to define a cup-shaped TFR layer structure including: (a) a laterally extending TFR element base conductively connected to both heads; and (b) an upright ridge extending upwardly from the laterally extending TFR element base. A high-density plasma (HDP) ridge removal process is performed to remove or shorten the upright ridge from the cup-shaped TFR layer structure, thereby defining a TFR element having a removed or shortened upright ridge. The removal or shortening of the upright ridge can improve the temperature coefficient of resistance (TCR) characteristics of the TFR element.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related patent applications

[0002] This application claims priority to jointly owned U.S. Provisional Patent Application No. 62 / 222,228, filed July 15, 2021, the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] This disclosure relates to thin-film resistor (TFR) modules formed in integrated circuit (IC) devices, and more specifically to TFR modules comprising TFR elements having removed or shortened vertical ridges, and methods for forming such TFR modules. Background Technology

[0004] As more features are packaged into individual semiconductor chips, there is a growing need to integrate a large number of passive components, such as resistors, into circuits. Some resistors, such as polycrystalline silicon resistors, can be created through ion implantation and diffusion. However, such resistors typically exhibit high resistance variations and can also have resistance values ​​that change drastically with temperature. Techniques used to construct integrated resistors (called thin-film resistors (TFRs)) generally improve the performance of integrated resistors. TFRs are typically formed from materials such as silicon-chromium (SiCr), silicon-silicon carbide-chromium (SiCCr), TaN, nickel-chromium (NiCr), aluminum-doped nickel-chromium (AlNiCr), or titanium-nickel-chromium (TiNiCr).

[0005] Figure 1 shows cross-sectional views of two exemplary TFR modules 100A and 100B implemented using conventional techniques. Referring to the background manufacturing processes of related IC devices, the fabrication of a conventional TFR module 100A or 100B typically requires three addition mask layers. Specifically, a first addition mask layer can be used to create TFR heads 102A and 102B, a second addition mask layer can be used to create TFR element 104, and a third addition mask layer can be used to create TFR vias 106A and 106B. As shown, the TFR element 104 of TFR 100A is formed across the top of TFR heads 102A and 102B, while the TFR element 104 of TFR 100B is formed across the bottom of TFR heads 102A and 102B; however, each design typically uses three addition mask layers.

[0006] Other TFR modules are formed using a damascene process, which reduces the number of additional mask layers required to form the TFR modules. A typical damascene process for forming copper interconnects in IC devices may involve patterning dielectric regions to form open trenches in which copper (or other metals) is intended to be formed. A copper diffusion barrier layer (e.g., a tantalum / tantalum nitride (Ta / TaN) bilayer) is deposited, followed by a copper seed layer, and then bulk copper filling, for example, using an electrochemical plating process. Any excess copper and barrier layer material can then be removed using a chemical-mechanical planarization (CMP) process. The copper retained in the individual trenches serves as a conductor. A dielectric barrier layer, such as silicon nitride (SiN) or silicon carbide (SiC), is then typically deposited on the wafer to prevent copper diffusion into adjacent silicon, thereby improving device reliability.

[0007] Figure 2A illustrates an exemplary TFR module 200 formed using a damascene process including a single added mask layer. The TFR module 200 includes TFR elements 202 formed on a pair of spaced-apart TFR heads 204 on a field oxide region 210. Each TFR head 204 may include a silicide structure comprising a polysilicon region 206 having a silicide contact layer 208 formed thereon. TFR contacts 212 may be connected to the silicide contact layer 208 formed on each respective TFR head 204.

[0008] The TFR element 202 is formed by a mosaic process, which includes forming an opening in a metal-front dielectric (PMD) region 211 and depositing a TFR element film into the opening to form the TFR element 202, such that the TFR element 202 includes a horizontally extending substrate 220 and a vertically extending ridge (sidewall) 222 extending upward from the peripheral edge of the horizontally extending substrate 220. The vertically extending ridge 222 typically has a vertical height substantially greater than 2,000 Å. The temperature coefficient of resistance (TCR) of the TFR element 202 may be affected by the vertically extending ridge 222 of the TFR element 202. For example, the TCR of the TFR element 202 can be taken as the width of the TFR element 202 along the y-axis direction (into the page), i.e., perpendicular to the length L of the TFR element along the x-axis direction. TFR The TCR varies as a function of the TFR width. Figure 2B provides a graph showing the TCR as a function of the TFR width for a set of exemplary TFR instances with a construction represented by TFR module 200, where the set of TFR instances has a common TFR element length (L) of 100 micrometers. TFR (and different TFR element widths in the range of 0.9 micrometers to 10 micrometers.)

[0009] There is a need for improved TFR modules and fabrication methods for integrated circuits. For example, there is a need or advantage for TFR modules with characteristics such as: using a reduced number of mask layers compared to the conventional TFR 100A and 100B discussed above; having a near-zero temperature coefficient of resistance (TCR) (e.g., in the range of -100ppm / ℃ to +100ppm / ℃); and having, for example, a lower dependence on the width of the TFR element compared to some existing fabrications. In some applications, it is also necessary to provide, for example, a thin-film resistance R of approximately 1 kΩ / square. s Such TFR modules. Summary of the Invention

[0010] This disclosure provides thin-film resistors (TFRs) that can be modularly integrated into an IC structure, and therefore such thin-film resistors are referred to herein as "TFR modules," as well as methods for forming such TFR modules. Specifically, this disclosure provides TFR modules having TFR elements with vertically extending TFR element ridges (also simply referred to as vertical ridges), which have been removed or vertically shortened using a high-density plasma (HDP) ridge removal process. This disclosure also provides exemplary methods for forming such TFR elements with reduced vertically extending TFR element ridges. For example, this disclosure provides TFR modules having TFR elements and exemplary methods for forming such TFR elements that do not have vertical ridges due to the HDP ridge removal process, or have vertical ridges with a height of less than 200 Å.

[0011] In some examples, a TFR element is formed by the following steps: (a) forming a cup-shaped TFR layer structure comprising a laterally extending TFR element substrate and vertical ridges (sidewalls) extending upward from the periphery of the laterally extending TFR element substrate; and (b) performing an HDP ridge removal process to remove or shorten the vertical ridges, thereby defining a TFR element comprising a laterally extending TFR element substrate and shortened or removed vertical ridges. In some examples, the HDP ridge removal process for removing or shortening the vertical ridges includes: (a) depositing a capping layer; and (b) performing high-density plasma sputtering etching to remove or shorten the vertical ridges, wherein the capping layer protects the laterally extending TFR element substrate from the effects of the sputtering etching. In some examples, a batch fill process is performed after the HDP ridge removal process to fill openings on the TFR element (e.g., with an oxide or nitride filler material).

