Fluorine-containing copolymer, method for producing fluorine-containing copolymer, fluorine-containing copolymer composition, and crosslinked rubber article

By using a fluorinated copolymer with a specific composition, the problem of insufficient release properties of cross-linked rubber articles is solved, resulting in better release properties and heat resistance, making it suitable for manufacturing high-performance cross-linked rubber articles.

CN117222680BActive Publication Date: 2026-11-20AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280027889.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-12
Filing Date
2022-04-06
Publication Date
2026-11-20
Estimated Expiration
2042-04-06

AI Technical Summary

Technical Problem

In the existing technology, there is room for improvement in the demolding properties of cross-linked rubber articles, especially since they are difficult to detach effectively during the molding process.

Method used

Fluorinated copolymers with specific compositions, including monomers based on tetrafluoroethylene, perfluorinated (alkyl vinyl ethers), monomers with fluorine atoms and more than two polymerizable unsaturated bonds, and monomers with nitrile groups and fluorine atoms, are used to achieve uniform distribution of branched structures and crosslinking sites by controlling the storage modulus ratio G'0.3/G'0.03 within the range of 1.00 to 1.45, thereby improving demolding properties.

Benefits of technology

It significantly improves the release properties of cross-linked rubber articles, ensuring that they can be more easily released after molding without affecting other properties such as heat resistance and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004488106140000261
    Figure BDA0004488106140000261
  • Figure BDA0004488106140000271
    Figure BDA0004488106140000271
  • Figure BDA0004488106140000291
    Figure BDA0004488106140000291
Patent Text Reader

Abstract

Provided are a fluorine-containing copolymer capable of producing a crosslinked rubber article having excellent mold releasability, a method for producing the fluorine-containing copolymer, a fluorine-containing copolymer composition, and a crosslinked rubber article. The fluorine-containing copolymer of the present invention has a tetrafluoroethylene-based unit, a perfluoro(alkyl vinyl ether)-based unit, a unit based on a monomer having a fluorine atom and 2 or more polymerizable unsaturated bonds, and a unit based on a monomer having a nitrile group and a fluorine atom, and the storage modulus of the fluorine-containing copolymer at an angular frequency of 0.3 rad / s, which is obtained by dynamic viscoelasticity measurement at 140°C, is set as G' 0.3 the storage modulus of the fluorine-containing copolymer at an angular frequency of 0.03 rad / s is set as G' 0.03 G' 0.3 / G' 0.03 is 1.00 to 1.45.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to fluorinated copolymers, methods for manufacturing fluorinated copolymers, fluorinated copolymer compositions, and crosslinked rubber articles. Background Technology

[0002] Crosslinked rubber articles obtained by crosslinking fluorinated copolymers have excellent heat resistance, chemical resistance, oil resistance, and weather resistance, and are therefore suitable for use in various environments.

[0003] As a fluorinated copolymer for obtaining such cross-linked rubber articles, Patent Document 1 discloses a fluorinated copolymer containing units based on tetrafluoroethylene, units based on perfluorinated (alkyl vinyl ether) and units based on monomers having nitrile (cyano) groups.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 6-263952 Summary of the Invention

[0007] The problem the invention aims to solve

[0008] Crosslinked rubber articles are manufactured, for example, by supplying a fluorinated copolymer to a mold and then heating and molding it. The inventors manufactured crosslinked rubber articles using the fluorinated copolymer described in Patent Document 1 and found room for improvement regarding the demolding properties of the crosslinked rubber articles.

[0009] The present invention was made in view of the above-mentioned problems, the problem of which is to provide a fluorinated copolymer capable of producing cross-linked rubber articles with excellent release properties, a method for producing a fluorinated copolymer, a fluorinated copolymer composition, and a cross-linked rubber article.

[0010] Solution for solving the problem

[0011] The inventors have conducted in-depth research on the above-mentioned issues and have discovered that using the following fluorinated copolymers, which have: tetrafluoroethylene-based units, perfluoro(alkyl vinyl ether)-based units, units based on monomers having fluorine atoms and two or more polymerizable unsaturated bonds, and units based on monomers having nitrile groups and fluorine atoms, and G' 0.3 / G' 0.03 Within a specific range, cross-linked rubber articles with excellent release properties can be obtained, thus completing the present invention.

[0012] That is, the inventors discovered that the above-mentioned problems can be solved by the following configuration.

[0013] [1] A fluorinated copolymer comprising: units based on tetrafluoroethylene, units based on perfluorinated (alkyl vinyl ether), units based on monomers having fluorine atoms and two or more polymerizable unsaturated bonds, and units based on monomers having nitrile groups and fluorine atoms.

[0014] The storage modulus of the aforementioned fluorinated copolymer at 140°C and an angular frequency of 0.3 rad / s, determined by dynamic viscoelasticity measurement, is denoted as G'. 0.3 The storage modulus of the aforementioned fluorinated copolymer at an angular frequency of 0.03 rad / s is set as G'. 0.03 At that time, G' 0.3 / G' 0.03 It ranges from 1.00 to 1.45.

[0015] [2] According to the fluorinated copolymer of [1], the molar ratio of the content of the aforementioned unit based on the monomer having fluorine atoms and two or more polymerizable unsaturated bonds to the content of the aforementioned unit based on the monomer having nitrile groups and fluorine atoms is 0.002 to 7.

[0016] [3] The fluorinated copolymer according to [1] or [2], wherein the aforementioned perfluorinated (alkyl vinyl ether) is a monomer represented by formula (1).

[0017] CF2 = CF-OR f1 (1)

[0018] In equation (1), R f1 It refers to perfluoroalkyl groups with 1 to 10 carbon atoms.

[0019] [4] The fluorinated copolymer according to any one of [1] to [3], wherein the monomer having fluorine atoms and two or more polymerizable unsaturated bonds is the monomer shown in formula (2).

[0020] (CR 21 R 22 =CR 23 -) a1 R 24 (2)

[0021] In equation (2), R 21 R 22 and R 23 Each of these can be independently represented by a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group; a1 represents an integer from 2 to 6; R 24 This refers to a perfluoroalkyl group with 1 to 10 carbon atoms and an a1 valence, or a group with an ether-like oxygen atom at the end of the perfluoroalkyl group or between carbon-carbon bonds. Multiple R 21 Multiple R 22 and multiple R 23 Each can choose to be the same as or different from the other.

[0022] [5] According to the fluorinated copolymer described in [4], wherein the monomer shown in the aforementioned formula (2) is the monomer shown in formula (3) or the monomer shown in formula (4).

[0023] (CF2=CF-)2R 31 (3)

[0024] In equation (3), R 31 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0025] (CH2=CH-)2R 41 (4)

[0026] In equation (4), R 41 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0027] [6] The fluorinated copolymer according to any one of [1] to [5], wherein the monomer having nitrile group and fluorine atom is the monomer shown in formula (5).

[0028] CR 51 R 52 =CR 53 -R 54 -CN (5)

[0029] In equation (5), R 51 R 52 and R 53 Each can independently represent a hydrogen atom, a fluorine atom, or a methyl group, R 54 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0030] [7] According to the fluorinated copolymer described in [6], wherein the aforementioned R 51 R 52 and R 53 All of them are fluorine atoms or they are all hydrogen atoms, the aforementioned R 54 It has ether-type oxygen atoms and the number of ether-type oxygen atoms is 1 to 3.

[0031] [8] The fluorinated copolymer according to any one of [1] to [7] is substantially free of iodine atoms.

[0032] [9] A method for manufacturing a fluorinated copolymer, which is a method for manufacturing a fluorinated copolymer as described in any one of [1] to [8], wherein tetrafluoroethylene, perfluorinated (alkyl vinyl ether), monomers having fluorine atoms and two or more polymerizable unsaturated bonds, and monomers having nitrile groups and fluorine atoms are copolymerized in the presence of a free radical polymerization initiator.

[0033]

[10] The method for manufacturing the fluorinated copolymer according to [9] wherein copolymerization is carried out in the absence of a chain transfer agent containing iodine atoms.

[0034]

[11] A fluorinated copolymer composition comprising any one of [1] to [8] a fluorinated copolymer and a crosslinking agent.

[0035]

[12] The fluorinated copolymer composition according to

[11] , wherein the aforementioned crosslinking agent is a compound having two or more amino groups.

[0036]

[13] The fluorinated copolymer composition according to

[11] or

[12] , wherein the content of the crosslinking agent is less than 1.0 parts by weight relative to 100 parts by weight of the aforementioned fluorinated copolymer.