[0012] In some examples, a TFR element with removed or shortened vertical ridges can be formed between a polysilicon layer (e.g., for forming the gate or other components of a complementary metal-oxide-semiconductor (CMOS) transistor) and a first metal interconnect layer (metal-1 or M1 layer). In other examples, a TFR element with removed or shortened vertical ridges can be formed between two metal interconnect layers M1 and M2. x and M x+1 In either case, compared to background CMOS fabrication processes, a mosaic method with a single mask layer can be used to form TFR devices.

[0013] TFR elements with removed or shortened vertical ridges, as disclosed herein, can exhibit improved temperature coefficient of resistance (TCR) characteristics compared to TFR elements with full-height vertical ridges (i.e., vertical ridges not removed or shortened, as disclosed herein). For example, as referenced below... Figure 5 The TCR as a function of the TFR element width can vary significantly less for TFR elements (as disclosed herein) with a removed or shortened vertical ridge compared to the corresponding TFR with a full-height vertical ridge.

[0014] One aspect provides a method for manufacturing a TFR module. The method includes: forming a pair of spaced-apart heads; depositing a dielectric region on the pair of heads; and forming an opening in the dielectric region extending on each of the pair of heads. A TFR layer is deposited on the dielectric region and extends into the opening to define a cup-shaped TFR layer structure including: (a) a laterally extending TFR element substrate electrically connected to the two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate. A high-density plasma (HDP) ridge removal process is performed to remove or shorten the vertical ridge from the cup-shaped TFR layer structure, thereby defining a TFR element having the removed or shortened vertical ridge.

[0015] In one example, forming an opening in the dielectric region includes depositing a photoresist layer, patterning a photoresist opening in the photoresist layer, the patterned photoresist opening extending laterally over at least a portion of each of the pair of heads, and etching through the patterned photoresist opening to form an opening in the dielectric region.

[0016] In one example, the high-density plasma ridge removal process includes depositing a capping layer on a laterally extended TFR element and performing high-density plasma sputtering etching to remove or shorten the vertical ridge.

[0017] In one example, a batch fill process is performed after high-density plasma sputtering etching to fill the openings with oxide material.

[0018] In one example, the capping layer contains silicon oxide. In another example, the capping layer contains silicon nitride.

[0019] In one example, high-density plasma sputtering etching forms sloping sidewalls on opposite sides of the opening.

[0020] In one example, high-density plasma sputtering etching removes the full height of the vertical ridge.

[0021] In one example, each of the pair of heads includes a polysilicon structure having a silicide layer formed thereon. In another example, each of the pair of heads includes a metal structure formed in a metal interconnect layer.

[0022] In some examples, the TFR layer contains silicon-chromium (SiCr) or silicon-silicon carbide-chromium (SiCCr).

[0023] In one example, annealing is performed after depositing the TFR layer but before performing the high-density plasma process, where annealing alters the temperature coefficient of resistance (TCR) of the TFR layer.

[0024] In some examples, annealing achieves a TCR of 0 ± 50 ppm / ℃ for the TFR layer. In other examples, annealing achieves a TCR of 0 ± 10 ppm / ℃ for the TFR layer. Furthermore, in some examples, annealing is performed at temperatures ranging from 450℃ to 550℃.

[0025] In one example, the method includes performing a chemical mechanical polishing (CMP) process to remove the portion of the TFR layer outside the opening.

[0026] In one example, the method includes: forming a pair of vertically extending contacts, each vertically extending contact being electrically connected to a corresponding head of the pair; and forming a pair of upper connecting elements, each upper connecting element being electrically connected to a corresponding vertically extending contact of the pair.

[0027] Another aspect provides a TFR module formed by a method comprising the steps of: forming a pair of heads spaced apart from each other; depositing a dielectric region on the pair of heads; forming an opening in the dielectric region extending on each of the pair of heads; depositing a TFR layer on the dielectric region and extending into the opening to define a cup-shaped TFR layer structure comprising: (a) a laterally extending TFR element substrate electrically connected to the two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate; and performing a high-density plasma ridge removal process to remove or shorten the vertical ridge.

[0028] Another aspect provides a TFR module including a pair of spaced-apart heads and a TFR element, the TFR element including a laterally extending TFR element substrate electrically connected to the two heads to define a conductive connection between the spaced-apart heads. The TFR module further includes: a first dielectric region above the pair of heads, the first dielectric region including a pair of inclined sidewalls extending upward from respective edges of the TFR element; and a second dielectric region between the pair of inclined sidewalls of the first dielectric region, wherein the second dielectric region has at least one material property different from the first dielectric region.

[0029] In one example, the maximum height of the TFR element is less than 1,000 Å.

[0030] In one example, the TFR element does not have a ridge extending vertically from the lateral TFR element base.

[0031] In one example, the TFR element includes vertical ridges extending upward from a laterally extending TFR element substrate, each vertical ridge having a vertical height of less than 200 Å.

[0032] In one example, the pair of spaced-out heads are spaced apart from each other in a first lateral direction; the TFR element has a lateral width in a second lateral direction perpendicular to the first lateral direction; and the TFR element includes vertical ridges extending upward from a laterally extending TFR element base, each vertical ridge having a vertical height less than 10% of the lateral width of the TFR element. In one example, each vertical ridge has a vertical height less than 1% of the lateral width of the TFR element. In another example, each vertical ridge has a vertical height less than 0.1% of the lateral width of the TFR element.

[0033] In one example, the dielectric constant of the second dielectric region is different from that of the first dielectric region.