[0037]

[14] A crosslinked rubber article, which is formed by crosslinking the fluorinated copolymer in any one of the fluorinated copolymer compositions described in

[11] to

[13] .

[0038] The effects of the invention

[0039] According to the present invention, a fluorinated copolymer capable of producing cross-linked rubber articles with excellent release properties, a method for producing the fluorinated copolymer, a fluorinated copolymer composition, and the cross-linked rubber article can be provided. Detailed Implementation

[0040] The terms used in this invention have the following meanings.

[0041] "Unit" refers to the atomic group derived directly from one molecule of the aforementioned monomer, formed by the polymerization of monomers, and the atomic group obtained by chemically transforming a portion of the aforementioned atomic group. "Monomer-based unit" is also referred to as "unit" below.

[0042] "Rubber" refers to rubber exhibiting the properties defined by JIS K6200 (2008), and is distinguished from "resin".

[0043] [Fluoropolymers]

[0044] The fluorinated copolymers of the present invention comprise: units based on tetrafluoroethylene (hereinafter also referred to as "TFE"), units based on perfluoro(alkyl vinyl ether) (hereinafter also referred to as "PAVE"), units based on monomers having fluorine atoms and two or more polymerizable unsaturated bonds (hereinafter also referred to as "monomer A"), and units based on monomers having nitrile groups and fluorine atoms (hereinafter also referred to as "R"). CN The unit is 。。

[0045] Furthermore, for the fluorinated copolymer of the present invention, the storage modulus of the fluorinated copolymer at an angular frequency of 0.3 rad / s, determined by dynamic viscoelasticity measurement at 140°C, is defined as G'. 0.3 The storage modulus of the above-mentioned fluorinated copolymer at an angular frequency of 0.03 rad / s is set as G'. 0.03 Time, G' 0.3 / G' 0.03 It ranges from 1.00 to 1.45.

[0046] Crosslinked rubber articles obtained using the fluorinated copolymer of the present invention exhibit excellent demolding properties. The details of the reason for this are not yet clear, but it is presumed to be due to the following reasons.

[0047] The fluorinated copolymer of the present invention has monomer A unit and R CN Unit. The monomer A unit in the fluorinated copolymer forms a branched structure in the crosslinked rubber article obtained using the fluorinated copolymer. Therefore, if monomer A unit is sufficiently introduced into the fluorinated copolymer, the crosslinked rubber article obtained using it becomes rigid. Additionally, R CN The nitrile group of the unit is a crosslinking group, which is achieved by making the monomer A unit and R... CN Crosslinked rubber articles obtained by crosslinking fluorinated copolymers of units become more rigid. For rigid crosslinked rubber articles, it is believed that when the crosslinked rubber article is removed from the mold, the crosslinked rubber becomes less likely to follow the mold, and therefore becomes easier to remove.

[0048] In particular, it is speculated that the fluorinated copolymer of the present invention is used in combination with monomers A or R that are not used in combination. CN Compared to fluorinated copolymers, the branched structure and crosslinking sites are uniformly distributed throughout the fluorinated copolymer. It is believed that in the case of polymerization of gaseous monomers and liquid monomers, the movement of the liquid monomers towards the reaction site is the rate-limiting step of the reaction. The detailed mechanism is not yet clear, but it is thought to be as follows: if monomers A and R... CN When used in combination, it is the same as when using single-component A alone or when using R alone. CN Compared to the previous time, it can promote monomers A and R CN The movement towards the reaction site. Therefore, it is believed that the release property is improved by increasing the hardness of the microscopic parts of cross-linked rubber articles, which is not noticeable from the usual rubber hardness and other physical properties.

[0049] Here, it is difficult to introduce all of monomer A into the fluorinated copolymer during polymerization. Furthermore, it is difficult to determine the extent to which monomer A units are present in the fluorinated copolymer.

[0050] To address this problem, as an indicator of the degree of branching structure present in fluorinated copolymers, the inventors focused on the storage modulus (specifically G') measured under conditions of high angular frequency. 0.3 Compared to the storage modulus measured under conditions of low angular frequency (specifically G') 0.03 The ratio of ) to G' 0.3 / G' 0.03 It can be said that G' 0.3 / G' 0.03 The closer the value is to 1.00, the more branched structures are present in the fluorinated copolymer. The reason for this is that: the more branched structures present, the shorter the easing time during storage modulus measurement, and the smaller the difference in storage modulus caused by shear rate, G' 0.3 / G' 0.03 It is a value close to 1.00.

[0051] Based on this reasoning, it is believed that if G' is used... 0.3 / G' 0.03 Fluorinated copolymers within the above range improve the mold release properties of cross-linked rubber articles.

[0052] Thus, it is inferred that it consists of a single A unit and R. CN The effect brought about by the unit and the G' 0.3 / G' 0.03 The effects within the aforementioned range complement each other, resulting in cross-linked rubber articles with excellent release properties.

[0053] The PAVE unit is a perfluorinated (alkyl vinyl ether) based unit.

[0054] From the perspective of excellent polymerization reactivity and rubber properties, PAVE prefers the monomer shown in formula (1).

[0055] CF2 = CF-OR f1 (1)

[0056] In equation (1), R f1 Represents perfluoroalkyl groups with 1 to 10 carbon atoms. From the perspective of superior polymerization reactivity, R... f1 The carbon number is preferably 1 to 8, more preferably 1 to 6, further preferably 1 to 5, and especially preferably 1 to 3.

[0057] Perfluoroalkyl groups can be linear or branched.

[0058] Specific examples of PAVE include perfluoro(methyl vinyl ether) (hereinafter also referred to as "PMVE"), perfluoro(ethyl vinyl ether) (hereinafter also referred to as "PEVE"), and perfluoro(propyl vinyl ether) (hereinafter also referred to as "PPVE"). Among these, PMVE and PPVE are preferred.

[0059] Monomer A unit is a unit based on a monomer having a fluorine atom and two or more polymerizable unsaturated bonds.

[0060] Specific examples of polymerizable unsaturated bonds include carbon-carbon double bonds (C=C) and carbon-carbon triple bonds (C≡C).

[0061] The number of polymerizable unsaturated bonds in monomer A is preferably 2 to 6, more preferably 2 or 3, and particularly preferably 2, which are more conducive to polymerization reactivity.

[0062] Monomer A unit preferably does not have a nitrile group.

[0063] Monomer A is preferably the monomer shown in formula (2) from the perspective of having better release properties of cross-linked rubber articles.

[0064] (CR 21 R 22 =CR 23 -) a1 R 24 (2)

[0065] In equation (2), R 21 R 22 and R 23 Each of these elements independently represents a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group; a1 represents an integer from 2 to 6; R 24 This refers to a perfluoroalkyl group with 1 to 10 carbon atoms and an a1 valence, or a group having an ether-like oxygen atom at the end of the perfluoroalkyl group or between carbon-carbon bonds. Multiple R 21 Multiple R 22 and multiple R 23 Each can choose to be the same as or different from the others, with a preference for them to be the same.

[0066] a1 is preferably 2 or 3, with 2 being the most preferred.

[0067] Starting from the superior polymerization reactivity of monomer A, R 21 R 22 R 23 Preferably, it is a fluorine atom or a hydrogen atom, more preferably R 21 R 22 R 23 R is particularly preferred for its superior release properties, as it consists entirely of fluorine atoms or entirely of hydrogen atoms, resulting in better mold release properties for cross-linked rubber articles. 21 R22 R 23 It consists entirely of fluorine atoms.

[0068] R 24 It can be any of the following: linear, branched, or cyclic, with linear or branched being preferred, and linear being particularly preferred. R 24 The carbon number is preferably 2 to 8, more preferably 3 to 7, further preferably 3 to 6, and especially preferably 3 to 5.

[0069] R 24 It may or may not have ether-containing oxygen atoms. From the perspective of better crosslinking reactivity and rubber properties, it is preferred to have ether-containing oxygen atoms.

[0070] R 24 The number of ether-containing oxygen atoms is preferably 1 to 6, more preferably 1 to 3, and particularly preferably 1 or 2. 24 The ether oxygen atom in R is preferably present in R 24 The end of.

[0071] Among the monomers shown in Equation (2), specific examples of suitable monomers can be the monomers shown in Equation (3) and Equation (4).