[0034] In one example, each of the heads includes a polysilicon structure having a silicide layer formed thereon. In another example, each of the heads includes a metal structure formed in a metal interconnect layer. Attached Figure Description

[0035] Exemplary aspects of this disclosure are described below with reference to the accompanying drawings, in which: Figure 1 is a cross-sectional view of two exemplary known thin-film resistors (TFRs); Figure 2A is a cross-sectional view of an exemplary known TFR formed using a mosaic process and including a TFR element with vertical ridges (sidewalls); Figure 2B is a graph showing the correlation between TCR as a function of the TFR element width for the TFR construction shown in Figure 2A. Figure 3 This is a cross-sectional view based on an example of an exemplary TFR with vertical ridges (sidewalls) removed or shortened; Figures 4A to 4L An exemplary process for forming an exemplary TFR having a removed or shortened vertical ridge is shown; Figure 5 It shows that for Figure 4L The exemplary TFR shown is illustrated with a graph showing the correlation between TCR and the width of the TFR element; and Figures 6A to 6K Another exemplary process is shown for forming an exemplary TFR with a removed or shortened vertical ridge. Detailed Implementation

[0036] This disclosure provides a TFR module having a TFR element having a vertically extending TFR element ridge (also simply referred to as a vertical ridge) that has been removed or vertically shortened. The disclosure also provides exemplary methods for forming such a TFR element having a vertically extending TFR element ridge. As described below, removing or shortening the vertical ridge of a TFR element can improve the temperature coefficient of resistance (TCR) characteristics of the TFR element, for example, compared to a TFR element having a full-height vertical ridge (i.e., a vertical ridge that has not been removed or shortened as disclosed herein).

[0037] Figure 3 This is a cross-sectional view of an exemplary thin-film resistor (TFR) module 300, which includes a TFR element 302 having vertical ridges that have been removed or shortened. The TFR element 302 is formed between a polysilicon layer 303 and a first metal interconnect layer M1 (also referred to as the metal-1 layer).

[0038] As shown in the figure, the TFR element 302 of the exemplary TFR module 300 is formed on a pair of spaced-apart TFR heads 304. Each TFR head includes a silicide polysilicon structure, which includes a polysilicon structure 306 having a metal silicide layer 308 formed thereon. Each TFR head 304 is contacted by a corresponding upper TFR connection element 340 via a corresponding TFR contact 312. Each TFR contact 312 may be electrically connected to the metal silicide layer 306 of the corresponding TFR head 304. Each upper TFR connection element 340 may be formed in a metal interconnect layer M1. In the illustrated example, the metal interconnect layer M1 may be formed on a phosphosilicate glass (PSG) layer 334 and an undoped silicate glass (USG) overlay oxide layer 336 deposited on the structure.

[0039] The TFR element 302 can be formed by a damascene process, which includes forming an opening in a dielectric region 310b (e.g., a metal front dielectric, PMD) and depositing a TFR element layer in the wide opening, the dielectric region 310b being formed on a field oxide region 310a and a TFR head 304. The TFR element layer deposited in the wide opening defines a cup-shaped TFR layer structure, which includes a horizontally extending TFR element substrate 320 and vertically extending ridges (sidewalls) 322 extending upward from the peripheral edge of the TFR element substrate 320.

[0040] The vertically extending ridge 322 of the cup-shaped TFR layer structure (also referred to herein as the vertical ridge 322) can be completely or partially removed by a high-density plasma (HDP) ridge removal process. As discussed in more detail below, the HDP ridge removal process can partially or completely remove the vertical ridge 322 (while protecting the TFR element substrate 320 from removal) and can define an opening 328 in the dielectric region 310b having an inclined (i.e., non-vertical) sidewall 330 extending upward from the TFR element substrate 320. A batch filling process can then be performed to fill the opening 328 with a dielectric material 332, which may have a different dielectric constant (and / or other different material properties) than the dielectric region 310b outside the opening 328.

[0041] In some examples, the HDP ridge removal process removes a portion of the height of each vertical ridge 322, leaving shortened vertical ridges 322'. Thus, the TFR element 302 of the fully formed TFR module 300 includes a horizontally extending TFR element base 320 and shortened vertical ridges 322' extending upward from the peripheral edge of the horizontally extending TFR element base 320.

[0042] In other examples, the HDP ridge removal process completely removes the vertical ridge 322, such that the TFR element 302 of the fully formed TFR module 300 includes only the horizontally extending TFR element base 320 without the shortened vertical ridge 322'.

[0043] In either case (i.e., partial or complete removal of the vertical ridge 322), in some examples, the maximum vertical height H of the TFR element 302, including the horizontally extending TFR element base 320 and (optionally) the shortened vertical ridge 322', is... TFR Less than 1,000 Å. In some examples, the maximum vertical height H of the TFR element 302 is... TFR Less than 600 Å.

[0044] In some examples involving only partial removal of the vertical ridge 322, the vertical height H of each shortened vertical ridge 322' is... SVR Less than 200 Å. In some examples, depending on specific process parameters, the vertical height H of each shortened vertical ridge 322' is... SVR It is less than 10% of the y-direction width of the horizontally extended TFR element substrate 320, less than 1% of the y-direction width of the TFR element substrate 320, or less than 0.1% of the y-direction width of the horizontally extended TFR element substrate 320.

[0045] Compared to a TFR element that includes an unshortened vertical ridge (e.g., as shown in FIG. 2A), a TFR element 302 with the vertical ridge 322 removed or shortened can have improved TCR characteristics. For example, see the following reference. Figure 5 The TCR of the TFR element 302 (with a removed or shortened vertical ridge) discussed herein varies significantly as a function of the TFR element width (in the y-axis direction, inwards from the page) compared to the corresponding width-dependent TCR variation of the TFR element with a full-height vertical ridge.

[0046] Figures 4A to 4L An exemplary process for forming an integrated circuit (IC) structure 400 according to an example is shown. This IC structure includes an exemplary TFR module 401, which includes TFR elements 458 having vertical ridges that have been removed or shortened. The completed TFR module 401... Figure 4L As shown below, the TFR element 458 is formed between the polysilicon layer 403 and the first metal interconnect layer M1 (also known as the metal-1 layer).

[0047] Figure 4AThe initial formation of an IC structure 400 including an exemplary TFR module 401 is illustrated by forming a pair of TFR heads 404 on a field oxide region 410a. Each TFR head 404 includes a polysilicon silicide structure comprising a metal silicide layer 406 formed on a corresponding polysilicon structure 408. For example, a polysilicon layer 403 is deposited, patterned, and etched to form the pair of polysilicon structures 408, and other polysilicon structures separate from the TFR module 401, such as defining a CMOS gate structure. A metal silicide region 406 is then formed on each polysilicon structure 408. Each metal silicide region 406 is self-aligned on the corresponding polysilicon structure 408; therefore, the TFR head 404 may be referred to as a self-aligned polysilicide (self-aligned silicide) TFR head 404. For example, the self-aligned polysilicide TFR head 404 may contain any suitable silicon-based chemical substance, such as CoSi2, NiSi, or TiSi2. In one example, each polysilicon structure 408 has a thickness in the range of 1000 Å to 3000 Å, and the metal silicide layer 406 on each polysilicon structure 408 has a thickness in the range of 100 Å to 300 Å.