[0072] (CF2=CF-)2R 31 (3)

[0073] In equation (3), R 31 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0074] (CH2=CH-)2R 41 (4)

[0075] In equation (4), R 41 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0076] As specific examples of the monomers shown in equation (3), we can give examples of CF2=CFO(CF2)2OCF=CF2, CF2=CFO(CF2)3OCF=CF2, CF2=CFO(CF2)4OCF=CF2, CF2=CFO(CF2)6OCF=CF 2、CF2=CFO(CF2)8OCF=CF2、CF2=CFO(CF2)2OCF(CF3)CF2OCF=CF2、CF2=CFO(CF2)2O(CF(CF3)CF2O)2CF=CF2、CF2=CFOCF2O(CF2CF2O)2CF=CF2 , CF2=CFO(CF2O)3O(CF(CF3)CF2O)2CF=CF2, CF2=CFOCF2CF(CF3)O(CF2)2OCF(CF3)CF2OCF=CF2, CF2=CFOCF2CF2O(CF2O)2CF2CF2OCF=CF2.

[0077] Among the monomers shown in equation (3), more suitable examples of monomers include CF2=CFO(CF2)3OCF=CF2 (hereinafter also referred to as "C3DVE") and CF2=CFO(CF2)4OCF=CF2 (hereinafter also referred to as "C4DVE").

[0078] Specific examples of the monomers shown in equation (4) include CH2=CH(CF2)2CH=CH2, CH2=CH(CF2)4CH=CH2, and CH2=CH(CF2)6CH=CH2.

[0079] Among the monomers shown in equation (4), CH2=CH(CF2)6CH=CH2 (hereinafter also referred to as "C6DV") is a more suitable example.

[0080] If monomer A is copolymerized, the polymerizable double bond at the end of monomer A will react during polymerization to obtain a branched fluorinated copolymer.

[0081] R CN The unit is based on a monomer having a nitrile group and a fluorine atom. This is achieved by giving the fluorinated copolymer an R... CN The unit crosslinks the rubber articles, resulting in excellent heat resistance.

[0082] From the perspective of polymerization reactivity, R CN Preferably, it has a polymerizable unsaturated bond, and particularly preferably, it has one polymerizable unsaturated bond. Specific examples of polymerizable unsaturated bonds are described above.

[0083] From the perspective of superior release properties and heat resistance of cross-linked rubber articles, R CN The preferred monomer is the one shown in formula (5).

[0084] CR 51 R 52 =CR 53 -R 54 -CN (5)

[0085] In equation (5), R 51 R 52 and R 53 Each can independently represent a hydrogen atom, a fluorine atom, or a methyl group, R 54 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

[0086] From R CN Based on its excellent polymerization reactivity, R 51 R 52 R 53 Preferably, it is a fluorine atom or a hydrogen atom, more preferably R 51 R 52 R 53 R is particularly preferred due to its superior release properties and heat resistance in cross-linked rubber articles, consisting entirely of fluorine atoms or entirely of hydrogen atoms. 51 R 52 R 53 It consists entirely of fluorine atoms.

[0087] R 54 It can be any of the following: linear, branched, or cyclic, with linear or branched being preferred. 54 The carbon number is preferably 2 to 8, more preferably 3 to 7, further preferably 3 to 6, and especially preferably 3 to 5.

[0088] R 54 It may or may not have ether-containing oxygen atoms. From the perspective of superior rubber properties, it is preferred to have ether-containing oxygen atoms.

[0089] R 54 The number of ether oxygen atoms in the sample is preferably 1 to 3, and particularly preferably 1 or 2.

[0090] Specific examples of the monomers shown in formula (5) include CF2=CFOCF2CF(CF3)OCF2CF2CN (hereinafter also referred to as "8CNVE"), CF2=CFO(CF2)5CN (hereinafter also referred to as "MV5CN"), CF2=CFOCF2CF2CF2OCF(CF3)CN, and CF2=CFO(CF2)3CN. From the perspective of superior release properties and heat resistance of cross-linked rubber articles, 8CNVE and MV5CN are preferred.

[0091] Fluorinated copolymers can have properties based on TFE, PAVE, monomers A and R. CN Other than TFE, PAVE, monomers A and R. Hereinafter, sometimes the units other than TFE, PAVE, monomers A and R will be referred to. CN Monomers other than those mentioned above are collectively referred to as "other monomers".

[0092] Specific examples of other monomers include the monomers shown in formula (6), vinylidene fluoride (hereinafter also referred to as "VdF"), hexafluoropropylene (hereinafter also referred to as "HFP"), trichlorofluoroethylene (hereinafter also referred to as "CTFE"), ethylene, and monomers other than TFE, PAVE, A, and R. CN The monomers shown in formula (6), VdF, HFP and CTFE and other monomers containing halogen atoms (hereinafter also referred to as other monomers containing halogen atoms). (For example, bromotrifluoroethylene, iodotrifluoroethylene).

[0093] Equation (6) is as follows.

[0094] CF2 = CF-OR f2 (6)

[0095] In equation (6), R f2 R represents a perfluoroalkyl group having 1 to 8 carbon atoms and containing 1 to 5 ether-containing oxygen atoms. f2 The carbon number is preferably 1 to 6, and particularly preferably 1 to 5.

[0096] Specific examples of the monomers shown in formula (6) include perfluoro(3,6-dioxa-1-heptene), perfluoro(3,6-dioxa-1-octene), and perfluoro(5-methyl-3,6-dioxa-1-nonene).

[0097] From the perspective of improving the heat resistance of cross-linked rubber articles, the content of TFE units is preferably 60-79 mol%, more preferably 63-75 mol%, and particularly preferably 66-72 mol% relative to the total units of the fluorinated copolymer.

[0098] From the perspective of superior elasticity of cross-linked rubber articles, the content of PAVE units relative to the total units of the fluorinated copolymer is preferably 20-39 mol%, more preferably 24-36 mol%, and particularly preferably 27-33 mol%.

[0099] From particularly easy to G' 0.3 / G' 0.03 With regard to improving the release properties, physical properties, and appearance of the crosslinked rubber articles within the aforementioned range, the content of monomer A unit relative to all units of the fluorinated copolymer is preferably 0.01 to 0.35 mol%, more preferably 0.03 to 0.20 mol%, further preferably 0.03 to 0.15 mol%, and particularly preferably 0.06 to 0.13 mol%.

[0100] From the perspective of superior release properties and heat resistance of cross-linked rubber articles, R CNThe content of the unit relative to all units of the fluorinated copolymer is preferably 0.05 to 5 mol%, more preferably 0.1 to 3 mol%, further preferably 0.2 to 1.5 mol%, and particularly preferably 0.4 to 0.8 mol%.

[0101] TFE unit, PAVE unit, single A unit and R CN When the unit is within the above range, it is easy to mistake G' 0.3 / G' 0.03 Adjust to the range mentioned above.

[0102] When the fluorinated copolymer contains other monomer units, from the perspective of the heat resistance of the crosslinked rubber article, the content of the other monomer units is preferably 0.01 to 20 mol%, more preferably 0.5 to 10 mol%, and particularly preferably 1 to 5 mol% relative to the total number of units in the fluorinated copolymer.

[0103] The content of monomer A unit relative to R CN The molar ratio of monomer A units / R CN The molar ratio of the crosslinked rubber article is preferably 0.002 to 7, more preferably 0.01 to 2, further preferably 0.02 to 0.75, particularly preferably 0.075 to 0.43, and most preferably 0.09 to 0.30. When the molar ratio is within the above range, the release properties and heat resistance of the crosslinked rubber article can be balanced at a high level, and the appearance is also excellent.

[0104] It should be noted that the monomer A unit in the fluorinated copolymer, relative to all units, is calculated based on the amount of monomer A used in the manufacture of the fluorinated copolymer (the amount of monomer A used). Here, "the amount of monomer A used" refers to the value obtained by subtracting the amount of unpolymerized monomer A from the amount of monomer A added to the polymerization vessel (the amount of monomer A added). Unpolymerized monomer A is considered to be included in the filtrate after the latex has coagulated and the fluorinated copolymer has been removed, as well as the filtrate remaining after washing the latex; its amount can be determined, for example, by measuring fluoride ions using an ion chromatography apparatus.

[0105] In addition, the TFE units, PAVE units, and R units in the fluorinated copolymer relative to all units CN Unit through 19 It is calculated using F-nuclear magnetic resonance (NMR) analysis. Specifically, it is calculated through... 19 F-NMR analysis was used to determine the TFE units, PAVE units, and R units in the fluorinated copolymer. CN Unit (molar ratio). Then, it will be passed through 19 TFE units and PAVE units in fluorinated copolymers identified by F-NMR analysis: R CNThe unit (molar ratio) is applied to the value obtained by subtracting the content (molar%) of monomer A unit from 100 mol% to determine the content of each unit.