[0048] like Figure 4B As shown, the IC structure 400 can be further processed by, for example, depositing a metal-before-dielectric (PMD) region 410b on the structure using a high-density plasma (HDP) deposition process. In one example, the PMD region 410b can be formed by depositing a silicon-rich oxide (SRO) layer with a thickness of approximately 1,000 Å, followed by depositing an HDP oxide layer with a thickness of approximately 10,000 Å.

[0049] like Figure 4C As shown, a pre-metal dielectric chemical / mechanical planarization (PMD CMP) process is performed on IC structure 400. In one exemplary embodiment, the PMD CMP process is performed to achieve a target thickness T of approximately 4,000 Å on polysilicon layer 403. PMD .

[0050] like Figure 4D As shown, a sacrificial oxide layer 410c (e.g., having a thickness of about 1,000 Å) is deposited on the IC structure 400, for example, using a plasma-enhanced chemical vapor deposition (PECVD) process. The sacrificial oxide layer 410c can subsequently be removed (e.g., polished away), as described below regarding... Figure 4J The discussion.

[0051] like Figure 4EAs shown, a photoresist layer 430 can be deposited and patterned to extend laterally over a portion of the width of each TFR head 404, or in other examples, to extend laterally over the full width of one or both TFR heads 404 as a photoresist opening 432.

[0052] like Figure 4F As shown, etching is performed through photoresist opening 432 to define opening 434 in the underlying sacrificial oxide layer 410c and PMD region 410b. Etching can be selective, stopping at the metal silicide layer 406 on the TFR head 404. In some examples, the etching process can be controlled to avoid significant over-etching into the PMD region 410b. After etching, any remaining photoresist material 430 can be removed, for example, by performing a photoresist stripping. As shown, opening 434 exposes an incomplete portion of the top surface of each metal silicide layer 406.

[0053] like Figure 4G As shown, the TFR layer 440 is deposited on the IC structure 400 and extends down into the opening 434, for example, using a physical vapor deposition (PVD) or sputtering deposition process. In one example, the TFR layer 440 comprises a SiCr layer with a thickness in the range of 400 Å–600 Å. In other examples, the TFR layer 440 may contain SiCCr, TaN, NiCr, AlNiCr, TiNiCr, or any other suitable TFR material.

[0054] The portion of TFR layer 440 extending downward into opening 434 defines a cup-shaped TFR layer structure 450, which includes: (a) a laterally extending TFR element substrate 452 electrically connected to two TFR heads 404 (in this example, the TFR element substrate 452 directly contacts a metal silicide layer 406 on each TFR head 404); and (b) vertical ridges 454 extending upward from the TFR element substrate 452. For example, when viewed from above, the TFR element substrate 452 may have a rectangular shape (i.e., a rectangular shape in the xy plane), wherein four vertical ridges 454 extend upward from the four lateral edges of the rectangular TFR element substrate 452.

[0055] The IC structure 400, including the TFR layer 440, can then be annealed, for example, at a temperature of about 500°C (e.g., 400°C-600°C or 450°C-550°C) to obtain a TCR (temperature coefficient of resistance) of 0 ppm or close to 0 ppm for the TFR layer 440. In some examples, depending on the specific example, a TCR "close to 0" ppm may include a TCR of 0 ± 100 ppm / °C, or a TCR of 0 ± 50 ppm / °C, or a TCR of 0 ± 20 ppm / °C, or a TCR of 0 ± 10 ppm / °C. Additionally, in some examples, the annealed TFR layer 440 may have a sheet resistance in the range of 500 Ω / square to 1 kΩ / square.

[0056] Next, as Figure 4H As shown, a high-density plasma (HDP) ridge removal process can be performed to remove or vertically shorten the vertical ridge 454 to define the TFR element 458. In one example, the HDP ridge removal process involves an HDP chemical vapor deposition (HDPCVD) process, which is a specific PECVD process using a higher plasma density than a typical PECVD process.

[0057] In some examples, the HDP ridge removal process may include two constituent processes: (1) depositing a capping layer 460 on the TFR element layer 440 (including on the TFR element substrate 452); and (2) HDP sputtering etching to remove the full height or a portion of the height of the vertical ridge 454. These two constituent processes may be performed together in a common HDP chamber and may overlap at least partially in time.

[0058] In some examples, the capping layer 460 may comprise an oxide layer. The deposited capping layer 460 protects the underlying TFR element substrate 452 from removal by HDP sputtering etching. The timing and other operating parameters of the two component processes of the HDP ridge removal process (i.e., depositing the capping layer 460 and HDP sputtering etching) can be selected and adjusted across a range of manufacturing processes to achieve target performance characteristics, such as completely eliminating or limiting shortening (e.g., below a defined height) the vertical ridge 454, while also protecting the TFR element substrate 452 from removal by HDP sputtering etching.

[0059] In some examples, HDP sputtering etching removes the full height of each vertical ridge 454, such that the resulting TFR element 458 comprises only the laterally extending TFR element substrate 452.

[0060] In other examples, HDP sputtering etching removes only a portion of the height of each vertical ridge 454, leaving shortened vertical ridges 454'. In such examples, the resulting TFR element 458 comprises a laterally extending TFR element substrate 452 and shortened vertical ridges 454' extending upward from the lateral edges of the TFR element substrate 452. In some examples, each shortened vertical ridge 454' has a vertical height H of less than 200 Å. SVR In some examples, depending on specific process parameters, the vertical height H of each shortened vertical ridge 454' is... SVR It is less than 10% of the y-direction width of the horizontally extended TFR element substrate 452, less than 1% of the y-direction width of the TFR element substrate 452, or less than 0.1% of the y-direction width of the horizontally extended TFR element substrate 452.

[0061] In some examples, regardless of whether the vertical ridge 454 is completely or partially removed, the maximum height H of the TFR element 458 is... TFR All are less than 1000 Å. In some examples, the maximum height H of the TFR element 458 is... TFR Less than 600 Å.

[0062] The HDP ridge removal process can alter the shape and size of the opening 434. For example, as Figure 4H As shown, the sputtering etching performed in the HDP ridge removal process widens the opening 434 by removing or shortening the vertical ridge 454 and the portion of the PMD region 410 near the vertical ridge 454, resulting in sloping (i.e., non-vertical) sidewalls or "facets" 466 of the remaining PMD region 410 on the opposite side of the opening 434.

[0063] Assuming the HDP ridge removal process is performed in a vertical orientation (e.g., vertical oxide deposition and sputtering etch direction), the oxide deposition rate (forming capping layer 460) and HDP sputtering etch rate can be considered as the rate at which each surface is acted upon relative to the horizontal plane (by...). Figure 4H The angle (target surface angle) varies as a function of the xy plane (represented in the figure). For example... Figure 4H As shown, this dependence of the HDP ridge removal process orientation on the relevant target surface angle can form: (a) a raised region of the cover layer 460 on the TFR element substrate 452, indicated at 460a; and (b) an inclined (i.e., non-vertical) sidewall 466 extending upward and outward from the lateral edge of the TFR element substrate 452.

[0064] Next, as Figure 4I As shown, in Figure 4HFollowing the HDP ridge removal process shown, a batch fill process is performed to completely fill the opening 434 with a dielectric material 470 (e.g., oxide). In some examples, the batch fill deposition of the dielectric material 470 can be performed within the same HDP chamber as the HDP ridge removal process. In other examples, the batch fill can be performed outside the HDP chamber. The dielectric material 470 (e.g., oxide) deposited in the opening 434 may have a different dielectric constant (and / or one or more other material properties) than the PMD region 410b laterally located outside the opening 434. For example, the dielectric constant of the dielectric material 470 may differ from the dielectric constant of the PMD region 410b (e.g., containing SRO) by at least 0.01.

[0065] like Figure 4J As shown, the IC structure 400 can be further processed by performing a CMP process to remove the portions of the dielectric material 470, the capping layer 460, and the TFR layer 440 located outside the opening 434, as well as the sacrificial oxide layer 410c. In one example, a CMP process is performed to achieve the same target thickness T as the CMP performed before the formation of the TFR module 401 begins. PMD (For example, 4,000 Å), that is, the above reference Figure 4C The CMP process is discussed. Therefore, the TFR module 401 can be formed in a modular manner at different depths in the IC structure 400 without changing the background process used to form other structures on the wafer.

[0066] like Figure 4K As shown, in one example, a phosphosilicate glass (PSG) layer or film 410d is deposited on the PMD region 410b, followed by the deposition of an undoped silicate glass (USG) overlay oxide layer 410e. The PSG layer 410d and the USG overlay oxide layer 410e can be deposited as steps in a background CMOS process for forming an IC structure 400 (e.g., for forming other structures on a wafer outside the occupied area of ​​the formed TFR module 401). In one exemplary embodiment, the PSG layer 410d and the USG overlay oxide layer 410e may each have a deposition thickness in the range of 1000 Å to 3000 Å (e.g., about 2000 Å).

[0067] Finally, as Figure 4LAs shown, a pair of vertically extending TFR contacts 490 (also referred to herein as TFR contacts 490 for convenience) can be formed, each TFR contact 490 contacting or otherwise electrically connected to a corresponding TFR head 404. In some examples, the TFR contacts 490 are formed simultaneously with CMOS contacts and may have the same diameter or width as the CMOS contacts in the IC structure 400. In one example, the TFR contacts 490 are formed by the following steps: patterning and etching the IC structure 400 to define a pair of openings (e.g., contact openings); filling the openings with a conductive material such as tungsten (W); and performing a CMP process to planarize the top surface of each TFR contact 490 with the top surface of the USG overlay oxide layer 410e.

[0068] Following the CMP process, a pair of upper TFR connection elements 494 can be formed in the first metal interconnect layer M1 (also known as the metal-1 layer). In such examples, the upper TFR connection elements 494 can be formed together with other metal-1 interconnect structures (e.g., interconnect lines or wires) separate from the TFR module 401. Each upper TFR connection element 494 is formed to contact or otherwise electrically connect to a corresponding TFR contact 490, such that each upper TFR connection element 494 is electrically connected to a corresponding TFR head 404.

[0069] The TFR contact 490 and the upper TFR connector 494 can be formed using any suitable process or one or more. For example, the TFR contact 490 can be formed using a damascene process, followed by the deposition and selective etching of the metal interconnect layer M1 to form the upper TFR connector 494. Alternatively, the TFR contact 490 can be formed using a first damascene process, followed by the upper TFR connector 494 using a second damascene process. Alternatively, the TFR contact 490 and the upper TFR connector 494 can be formed together using a dual damascene process. The TFR contact 490 and the upper TFR connector 494 can be formed from any suitable metal or one type of metal. For example, the TFR contact 490 can be formed from tungsten, and the upper TFR connector 494 can be formed from copper or aluminum. Alternatively, both the TFR contact 490 and the upper TFR connector 494 can be formed from copper or aluminum, for example, using a dual damascene process or other suitable processes.

[0070] In this manner, a TFR module 401, including a TFR element 458 having a completely removed vertical ridge 454 or a shortened vertical ridge 454', can be formed between a polysilicon layer 403 and a first metal interconnect layer M1 using an embedding method that adds a single mask layer to the background IC manufacturing process. Furthermore, in some embodiments, the TFR element 458 may be formed of SiCr or other suitable materials annealed to achieve 0 ppm or near-0 ppm TCR. Additionally, the TFR module 401 can be compatible with copper or aluminum interconnects (e.g., where the TFR contact 490 and the upper TFR connection element 494 are each formed of copper or aluminum).

[0071] As described above, compared to a TFR element that includes an unremoved TFR element ridge (e.g., extending upwards to the top of the dielectric region forming the TFR element), as shown in FIG2A, removing or shortening the vertical ridge 454 can improve the TCR characteristics of the resulting TFR element 458.

[0072] Figure 5 A graph illustrating exemplary TCR data for an exemplary TFR module 401 having a TFR element 458 is provided, wherein the TFR element has, for example, according to Figures 4A to 4L The process shown creates vertical ridges that have been removed or shortened. Specifically, the graph illustrates the length (L) of a common TFR element with a length of 100 micrometers in the x-axis direction. TFR However, multiple instances of TFR element 458 with different TFR element widths ranging from 0.9 micrometers to 10 micrometers are shown, with TCR representing the TFR element width (in...). Figure 4L The change in TCR value as a function of the TFR element width is shown in the diagram. The change in TCR value as a function of the TFR element width is significantly smaller than the TCR change of a similar TFR module including a TFR element with an unremoved (i.e., full-height) TFR element ridge, for example, as compared to... Figure 5 The exemplary graph shown is comparable to the exemplary graph shown in Figure 2B.