[0106] Fluorinated copolymers are preferably substantially free of iodine atoms.

[0107] By making the fluorinated copolymer substantially free of iodine atoms, the crosslinking properties of the fluorinated copolymer are excellent, resulting in crosslinked articles with less breakage and reduced compression set at high temperatures. Iodine atoms in fluorinated copolymers can serve as crosslinking points, therefore, the inclusion of iodine atoms is considered to result in excellent crosslinking properties. However, even when iodine atoms are included, the crosslinking agent in the fluorinated copolymer composition preferentially reacts with iodine atoms compared to the nitrile groups, even when fluorinated copolymers have nitrile groups as crosslinking points. When the iodine content in the fluorinated copolymer is low, the nitrile groups can react sufficiently with the crosslinking agent. Furthermore, the crosslinked structure formed by the reaction of the nitrile groups of the fluorinated copolymer with the crosslinking agent exhibits excellent heat resistance; therefore, by ensuring sufficient reaction between the nitrile groups of the fluorinated copolymer and the crosslinking agent, heat resistance is improved. Therefore, when using a fluorinated copolymer composition containing a fluorinated copolymer that is substantially free of iodine atoms, it is possible to form a crosslinked article with excellent crosslinking properties, less breakage, and low compression set at high temperatures. Especially when chain transfer agents containing iodine atoms are not used in the manufacture of fluorinated copolymers (described later), the resulting fluorinated copolymers exhibit a wider molecular weight distribution and a good balance between hardness and elongation, thus resulting in excellent mechanical properties (e.g., tensile strength). Furthermore, the wider molecular weight distribution of fluorinated copolymers allows for an increase in lower molecular weight fluorinated copolymers, making it easier to incorporate G' 0.3 / G' 0.03 Adjust to the above range.

[0108] Here, "the fluorinated copolymer is substantially free of iodine atoms" means that the content of iodine atoms is 0.09% by mass or less relative to the total mass of the fluorinated copolymer, preferably 0.05% by mass or less, more preferably 0.02% by mass or less, and particularly preferably 0% by mass (i.e., free of iodine atoms).

[0109] Examples of iodine atoms include iodine atoms derived from iodine compounds that function as chain transfer agents, and iodine atoms in units of monomers that have iodine atoms, such as iodotrifluoroethylene mentioned above, which are monomers containing halogen atoms.

[0110] Specific examples of iodine compounds that function as chain transfer agents include 1,3-diiodopropane, 1,4-diiodobutane (hereinafter also referred to as "DIB"), 1,6-diiodohexane, 1,8-diiodooctane, 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, and 1,8-diiodoperfluorooctane.

[0111] <Properties of Fluorinated Copolymers>

[0112] G' of fluorinated copolymers 0.3 / G' 0.03 The value is 1.00 to 1.45. From the perspective of better demolding properties of cross-linked rubber articles, 1.00 to 1.43 is preferred, 1.20 to 1.43 is more preferred, 1.30 to 1.43 is even more preferred, and 1.40 to 1.43 is most preferred.

[0113] The higher the angular frequency at the time of measurement, the larger the value of the storage modulus, G'. 0.3 / G' 0.03 The value will not be lower than 1.00.

[0114] G' of fluorinated copolymers 0.3 From the perspective of molding operability, 600-800 kPa is preferred, 650-750 kPa is more preferred, and 670-700 kPa is particularly preferred.

[0115] G' of fluorinated copolymers 0.03 From the perspective of molding operability, 400-600 kPa is preferred, 430-550 kPa is more preferred, and 470-500 kPa is particularly preferred.

[0116] Here, G' 0.3 This refers to the storage modulus of the fluorinated copolymer at 140℃ and an angular frequency of 0.3 rad / s, determined by dynamic viscoelasticity measurement. Additionally, G' 0.03 This refers to the storage modulus measured at 140℃ under dynamic viscoelastic conditions at various frequencies of 0.03 rad / s. It should be noted that "rad / s" refers to radians per second.

[0117] G' of the fluorinated copolymer in this invention 0.3 and G' 0.03 The detailed measurement conditions are as shown in the examples, for values ​​determined using a rubber processing analytical apparatus and in accordance with ASTM D6204.

[0118] It should be noted that the G' of the fluorinated copolymer 0.3 / G' 0.03 When the value is 0.92 times, it can be converted into G'1 / G' of the fluorinated copolymer. 0.1 The value of .

[0119] Here, G' 0.1 This refers to the storage modulus measured at 140℃ with an angular frequency of 0.1 rad / s determined by dynamic viscoelasticity. Additionally, G'1 refers to the storage modulus measured at 140℃ with an angular frequency of 1 rad / s determined by dynamic viscoelasticity.

[0120] <Methods for manufacturing fluorinated copolymers>

[0121] In addition, the present invention is a method for manufacturing the aforementioned fluorinated copolymer.

[0122] That is, the method for manufacturing the fluorinated copolymer of the present invention involves mixing TFE, PAVE, monomer A, and R... CN A copolymerization method in the presence of a free radical polymerization initiator.

[0123] As a method for manufacturing the fluorinated copolymer of the present invention, a preferred method is to copolymerize the aforementioned monomers in the presence of a free radical polymerization initiator and under conditions where a chain transfer agent containing iodine atoms is absent. The effect of polymerization under conditions where a chain transfer agent containing iodine atoms is absent is as described above.

[0124] As specific examples of polymerization methods, emulsion polymerization, solution polymerization, and suspension polymerization can be cited. From the perspectives of adjusting molecular weight and copolymer composition and excellent productivity, emulsion polymerization is preferred.

[0125] In the case of manufacturing fluorinated copolymers by emulsion polymerization, for example, it can be carried out by heating the monomers in the presence of an aqueous solvent, an emulsifier, and a free radical polymerization initiator.

[0126] The preferred aqueous solvent is water, or a mixture of water and a water-soluble organic solvent.

[0127] Examples of water-soluble organic solvents include tert-butanol, propylene glycol, dipropylene glycol, dipropylene glycol monomethyl ether, and tripropylene glycol. Tert-butanol and dipropylene glycol monomethyl ether are particularly preferred.

[0128] When the aqueous solvent includes a water-soluble organic solvent, the content of the water-soluble organic solvent is preferably 1 to 40 parts by mass, more preferably 3 to 30 parts by mass, relative to 100 parts by mass of water.

[0129] The amount of aqueous solvent used is preferably 150 to 400 parts by mass relative to 100 parts by mass of monomer, and particularly preferably 250 to 350 parts by mass.

[0130] As an emulsifier, any emulsifier that has been used in emulsion polymerization in the past can be used. From the perspective of the excellent mechanical and chemical stability of the obtained latex, ionic emulsifiers are preferred, and anionic emulsifiers are particularly preferred.

[0131] Specific examples of anionic emulsifiers include hydrocarbon-based emulsifiers such as sodium lauryl sulfate and sodium dodecylbenzene sulfonate, and fluorinated fatty acid salts such as ammonium perfluorooctanoate, sodium perfluorooctanoate, and ammonium perfluorohexanoate. Additionally, F(CF2) is also preferred. p O(CF(X 3 )CF2O) qCF(Y)COOA(where X) 3 Y and Y each independently represent a fluorine atom or a perfluoroalkyl group with 1 to 3 carbon atoms, A represents a hydrogen atom, an alkali metal atom, or NH4, p represents an integer from 1 to 10, and q represents an integer from 0 to 3. The fluorinated emulsifier is shown in the figure. Specific examples of alkali metal atoms in A include sodium and potassium.

[0132] As F(CF2) p O(CF(X 3 )CF2O) q Specific examples of fluorinated emulsifiers represented by CF(Y)COOA include F(CF2)3O(CF(CF3)CF2O)2CF(CF3)COONH4, F(CF2)3OCF(CF3)CF2OCF(CF3)COONH4, F(CF2)3OCF2CF2OCF2COONH4, F(CF2)3O(CF2CF2O)2CF2COONH4, and F(CF2)4OCF2CF2OC F2COONH4, F(CF2)4O(CF2CF2O)2CF2COONH4, F(CF2)3OCF2CF2OCF2COONa, F(CF2)3O(CF2CF2O)2CF 2COONa, F(CF2)4OCF2CF2OCF2COONa, F(CF2)4O(CF2CF2O)2CF2COONa, F(CF2)2OCF2CF2OCF2COONH4 , F(CF2)2O(CF2CF2O)2CF2COONH4, F(CF2)2OCF2CF2OCF2COONa, F(CF2)2O(CF2CF2O)2CF2COONa, C F3OCF2CF2CF2OCF2COONH4, CF3OCF2CF2CF2OCF(CF3)COONH4, CF3OCF2CF2CF2OCF2COONa, CF3OCF2C F2CF2OCF(CF3)COONa, CF3O(CF2O)3CF2COONH4, CF3O(CF2O)3CF2COONa, CF3OCF(CF3)CF2OCF(CF3) COONH4, CF3OCF(CF3)CF2OCF(CF3)COONa, CF3O(CF2CF2O)2CF2COONH4, CF3O(CF2CF2O)2CF2COONa.