[0073] Figures 6A to 6K An exemplary process for forming an IC structure 600 according to one example is shown, which includes another exemplary TFR module 601, the TFR module including TFR elements 658 having vertical ridges removed or shortened. TFR module 601 is generally similar to TFR module 401 discussed above, but wherein the TFR elements 658 are formed on two metal interconnect layers M. x and M x+1 It is located between, rather than between, the polysilicon layer and the first metal interconnect layer M1.

[0074] Figure 6AThrough the lower metal interconnect layer M on the first dielectric region 610a (e.g., the first intermetallic dielectric (IMD) region) x A pair of metal TFR heads 604 are formed, illustrating the initial formation of an IC structure 600 including an exemplary TFR module 601. Lower metal interconnect layer M x This can include any metal interconnect layer at any depth in the IC structure 600, such as, but not limited to, metal-1 layer (M1) and metal-2 layer (M2). Lower metal interconnect layer M x It may contain aluminum, copper, or a suitable metal, and may include various interconnect structures, such as metal lines or conductors, in addition to the pair of TFR heads 604. For example, such interconnect structures and TFR heads 604 may be formed by deposition and etching of metal layers or by a damascene process.

[0075] like Figure 6B As shown, the second dielectric region 610b, such as the second IMD region, is deposited on the lower metal interconnect layer M including the TFR header 604. x Above. (As shown) Figure 6C As shown, an intermetallic dielectric CMP (IMD CMP) process can be performed on the underlying metal interconnect layer M. x The target thickness T of the second IMD region 610b will be reduced to approximately 6,000 Å. IMD .

[0076] Next, as Figure 6D As shown, a sacrificial oxide layer 610c (e.g., having a thickness of approximately 1000 Å) can be deposited on the IC structure 600, for example, using a plasma-enhanced chemical vapor deposition (PECVD) process. The sacrificial oxide 610c can then be polished away, as described below regarding... Figure 6J The discussion.

[0077] Next, as Figure 6E As shown, a photoresist layer 630 can be deposited and patterned to define photoresist openings 632 that extend laterally at least partially on both TFR heads 604. Figure 6F As shown, using any suitable etching process, etching is performed through the photoresist opening 632 to define the TFR opening 634 in the underlying sacrificial oxide layer 610c and IMD region 610b. This etching process can be stopped at the metal TFR head 604 and can be controlled to avoid significant over-etching into the IMD region 610b. After etching, any remaining photoresist material 630 can be removed, for example, by performing a photoresist stripping.

[0078] like Figure 6GAs shown, for example, a PVD or sputtering deposition process is used to deposit a TFR layer 640 on the IC structure 600 and extend downward into the TFR opening 634. (As mentioned above...) Figure 4G As discussed in the example shown, annealing the TFR layer 640 to improve its TCR characteristics may be advantageous. However, unlike the polysilicon layer 403 in which the TFR head 404 of the exemplary 4L TFR module 401 described above is constructed, the lower metal interconnect layer M in which the TFR head 604 of the TFR module 601 is formed... x The material may not be effectively resistant to high-temperature annealing (e.g., above 400°C) used to improve the TCR properties of the TFR layer 640. Therefore, in some examples, the TFR layer 640 may be formed from a material with suitable or target TCR properties without annealing. For example, the TFR layer 640 may comprise a SiCCr layer with a thickness of approximately 100 Å (e.g., in the range of 50 Å–200 Å). Alternatively, the TFR layer 640 may comprise SiCr, TaN, NiCr, AlNiCr, TiNiCr, or any other suitable TFR material.

[0079] The portion of TFR layer 640 extending downward into TFR opening 634 defines a cup-shaped TFR layer structure 650, which includes: (a) a laterally extending TFR element substrate 652 electrically connected to two TFR heads 604 (in this example, the TFR element substrate 652 directly contacts each TFR head 604); and (b) vertical ridges 654 extending upward from the TFR element substrate 652 (also simply referred to as vertical ridges 654). For example, the TFR element substrate 652 may have a rectangular shape when viewed from above (i.e., a rectangular shape in the xy plane), wherein four vertical ridges 654 extend upward from the four lateral edges of the rectangular TFR element substrate 652.

[0080] Next, as Figure 6H As shown, a high-density plasma (HDP) ridge removal process can be performed to remove or vertically shorten the vertical ridge 654 to define the TFR element 658. In one example, the HDP ridge removal process involves an HDP chemical vapor deposition (HDPCVD) process.

[0081] The HDP ridge removal process may include two constituent processes: (1) depositing a capping layer 660 on the TFR element layer 640 (including on the TFR element substrate 652); and (2) HDP sputtering etching to remove the full height or a portion of the height of the vertical ridge 654. These two constituent processes may be performed together in a common HDP chamber and may overlap at least partially in time.

[0082] In some examples, the capping layer 660 may comprise silicon oxide, silicon nitride, or a combination thereof. The deposited capping layer 660 can protect the underlying TFR element substrate 652 from removal by HDP sputtering etching. The timing and other operating parameters of the two component processes of the HDP ridge removal process (i.e., the deposition of the capping layer 660 and the HDP sputtering etching) can be selected and adjusted across a range of manufacturing processes to achieve target performance characteristics, such as completely eliminating or limiting shortened (e.g., below a defined height) vertical ridge 654, while also protecting the TFR element substrate 652 from removal by HDP sputtering etching.

[0083] In some examples, HDP sputtering etch removes the full height of each vertical ridge 654, so that the resulting TFR element 658 consists only of the laterally extending TFR element substrate 652.

[0084] In other examples, HDP sputtering etching removes only a portion of the height of each vertical ridge 654, leaving shortened vertical ridges 654'. In such examples, the resulting TFR element 658 comprises a laterally extending TFR element substrate 652 and shortened vertical ridges 654' extending upward from the lateral edges of the TFR element substrate 652. In some examples, each shortened vertical ridge 654' has a vertical height H of less than 200 Å. SVR In some examples, depending on specific process parameters, the vertical height H of each shortened vertical ridge 654' is... SVR It is less than 10% of the y-direction width of the horizontally extended TFR element substrate 652, less than 1% of the y-direction width of the TFR element substrate 652, or less than 0.1% of the y-direction width of the horizontally extended TFR element substrate 652.

[0085] In some examples, regardless of whether the vertical ridge 654 is completely or partially removed, the maximum height H of the TFR element 658 is... TFR All are less than 1,000 Å. In some examples, the maximum height H of the TFR element 658 is... TFR Less than 600 Å.

[0086] As referenced above Figure 4H The capping deposition rate (forming capping 660) and HDP sputtering etch rate discussed can vary as a function of the angle (target surface angle) of each surface being acted upon relative to the horizontal plane, which can result in the formation of: (a) a raised region of capping 660 on the TFR element substrate 652, indicated at 660a; (b) inclined (i.e., non-vertical) sidewalls or “facets” 666 extending upward and outward from the lateral edge of the TFR element substrate 652; and (c) an opening 668 above the raised capping region 660a and between the inclined sidewalls 666.

[0087] Next, as Figure 6I As shown, a batch fill process is performed after the HDP ridge removal process described above. Specifically, a dielectric material 670 (e.g., an oxide or nitride) may be deposited on the IC structure 600 to completely fill the opening 668. According to a particular embodiment, this batch fill deposition of the dielectric material 670 may be performed inside or outside the HDP chamber during the HDP ridge removal process. The dielectric material 670 (e.g., an oxide or nitride) deposited in the opening 668 may have a different dielectric constant (and / or one or more other material properties) than the IMD region 610b located laterally outside the opening 668. For example, the dielectric constant of the dielectric material 670 may differ from the dielectric constant of the IMD region 610b (e.g., containing an oxide) by at least 0.1 or at least 1.0. For example, in one example, the dielectric material 670 may contain a nitride having a dielectric constant of about 7.0, while the IMD region 610b may contain an oxide having a dielectric constant of about 3.9.

[0088] like Figure 6J As shown, the IC structure 600 can be further processed by performing a CMP process to remove portions of the dielectric material 670, capping layer 660, and TFR layer 640 located outside the opening 668, as well as the sacrificial oxide layer 610c. In one example, a CMP process is performed to achieve the same target thickness T as the CMP performed before the formation of the TFR module 601 begins. IMD (For example, 6,000 Å), that is, the above reference Figure 6C The CMP process is discussed. Therefore, the TFR module 601 can be formed in a modular manner at different depths in the IC structure 600 without changing the background process used to form other structures on the wafer.

[0089] Finally, as Figure 6K As shown, a pair of vertically extending TFR contacts 690 (also referred to herein as TFR contacts 690 for convenience) can be formed, each TFR contact 690 contacting or otherwise electrically connected to a corresponding TFR head 604. In some examples, the TFR contacts 690 resemble interconnect vias (and can be formed simultaneously with interconnect vias different from those in TFR module 601), and can have the same diameter or width as the interconnect vias in IC structure 600. Therefore, TFR contacts 690 can also be referred to as TFR vias because they can be formed as a metal interconnect layer M. x and M x+1 Through holes between them.

[0090] In one example, the TFR contact 690 is formed by the following steps: patterning and etching the IC structure 600 to define a pair of openings (e.g., through-hole openings); filling the openings with a conductive material such as tungsten (W); and performing a CMP process to planarize the top surface of each TFR contact 690.

[0091] After the CMP process, an upper metal interconnect layer M can be added. x+1 A pair of upper TFR connection elements 694 are formed, together with additional metal interconnect structures (e.g., interconnect lines or wires) separate from the TFR module 601. Each upper TFR connection element 694 is formed to contact or otherwise electrically connect to a corresponding TFR contact, such that each upper TFR connection element 694 is electrically connected to a corresponding TFR head 604.

[0092] The TFR contact 690 and the upper TFR connection element 694 can be formed using any suitable process or one or more. For example, the TFR contact 690 can be formed by an inlay process, followed by an upper metal interconnect layer M. x+1 The upper TFR connector 694 is formed by deposition and selective etching. Alternatively, the TFR contact 690 can be formed by a first damascene process, followed by a second damascene process to form the upper TFR connector 694. Alternatively, the TFR contact 690 and the upper TFR connector 694 can be formed together using a dual damascene process. The TFR contact 690 and the upper TFR connector 694 can be formed of any suitable one or more metals. For example, the TFR contact 690 can be formed of tungsten, and the upper TFR connector 694 can be formed of copper or aluminum. Alternatively, both the TFR contact 690 and the upper TFR connector 694 can be formed of copper or aluminum, for example, using a dual damascene process or other suitable processes.

[0093] In this way, a TFR module 601, including a TFR element 658 with a completely removed vertical ridge 654 or a shortened vertical ridge 654', can be fabricated using an inlay method that adds a single mask layer to the background IC manufacturing process on two metal interconnect layers M. x and M x+1 The TFR element 658 is formed between the two materials. Furthermore, in some embodiments, the TFR element 658 may be formed from SiCCr or other suitable materials annealed to achieve 0 ppm or near-0 ppm TCR. Additionally, the TFR module 601 may be compatible with copper or aluminum interconnects (e.g., where the TFR contact 690 and the upper TFR connection element 694 are each formed from copper or aluminum).

[0094] As described above, for example as shown in FIG2A, removing or shortening the vertical ridge 654 can improve the TCR characteristics of the resulting TFR element 658 compared to a TFR element that includes an unremoved TFR element ridge (e.g., extending upward to the top of the dielectric region forming the TFR element).

Claims

1. A method for manufacturing a thin-film resistor (TFR) module, the method comprising: Forming a pair of heads spaced apart from each other; Dielectric regions are deposited on the pair of heads; An opening is formed in the dielectric region, the opening extending over at least a portion of the width of each of the pair of heads; A TFR layer is deposited on the dielectric region and extends into the opening to define a cup-shaped TFR layer structure, the cup-shaped TFR layer structure comprising: (a) a laterally extending TFR element substrate electrically connected to two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate; and A high-density plasma ridge removal process is performed to remove or shorten the vertical ridge from the cup-shaped TFR layer structure, thereby defining a TFR element with the removed or shortened vertical ridge, wherein high-density plasma sputtering etching forms inclined sidewalls on opposite sides of the opening.

2. The method of claim 1, wherein forming the opening comprises: Deposition of photoresist layer; The photoresist openings are patterned in the photoresist layer, and the patterned photoresist openings extend laterally over at least a portion of each of the pair of heads. as well as Etching through the patterned photoresist openings to form the openings in the dielectric region.