[0133] Among them, the preferred emulsifiers are ammonium perfluorooctanoate, F(CF2)4OCF2CF2OCF2COONH4, F(CF2)3OCF2CF2OCF2COONH4, F(CF2)2OCF2CF2OCF2COONH4 and CF3OCF2CF2CF2OCF2COONH4.

[0134] Regarding the molecular weight of the emulsifier, from the perspective of facilitating the removal of the emulsifier when the obtained latex coagulates and the fluorinated copolymer is separated, a molecular weight of 100 to 1000 is preferred, and a molecular weight of 100 to 500 is particularly preferred.

[0135] The amount of emulsifier used is preferably 1 to 10 parts by weight, more preferably 3 to 5 parts by weight, relative to 100 parts by weight of the aqueous solvent.

[0136] Water-soluble polymerization initiators and redox polymerization initiators are preferred as free radical polymerization initiators.

[0137] Specific examples of water-soluble polymerization initiators include persulfate-based initiators such as ammonium persulfate, sodium persulfate, and potassium persulfate, as well as organic polymerization initiators such as disuccinic acid peroxide and azobisisobutylamidine dihydrochloride. Among these, persulfate-based initiators are preferred, and ammonium persulfate is more preferred.

[0138] As redox polymerization initiators, examples include polymerization initiators that combine sulfuric acid and a reducing agent. Among these, polymerization initiators that can polymerize each monomer within a polymerization temperature range of 0–80°C are preferred. Specific examples of persulfates constituting redox polymerization initiators include alkali metal salts of persulfate such as ammonium persulfate, sodium persulfate, and potassium persulfate, with ammonium persulfate being preferred. Specific examples of reducing agents combined with persulfates include thiosulfates, sulfites, bisulfites, metabisulfites, and hydroxymethanesulfinates, with hydroxymethanesulfinates being preferred, and sodium hydroxymethanesulfinate being particularly preferred.

[0139] In the manufacture of the fluorinated copolymers of the present invention, it is preferable to add the monomers in multiple stages. TFE, PAVE, and R are particularly preferred. CN Add in multiple stages. By adding in multiple stages, the monomer units can be evenly distributed in the fluorinated copolymer.

[0140] The amount of free radical polymerization initiator is preferably 0.03 to 0.50 parts by mass relative to 100 parts by mass of monomer, and particularly preferably 0.05 to 0.10 parts by mass.

[0141] In the case of manufacturing fluorinated copolymers via emulsion polymerization, the latex obtained by emulsion polymerization can be coagulated to separate the fluorinated copolymer.

[0142] Examples of coagulation methods include the addition of metal salts, or the addition of inorganic acids such as hydrochloric acid, sulfuric acid, or nitric acid. From the perspective of reducing the mixing of metals into the resulting fluorinated copolymer and making it suitable for use in components (e.g., O-rings) in semiconductor manufacturing apparatuses, the addition of inorganic acids is preferred.

[0143] For details regarding the other components used in the manufacture of fluorinated copolymers and the manufacturing methods, please refer to the methods described in paragraphs 0019 to 0034 of International Publication No. 2010 / 082633.

[0144] In the manufacture of the fluorinated copolymer of the present invention, it is preferable not to use a chain transfer agent containing iodine atoms. Therefore, G' 0.3 / G' 0.03 Adjusting to the above range becomes easy.

[0145] [Fluoropolymer Composition]

[0146] The fluorinated copolymer composition of the present invention comprises the above-described fluorinated copolymer and a crosslinking agent.

[0147] Specific examples of crosslinking agents include organic peroxides and compounds having two or more amino groups (hereinafter also referred to as "polyamine compounds"). From the perspective of the excellent crosslinking properties of fluorinated copolymers and the resulting crosslinked rubber articles with lower compression set at high temperatures, polyamine compounds are preferred.

[0148] Specific examples of organic peroxides include dialkyl peroxides, α,α'-bis(tert-butylperoxide)-p-diisopropylbenzene, α,α'-bis(tert-butylperoxide)-m-diisopropylbenzene, benzoyl peroxide, tert-butylperoxide, and 2,5-dimethyl-2,5-di(benzoylperoxide)hexane.

[0149] Specific examples of dialkyl peroxides include 1,1-di(tert-butylperoxide)-3,3,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroxyperoxide, tert-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxide)-3-hexyne, tert-butyl maleate peroxide, and tert-butyl isopropyl carbonate peroxide.

[0150] Specific examples of polyamine compounds include hexamethylenediamine, hexamethylenediamine carbamate, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter also referred to as "BOAP," alternatively known as bisaminophenol AF.), 2,2-bis(3,4-diaminophenyl)propane, 2,2-bis(3,4-diaminophenyl)hexafluoropropane, 2,2-bis(3-amino-4-(N-phenylamino)phenyl)hexafluoropropane, 4,4'-methylenediphenylamine, m-phenylenediamine, adipic acid dihydrazide, and compounds of formula (XII) in Japanese Patent No. 5833657. Among these, BOAP is preferred from the perspective of superior effects of the present invention.

[0151] The content of the crosslinking agent is preferably less than 1.0 part by weight relative to 100 parts by weight of the fluorinated copolymer, more preferably less than 0.9 parts by weight, even more preferably less than 0.8 parts by weight, and particularly preferably less than 0.6 parts by weight. When the content of the crosslinking agent is within the above range, crosslinked rubber articles with lower compression set at high temperatures can be obtained.

[0152] The lower limit of the crosslinking agent content is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, further preferably 0.2 parts by mass or more, and most preferably 0.4 parts by mass or more, relative to 100 parts by mass of the fluorinated copolymer. When the crosslinking agent content is within the above range, the release properties of the crosslinked article are more excellent.

[0153] <Other Ingredients>

[0154] Fluorinated copolymer compositions may contain components other than those described above, without impairing the effects of the present invention. Other components include crosslinking aids (e.g., triallyl cyanurate, triallyl isocyanurate, trimethylallyl isocyanurate), acid absorbents (e.g., fatty acid esters, fatty acid metal salts, oxides of divalent metals (magnesium oxide, calcium oxide, zinc oxide, lead oxide, etc.)), fillers and reinforcing materials (e.g., carbon black, barium sulfate, calcium metasilicate, calcium carbonate, titanium dioxide, silica, clay, talc), scorch delay agents (e.g., phenolic hydroxyl compounds such as bisphenol A, quinones such as hydroquinone, α-methylstyrene dimers such as 2,4-di(3-isopropylphenyl)-4-methyl-1-pentene), crown ethers (e.g., 18-crown-6), and release agents (e.g., sodium stearate).

[0155] Fluorinated copolymer compositions may contain mold release agents, but sometimes these agents can leach from the surface of cross-linked rubber articles obtained using them, becoming a cause of contamination. Therefore, from the perspective of suitability for use as components (e.g., O-rings) in semiconductor manufacturing apparatuses, fluorinated copolymer compositions are preferably substantially free of mold release agents.

[0156] Here, "the fluorinated copolymer composition is substantially free of mold release agent" means that the content of mold release agent is 0.1 parts by mass or less relative to 100 parts by mass of the fluorinated copolymer, preferably 0.01 parts by mass or less, and particularly preferably 0 parts by mass.

[0157] When the fluorinated copolymer composition contains other components, the total content of the other components is preferably more than 0.1 parts by weight and less than 30 parts by weight relative to 100 parts by weight of the fluorinated copolymer, more preferably 1 to 25 parts by weight, and particularly preferably 5 to 15 parts by weight.

[0158] One method for preparing the fluorinated copolymer composition is to mix the above-mentioned components. The mixing of the components can be carried out using rubber mixing equipment such as rollers, kneaders, Banbury mixers, or extruders.

[0159] Furthermore, after obtaining a mixture containing the above-mentioned components, the mixture can be shaped. Specific examples of shaping methods for the mixture include compression molding, injection molding, extrusion molding, calendering, or methods that dissolve the mixture in a solvent and impregnate or coat it onto a substrate.

[0160] [Cross-linked rubber articles]

[0161] The crosslinked rubber article of the present invention is a rubber article obtained by crosslinking the fluorinated copolymer in the above-mentioned fluorinated copolymer composition.

[0162] As a method for crosslinking the fluorinated copolymer in a fluorinated copolymer composition, a method of crosslinking by heating the fluorinated copolymer composition is preferred.

[0163] Specific examples of heat-based crosslinking methods include hot-press crosslinking, steam crosslinking, and hot-air crosslinking. The appropriate method can be selected based on the shape and intended use of the fluorinated copolymer or the fluorinated copolymer composition.

[0164] The preferred heating conditions are 100–400°C for 1 second to 24 hours.

[0165] The cross-linked rubber, obtained by heating the fluorinated copolymer composition (for primary cross-linking), can be further heated to achieve secondary cross-linking. Secondary cross-linking can stabilize or improve the mechanical properties, compression set, and other properties of the cross-linked rubber.

[0166] The preferred heating conditions for the second crosslinking are 80–350°C for 30 minutes to 48 hours.

[0167] As a crosslinking method other than heating to crosslink fluorinated copolymers, one example is irradiating the fluorinated copolymer composition with radiation to crosslink the fluorinated copolymer. Specific examples of the irradiated radiation include electron beams and ultraviolet light.

[0168] <Physical properties>

[0169] The tensile strength (tensile breaking strength) of cross-linked rubber articles is preferably 15-40 MPa, and particularly preferably 21-35 MPa, based on the excellent properties of rubber.

[0170] The 100% modulus (tensile stress at 100% elongation) of cross-linked rubber articles is preferably 3.0 to 5.0 MPa, and particularly preferably 3.5 to 4.4 MPa, from the perspective of excellent rubber properties.

[0171] The tensile elongation (elongation at cut) of cross-linked rubber articles is preferably 100-250% and particularly preferably 180-215% from the perspective of excellent rubber properties.

[0172] The tensile strength, 100% modulus and elongation at cut of cross-linked rubber articles are determined by means of JIS K6251:2010 (corresponding to international standard ISO 37:2005).

[0173] From the perspective of excellent rubber properties, the hardness (Shore-A) of cross-linked rubber articles is preferably 50 to 90, more preferably 60 to 80, and particularly preferably 65 to 75.

[0174] The hardness (Shore-A) of cross-linked rubber articles is the value measured using a type A hardness tester according to JIS K 6253-1:2012, based on a sheet-like molded cross-linked rubber article (1 mm thick).

[0175] The compression set of the cross-linked rubber article at 300°C is preferably 20% or less. From the perspective of good cross-linking of the fluorinated copolymer and excellent shape recovery of the cross-linked rubber article after pressure, it is more preferably 15% or less, further preferably 13% or less, and particularly preferably 11% or less.

[0176] The lower limit of compression set of cross-linked rubber articles at 300°C is preferably 0%.

[0177] The compression set of the cross-linked rubber article at 320°C is preferably 35% or less. From the perspective of good cross-linking of the fluorinated copolymer and excellent shape recovery of the cross-linked rubber article after pressure, it is more preferably 30% or less, further preferably 29% or less, and particularly preferably 24% or less.

[0178] The lower limit of compression set of cross-linked rubber articles at 320°C is preferably 0%.

[0179] The compression set of the cross-linked rubber article at 325°C is preferably 35% or less. From the perspective of good cross-linking of the fluorinated copolymer and excellent shape recovery of the cross-linked rubber article after pressure, it is more preferably 30% or less, further preferably 29% or less, and particularly preferably 27% or less.

[0180] The lower limit of compression set of cross-linked rubber articles at 325°C is preferably 0%.

[0181] The compression set of cross-linked rubber articles at 300°C, 320°C and 325°C are values ​​measured using a sheet-like molded part (1 mm thick) of cross-linked rubber article according to JIS K6301.

[0182] The aforementioned physical properties of cross-linked rubber articles can be adjusted, for example, by the manufacturing conditions of the fluorinated copolymer (e.g., the order, number, and amount of addition of each monomer), the types and contents of each component contained in the fluorinated copolymer composition, and the manufacturing conditions of the cross-linked rubber articles (e.g., cross-linking conditions).

[0183] <Application>

[0184] Cross-linked rubber products are suitable for materials such as O-rings, sheets, gaskets, oil seals, diaphragms, and V-rings. Additionally, it can be used in heat-resistant and chemical-resistant sealing materials, heat-resistant and oil-resistant sealing materials, wire sheathing materials, sealing materials for semiconductor devices, sealing materials for liquid crystal display panel manufacturing devices, sealing materials for light-emitting diode manufacturing devices, corrosion-resistant rubber coatings, sealing materials for urea-based greases, rubber coatings, adhesive rubber, hoses, tubes, calendered sheets (rolls), sponges, rubber rollers, components for oil drilling, heat sinks, solution crosslinks, rubber sponges, bearing seals (urea-resistant greases, etc.), linings (chemical-resistant), automotive insulating sheets, electronic machine insulating sheets, watchmaking rubber strips, endoscope seals (amine-resistant), bellows (processed from calendered sheets), water heater seals / valves, fender materials (marine and civil engineering, shipbuilding), fiber and non-woven fabrics (protective clothing, etc.), base sealing materials, rubber handbags, stators for single-shaft eccentric screw pumps, components for urea SCR systems, vibration damping agents, shock absorbers, sealants, additives in other materials, and toys.

[0185] Example

[0186] The present invention will now be described in detail with examples. Examples 1-1, 1-2, 1-5, 1-6, 2-1 to 2-4, 2-8, 2-9, 2-11, and 2-12 are examples, and examples 1-3, 1-4, 2-5, 2-6, 2-7, and 2-10 are comparative examples. However, the present invention is not limited to these examples. It should be noted that, unless otherwise specified, the content of each component in the tables described below represents the mass standard.

[0187] [The content of units based on each monomer in fluorinated copolymers]

[0188] The content (mol%) of monomer A unit relative to all units of the fluorinated copolymer is calculated based on the amount of monomer A used in the manufacture of the fluorinated copolymer (amount of monomer A).

[0189] In addition, relative to all units of the fluorinated copolymer, TFE unit, PAVE unit, R CN The content of the unit (mol%) is based on 19 It is calculated using F-nuclear magnetic resonance (NMR) analysis.

[0190] <Calculation of the content of monomer A unit relative to the total number of units in the fluorinated copolymer>

[0191] The filtrate after the polymerized latex coagulates and the fluorinated copolymer is removed, along with the residual filtrate after washing the latex, is filtered using a disc filter. The resulting liquid is then analyzed using an ion chromatography apparatus (manufactured by Daiinstein Ments Co., Ltd., which combines an automatic sample combustion device with an ion chromatography pretreatment device AQF-100 and an ion chromatography apparatus).

[0192] When fluoride ions of 3% by mass or more relative to the amount of monomer A are detected, the amount of monomer A is obtained by subtracting the amount of monomer A in the liquid calculated based on the above ion chromatography results from the amount of monomer A added to the reactor (the amount of monomer A added).

[0193] On the other hand, if no fluoride ions of more than 3% by mass relative to the amount of monomer A are detected, all of the monomer A used is polymerized, and the amount of monomer A used is the amount of monomer A added.

[0194] Based on the amount of monomer A unit obtained in this way, the content (mol%) of monomer A unit relative to all units of the fluorinated copolymer is calculated.

[0195] <Iodine atom content in fluorinated copolymers>

[0196] All the DIBs were polymerized. The ratio (mass%) of the mass of iodine atoms contained in the DIBs to the total mass of the fluorinated copolymers was set as the content of iodine atoms in copolymer 4 (described later) as the fluorinated copolymer.

[0197] Copolymers 1 to 3, 5 and 6, which are fluorinated copolymers, were polymerized without the use of raw materials containing iodine atoms, and therefore do not contain iodine atoms.

[0198] G' of fluorinated copolymers 0.3 / G' 0.03 ]

[0199] Using a rubber processing analytical apparatus (Alpha Technologies, RPA2000), and in accordance with ASTM D6204, the value measured at a temperature of 140°C and an angular frequency of 0.3 rad / s is taken as the G' of the fluorinated copolymer. 0.3 .

[0200] The angular frequency was changed to 0.03 rad / s; otherwise, it was the same as the above G'. 0.3 The same procedure was followed to determine the G' of the fluorinated copolymer. 0.03 .

[0201] Based on the obtained values, the G' of the fluorinated copolymer was calculated. 0.3 / G' 0.03 .