3. The method according to claim 1, wherein the high-density plasma ridge removal process comprises: A capping layer is deposited on the laterally extending TFR element; as well as Perform the high-density plasma sputtering etching to remove or shorten the vertical ridges.

4. The method of claim 3, further comprising filling the opening with an oxide material after the high-density plasma sputtering etching.

5. The method of claim 3, wherein the covering layer comprises silicon oxide.

6. The method of claim 3, wherein the capping layer comprises silicon nitride.

7. The method of claim 3, wherein the high-density plasma sputtering etching removes the full height of the vertical ridge.

8. The method of claim 1, wherein each of the pair of heads comprises a polysilicon structure having a silicide layer formed thereon.

9. The method of claim 1, wherein each of the pair of heads comprises a metal structure formed in a metal interconnect layer.

10. The method of claim 1, wherein the TFR layer comprises SiCr or SiCCr.

11. The method of claim 1, comprising performing annealing after depositing the TFR layer but before performing the high-density plasma ridge removal process, wherein the annealing is performed at a selected temperature and duration to change the temperature coefficient of resistance (TCR) of the TFR layer.

12. The method of claim 11, further comprising performing annealing to achieve a TCR of 0 ± 50 ppm / °C for the TFR layer.

13. The method of claim 11, further comprising performing annealing to achieve a TCR of 0 ± 10 ppm / °C for the TFR layer.

14. The method of claim 11, comprising performing the annealing at a temperature in the range of 450°C to 550°C.

15. The method of claim 1, further comprising performing a chemical mechanical polishing process to remove a portion of the TFR layer outside the opening.

16. The method of claim 15, further comprising forming at least one of a phosphosilicate glass layer or an undoped silicate glass overlay oxide layer after the chemical mechanical polishing process.

17. The method of claim 1, comprising: A pair of vertically extending contacts are formed, each of which is electrically connected to a corresponding head in the pair of heads; as well as A pair of upper connecting elements are formed, wherein each upper connecting element is electrically connected to a corresponding vertically extending contact of the vertically extending contacts.

18. A thin-film resistor (TFR) module, said thin-film resistor module being formed by a method comprising the following: Forming a pair of heads spaced apart from each other; Dielectric regions are deposited on the pair of heads; An opening is formed in the dielectric region, the opening extending over at least a portion of the width of each of the pair of heads; A TFR layer is deposited on the dielectric region and extends into the opening to define a cup-shaped TFR layer structure, the cup-shaped TFR layer structure comprising: (a) a laterally extending TFR element substrate electrically connected to two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate; and A high-density plasma ridge removal process is performed to remove or shorten the vertical ridge, wherein high-density plasma sputtering etching forms inclined sidewalls on opposite sides of the opening.

19. A thin-film resistor (TFR) module, comprising: A pair of heads spaced apart; A TFR element, comprising a laterally extending TFR element substrate electrically connected to two heads, thereby defining a conductive connection between the spaced-out pair of heads. The first dielectric region on the pair of heads; The first dielectric region has a pair of inclined sidewalls extending upward from the respective edge of the TFR element; as well as A second dielectric region is located between the pair of inclined sidewalls of the first dielectric region; The second dielectric region has at least one material property that is different from that of the first dielectric region.

20. The TFR module of claim 19, wherein the maximum height of the TFR element is less than 1,000 Å.

21. The TFR module of claim 19, wherein the TFR element has no ridge extending vertically from the laterally extending TFR element base.

22. The TFR module of claim 19, wherein the TFR element includes vertical ridges extending upward from the laterally extending TFR element base, each vertical ridge having a vertical height of less than 200 Å.

23. The TFR module according to claim 19, wherein: A pair of spaced-out heads are spaced apart from each other in the first lateral direction; The TFR element has a lateral width in a second lateral direction perpendicular to the first lateral direction; and The TFR element includes vertical ridges extending upward from the laterally extending TFR element base, each vertical ridge having a vertical height less than 10% of the lateral width of the TFR element.

24. The TFR module of claim 19, wherein each of the heads comprises a polysilicon structure having a silicide layer formed thereon.

25. The TFR module of claim 19, wherein each of the heads comprises a metal structure formed in a metal interconnect layer.

26. A method for manufacturing a thin-film resistor (TFR) module, the method comprising: Forming a pair of heads spaced apart from each other; Dielectric regions are deposited on the pair of heads; An opening is formed in the dielectric region, the opening extending over at least a portion of the width of each of the pair of heads; A TFR layer is deposited on the dielectric region and extends into the opening to define a cup-shaped TFR layer structure, the cup-shaped TFR layer structure comprising: (a) a laterally extending TFR element substrate electrically connected to two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate; and A high-density plasma ridge removal process is performed to remove the full height of the vertical ridge from the cup-shaped TFR layer structure, thereby defining a TFR element with a removed or shortened vertical ridge, wherein high-density plasma sputtering etching forms inclined sidewalls on opposite sides of the opening.

27. The method of claim 26, wherein the high-density plasma ridge removal process comprises: A capping layer is deposited on the laterally extending TFR element; as well as The high-density plasma sputtering etching is performed to remove the full height of the vertical ridge from the cup-shaped TFR layer structure.

28. A method for manufacturing a thin-film resistor (TFR) module, the method comprising: Forming a pair of heads spaced apart from each other; A first dielectric region is deposited on the pair of heads; An opening is formed in the first dielectric region, the opening extending over at least a portion of the width of each of the pair of heads; A TFR layer is deposited on the first dielectric region and extends into the opening to define a cup-shaped TFR layer structure, the cup-shaped TFR layer structure comprising: (a) a laterally extending TFR element substrate electrically connected to two heads; and (b) a vertical ridge extending upward from the laterally extending TFR element substrate. A high-density plasma ridge removal process is performed to remove or shorten the vertical ridges from the cup-shaped TFR layer structure, thereby defining a TFR element having the removed or shortened vertical ridges. The high-density plasma ridge removal process also expands the opening in the first dielectric region. An enlarged opening in a first dielectric region is filled with a second dielectric region, wherein the second dielectric region has at least one material property different from that of the first dielectric region.

Citation Information

Patent Citations

  • Thin-film resistor in an integrated circuit and manufacturing method thereof

    CN112335065A

  • Damascene Thin-Film Resistor (TFR) In Poly-Metal Dielectric and Method of Fabrication

    US20190109186A1