[0202] [Degree of crosslinking in fluorinated copolymer compositions]

[0203] For fluorinated copolymer compositions, M was measured using a rubber processing analytical apparatus (Alpha Technologies, RPA2000) at 177°C for 12 minutes, with an amplitude of 3 degrees and a vibration frequency of 100 times per minute. H and M L .

[0204] The measured M H M represents the maximum torque. L M represents the minimum torque. H -M L (by M) H Subtract M L The obtained value represents the degree of crosslinking (unit: dNm). The degree of crosslinking is an indicator of the crosslinking reactivity of fluorinated copolymers, M H -M L The higher the value, the better the crosslinking reactivity.

[0205] [Specific gravity of cross-linked rubber products]

[0206] The specific gravity of cross-linked rubber articles was determined using a hydrometer (manufactured by Shinko Electronics Co., Ltd.) according to JIS K6220-1:2015.

[0207] [Tensile strength, 100% modulus, and elongation at break of cross-linked rubber articles]

[0208] The tensile strength, 100% modulus and elongation were determined using a test piece made by punching a sheet-shaped cross-linked rubber article (1 mm thick) with a No. 4 dumbbell, according to JISK6251:2010 (corresponding to international standard ISO37:2005).

[0209] It should be noted that the measuring device used is a tensile testing machine with data processing (Quick Reader TS-2530, manufactured by Uejima Manufacturing Co., Ltd.).

[0210] In addition, each experiment was conducted using 3 test pieces, and the arithmetic mean of the measured values ​​of the 3 test pieces was recorded.

[0211] 〔hardness〕

[0212] The hardness (Shore-A) of cross-linked rubber articles was determined using a type A hardness tester according to JIS K6253-3:2012.

[0213] It should be noted that the measuring device used is an automatic hardness tester for rubber (manufactured by Digitest Shore A, H, and Bareiss Testing Machines Co., Ltd.).

[0214] In addition, the experiment was conducted using three test pieces, and the arithmetic mean of the measured values ​​from the three test pieces was recorded.

[0215] [Compression permanent deformation]

[0216] Using test pieces of cross-linked rubber articles, according to JIS K6301, the compression set (%) was measured when the test pieces were kept at 300°C for 70 hours, the compression set (%) was measured when they were kept at 320°C for 70 hours, and the compression set (%) was measured when they were kept at 325°C for 70 hours. The smaller the value of the compression set, the better the recovery of the cross-linked rubber article, that is, the better the cross-linking.

[0217] In addition, the experiment was conducted using three test pieces, and the arithmetic mean of the measured values ​​from the three test pieces was recorded.

[0218] [Thermal Aging Test]

[0219] After measuring the thickness of the cross-linked rubber test piece using a thickness gauge, the test piece was heated at 300°C for 70 hours in air (thermal aging).

[0220] After the heat-aged test pieces were cooled to room temperature, the tensile strength and elongation were measured under the same conditions as the test method described above.

[0221] The experiment was conducted using three test pieces, and the arithmetic mean of the measured values ​​from the three test pieces was recorded.

[0222] Based on the measured values ​​of the test pieces without heat aging (normal test values) and the measured values ​​of the test pieces after heat aging (test values ​​after heat aging), the rate of change before and after the heat aging test (heat aging test change rate) is calculated according to the following formula. The closer the change rate is to 0%, the better the heat resistance.

[0223] Change rate (%) of heat aging test = 100 × {(normal test value) - (test value after heat aging)} / (normal test value)

[0224] [Demolding Test]

[0225] A fluorinated copolymer composition was introduced into a sheet-like mold, and the composition was crosslinked at 180°C for 20 minutes to obtain a crosslinked rubber article (100mm long × 60mm wide × 1mm thick) attached to the mold. Immediately after the crosslinking reaction was completed, air was sprayed onto the interface between the crosslinked rubber article and the mold using an air gun (product name CYCLONE DUSTER, manufactured by Chuo Aircraft Co., Ltd.), and the demolding performance was evaluated according to the following evaluation criteria.

[0226] It should be noted that air was sprayed immediately after the cross-linking reaction was completed, therefore the temperature of the cross-linked material at the time of air spraying is considered to be close to 180°C.

[0227] <Air jet conditions based on air guns>

[0228] Pressure: 0.5 MPa

[0229] Air ejection time: 3 seconds

[0230] <Evaluation Criteria>

[0231] ○: Cross-linked rubber articles are released from the mold.

[0232] ×: The cross-linked rubber article has not detached from the mold.

[0233] [Example 1-1]

[0234] <Manufacturing of Fluorinated Copolymers>

[0235] After degassing a 20L stainless steel pressure reactor equipped with anchoring blades, 7.2L of ultrapure water, 880g of a 30% (w / w) aqueous solution of C2F5OCF2CF2OCF2COONH4 (as emulsifier), 7.3g of 8CNVE, 6.8g of C3DVE, and 15.9g of a 5% (w / w) aqueous solution of disodium hydrogen phosphate dodecahydrate were added. While stirring with the anchoring blades, 137g of TFE and 635g of PMVE were added to the container, and the internal temperature was raised to 80°C. The reactor pressure was 0.90MPa. 40mL of a 3% (w / w) aqueous solution of ammonium persulfate (APS) was added to initiate polymerization. The monomers added before the start of polymerization will be referred to as "initial monomer additions".

[0236] After polymerization begins, monomers are introduced as polymerization proceeds, as follows. Hereinafter, the introduction of monomers after polymerization begins will be referred to as "post-addition," and the monomers introduced after polymerization begins will also be referred to as "post-added monomers."

[0237] When the reactor pressure drops to 0.89 MPa, TFE, 8CNVE, and PMVE are injected to raise the reactor pressure to 0.90 MPa. This operation is repeated each time the reactor pressure drops to 0.89 MPa.

[0238] A 3% by mass aqueous solution of APS is appropriately added when the polymerization rate decreases. The total amount of 3% by mass aqueous solution of APS added after the start of polymerization is 40 mL.

[0239] After the total TFE addition reached 1193 g, the monomer addition was stopped, and the reactor was cooled to stop the polymerization reaction, yielding a latex containing a fluorinated copolymer. The polymerization time was 429 minutes. The total added monomers were: TFE 1193 g, PMVE 668 g, and 8CNVE 66.7 g.

[0240] The obtained latex was added to a 3% (w / w) aqueous solution of nitric acid (manufactured by Kanto Chemical Co., Ltd., premium grade) to coagulate the fluorinated copolymer. The fluorinated copolymer was filtered, washed with water, and vacuum dried to obtain a white fluorinated copolymer. The content (molar ratio) of each unit in the obtained fluorinated copolymer (hereinafter also referred to as "copolymer 1") was TFE unit / PMVE unit / 8CNVE unit / C3DVE unit = 69.8 / 29.5 / 0.6 / 0.1.

[0241] It should be noted that the filtrate after coagulating the polymerized latex and removing the fluorinated copolymer, as well as the residual filtrate after washing the latex, was filtered using a disc filter. The resulting liquid was analyzed using ion chromatography, and no fluoride ions exceeding 3% by mass relative to the C3DVE input were detected. Therefore, all the C3DVE used was polymerized. Based on the amount of C3DVE used, the content of C3DVE units relative to all units in the polymer was calculated.

[0242] [Example 1-2 ~ Example 1-3, Example 1-5, Example 1-6]

[0243] The types of monomers used, the amount of initial monomers added, the amount of subsequent monomers added, and the amount of polymerization initiator added are changed as shown in Table 1. Otherwise, the same procedure as in Example 1-1 is followed to obtain the fluorinated copolymer. Hereinafter, the fluorinated copolymer obtained in Example 1-2 will be referred to as "Copolymer 2", the fluorinated copolymer obtained in Example 1-3 will be referred to as "Copolymer 3", the fluorinated copolymer obtained in Example 1-5 will be referred to as "Copolymer 5", and the fluorinated copolymer obtained in Example 1-6 will be referred to as "Copolymer 6".

[0244] [Example 1-4]

[0245] The types of monomers used, the amount of initial monomers added, the amount of subsequent monomers added, and the amount of polymerization initiator added were changed as shown in Table 1. 3.8 g of DIB, used as a chain transfer agent, was added to the polymerization tank along with ultrapure water, emulsifier, 8CNVE, C3DVE, and disodium hydrogen phosphate dodecahydrate before polymerization began. Otherwise, the process was the same as in Example 1-1 to obtain the fluorinated copolymer. The fluorinated copolymer obtained in Example 1-4 will be referred to as "Copolymer 4" below.

[0246] [Table 1]

[0247]

[0248] The physical properties of the obtained fluorinated copolymers were determined. The results are shown in Table 2.

[0249] [Table 2]

[0250]

[0251] [Example 2-1]

[0252] <Preparation of Fluorinated Copolymer Compositions>

[0253] The components were blended in a ratio of 100 parts by weight of copolymer 1, 5 parts by weight of MT-C (manufactured by Cancarb, MT carbon), and 0.5 parts by weight of BOAP (2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, crosslinking agent), and kneaded using two rollers to obtain a fluorinated copolymer composition. The resulting fluorinated copolymer composition will be referred to as "fluorinated copolymer composition 1" below.

[0254] <Manufacturing of Cross-linked Rubber Articles>

[0255] The fluorinated copolymer composition 1 was crosslinked and molded at 180°C for 20 minutes to obtain a crosslinked rubber sheet with dimensions of 100 mm in length, 60 mm in width, and 1 mm in thickness (first crosslinking). Then, under a nitrogen atmosphere, the crosslinked rubber sheet was heated at 90°C for 3 hours, then heated to 305°C over 5 hours, and then heated for 13 hours while maintaining the temperature at 305°C (second crosslinking).

[0256] After cooling the obtained cross-linked rubber sheet after two cross-linking processes to room temperature, it was punched into a dumbbell shape as specified in JIS K6251, resulting in three test pieces of cross-linked rubber articles. The obtained cross-linked rubber article will be referred to as "cross-linked rubber article 1" below.

[0257] [Example 2-2~Example 2-12]

[0258] Using the fluorinated copolymers, crosslinking agents, and carbon black shown in Tables 3-1 and 3-2, except for the same procedures as in the manufacture of fluorinated copolymer composition 1, fluorinated copolymer compositions 2 to 12 were obtained. Furthermore, using fluorinated copolymer compositions 2 to 12, except for the same procedures as in the manufacture of crosslinked rubber article 1, test pieces of crosslinked rubber articles 2 to 12 were obtained.

[0259] The physical properties of the obtained fluorinated copolymer composition and cross-linked rubber articles were determined, and various evaluation tests were performed on the cross-linked rubber articles. The results are shown in Tables 3-1 and 3-2.

[0260] It should be noted that, for the cross-linked rubber article 9 in Examples 2-9, small cracks were observed after measuring the compression set at 300°C for 70 hours. Furthermore, for the cross-linked rubber article 11 in Examples 2-11 and the cross-linked rubber article 12 in Examples 2-12, small cracks were observed after measuring the compression set at 325°C for 70 hours.

[0261] [Table 3-1]

[0262]

[0263] [Table 3-2]

[0264]

[0265] As shown in Tables 3-1 and 3-2, it was confirmed that by using TFE units, PAVE units, single-unit A units, and R... CN unit, and G' 0.3 / G' 0.03 Fluorinated copolymers in the range of 1.00 to 1.45 and appropriate amounts of crosslinking agents can yield crosslinked rubber articles with excellent release properties (Examples 2-1 to 2-4, 2-8, 2-9, 2-11, and 2-12).

[0266] It should be noted that the entire contents of the specification, claims and abstract of Japanese Patent Application No. 2021-066993, filed on April 12, 2021, are incorporated herein as a disclosure of the specification of this invention.

Claims

1. A fluorinated copolymer comprising: units based on tetrafluoroethylene, units based on perfluorinated (alkyl vinyl ethers), units based on monomers having fluorine atoms and two or more polymerizable unsaturated bonds, and units based on monomers having nitrile groups and fluorine atoms. The monomer having fluorine atoms and two or more polymerizable unsaturated bonds is the monomer shown in formula (2) below. (CR 21 R 22 =CR 23 -) a1 R 24 (2) In equation (2), R 21 R 22 and R 23 Each of these elements independently represents a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group; a1 represents an integer from 2 to 6; R 24 This refers to a group with an ether-like oxygen atom at the end of a perfluorocarbon group having 3 to 7 carbon atoms in the a1 valence, and multiple R... 21 Multiple R 22 and multiple R 23 Each can choose to be the same as or different from the others; The content of the unit based on the monomer having fluorine atoms and two or more polymerizable unsaturated bonds is 0.06~0.20 mol% relative to all units of the fluorinated copolymer. The content of the tetrafluoroethylene-based unit relative to all units of the fluorinated copolymer is 60-79 mol%; The content of the perfluorinated (alkyl vinyl ether)-based unit is 20-39 mol% relative to all units of the fluorinated copolymer. The content of the monomer-based units having nitrile and fluorine atoms is 0.05~5 mol% relative to all units of the fluorinated copolymer. The storage modulus of the fluorinated copolymer at 140°C and an angular frequency of 0.3 rad / s, determined by dynamic viscoelasticity measurement, is denoted as G'. 0.3 The storage modulus of the fluorinated copolymer at an angular frequency of 0.03 rad / s is set as G'. 0.03 At that time, G' 0.3 / G' 0.03 The value is between 1.00 and 1.

45.

2. The fluorinated copolymer according to claim 1, wherein, The molar ratio of the content of the unit based on the monomer having fluorine atoms and two or more polymerizable unsaturated bonds to the content of the unit based on the monomer having nitrile groups and fluorine atoms is 0.002 to 7.

3. The fluorinated copolymer according to claim 1 or 2, wherein, The perfluorinated (alkyl vinyl ether) is a monomer represented by formula (1). CF2=CF-O-R f1 (1) In equation (1), R f1 It refers to perfluoroalkyl groups with 1 to 10 carbon atoms.

4. The fluorinated copolymer according to claim 1, wherein, The monomer shown in formula (2) is either the monomer shown in formula (3) or the monomer shown in formula (4). (CF2=CF-)2R 31 (3) In equation (3), R 31 This indicates a group with an ether-like oxygen atom at the end of a divalent perfluorocarbon group (3-7 carbon atoms). (CH2=CH-)2R 41 (4) In equation (4), R 41 This refers to a group that has an ether-like oxygen atom at the end of a divalent perfluorocarbon group with 3 to 7 carbon atoms.

5. The fluorinated copolymer according to claim 1 or 2, wherein, The monomer having a nitrile group and a fluorine atom is the monomer shown in formula (5). CR 51 R 52 =CR 53 -R 54 -CN (5) In equation (5), R 51 R 52 and R 53 Each can independently represent a hydrogen atom, a fluorine atom, or a methyl group, R 54 It refers to a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon-carbon bonds.

6. The fluorinated copolymer according to claim 5, wherein, The R 51 R 52 and R 53 R is composed entirely of fluorine atoms or entirely of hydrogen atoms. 54 It has ether-type oxygen atoms and the number of ether-type oxygen atoms is 1 to 3.

7. The fluorinated copolymer according to claim 1 or 2 is substantially free of iodine atoms.

8. A method for manufacturing a fluorinated copolymer, comprising the method for manufacturing the fluorinated copolymer according to any one of claims 1 to 7, wherein, In the presence of a free radical polymerization initiator, tetrafluoroethylene, perfluoro(alkyl vinyl ether), monomers having fluorine atoms and two or more polymerizable unsaturated bonds, and monomers having nitrile groups and fluorine atoms are copolymerized.

9. The method for manufacturing the fluorinated copolymer according to claim 8, wherein, Copolymerization was carried out in the absence of chain transfer agents containing iodine atoms.

10. A fluorinated copolymer composition comprising the fluorinated copolymer according to any one of claims 1 to 7 and a crosslinking agent. The crosslinking agent content is 0.4 parts by mass or more relative to 100 parts by mass of the fluorinated copolymer.

11. The fluorinated copolymer composition according to claim 10, wherein, The crosslinking agent is a compound having two or more amino groups.

12. The fluorinated copolymer composition according to claim 10 or 11, wherein, The content of the crosslinking agent is less than 1.0 part by weight relative to 100 parts by weight of the fluorinated copolymer.

13. A crosslinked rubber article formed by crosslinking the fluorinated copolymer in any one of claims 10-12.

Citation Information

Patent Citations

  • Scanning electron microscope

    JP1983033657B2

  • Fluoroelastomer composition

    JP1994263952A

  • Convergence device for draft device of spinning machine and draft device of convergence device

    JP2021066993A

  • Fluorine-containing elastic copolymer, process for the production thereof, and crosslinked rubber articles

    WO2010082633A1

  • Fluorine-containing copolymer, fluorine-containing copolymer composition, and crosslinked rubber article

    CN114630845A