A self-supporting carbon nanofiber-based electrode and a preparation method and application thereof

By loading cobalt phosphide onto a carbon nanofiber-based electrode and using zirconium boride crosslinking to enhance the carbon nanofiber membrane, the problems of low efficiency and high cost of precious metals in existing water electrolysis hydrogen production catalysts are solved, achieving highly efficient hydrogen evolution catalytic performance and stability.

CN117230470BActive Publication Date: 2026-11-20GUANGDONG UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311154359.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2026-11-20
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Existing water electrolysis catalysts for hydrogen production suffer from excessively high reaction potentials, resulting in low efficiency. Precious metal catalysts are expensive and require support, limiting their large-scale application. Non-precious metal catalysts also have insufficient performance.

Method used

A self-supporting carbon nanofiber-based electrode is used. By controlling the diameter of the carbon nanofibers and using zirconium boride crosslinking to form a carbon nanofiber membrane, and loading a layered cobalt phosphide, the mechanical strength and electrochemical active area of ​​the electrode are improved, thus achieving good hydrogen evolution catalytic performance.

Benefits of technology

Self-supporting carbon nanofiber-based electrodes exhibit good hydrogen evolution catalytic activity and stability, low overpotential, small Tafel slope, low charge transfer resistance, and large electrochemical active area, making them suitable for direct use as electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117230470B_ABST
    Figure CN117230470B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of self-supporting carbon nanofiber-based electrode and its preparation method and application.The self-supporting carbon nanofiber-based electrode includes carbon nanofiber membrane and phosphide loaded on the surface of carbon nanofiber of carbon nanofiber membrane;The cross-sectional diameter of the carbon nanofiber is 400-500nm;The carbon nanofiber is crosslinked by zirconium boride;The phosphide is sheet structure, and the thickness of the sheet structure is 10-20nm, and the sheet diameter is 100-200nm;The phosphide is cobalt phosphide.The self-supporting carbon nanofiber-based electrode can be directly used as electrode, and has good hydrogen evolution catalytic activity and hydrogen evolution catalytic stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrode materials technology, and more specifically, to a self-supporting carbon nanofiber-based electrode, its preparation method, and its application. Background Technology

[0002] With industrial development, global energy consumption is increasing, with a large reliance on fossil fuels. This leads to not only the challenge of fossil fuel reserves but also the pressure of greenhouse gas emissions (such as CO2) contributing to the greenhouse effect. Against this backdrop, hydrogen energy has attracted global attention. Hydrogen is abundant and widely distributed in nature, and unlike coal, oil, and natural gas, it does not produce the environmental pollution associated with combustion. Water electrolysis for hydrogen production is considered the most promising method due to its convenient process and low pollution levels. However, water electrolysis still faces challenges such as low efficiency caused by excessively high reaction potentials. While precious metals exhibit excellent catalytic properties (e.g., a patented Au@Pt / CNT catalyst and its preparation method and application) and can effectively reduce the overpotential of the hydrogen electrolysis reaction, their high cost and limited reserves prevent large-scale use. Furthermore, most existing catalysts require loading onto a support to achieve a certain mechanical strength, which also presents challenges and limitations in their application. Therefore, there is an urgent need to develop a high-performance, inexpensive, and easy-to-use non-precious metal electrocatalyst to increase the usability of water electrolysis for hydrogen production. Summary of the Invention

[0003] The primary objective of this invention is to overcome the problems of existing hydrogen evolution electrocatalysts, such as poor performance, high cost, or the need for support during use, and to provide a self-supporting carbon nanofiber-based electrode. The self-supporting carbon nanofiber-based electrode of this invention can be used directly as an electrode and exhibits excellent hydrogen evolution catalytic activity and stability.

[0004] A further objective of this invention is to provide a method for preparing the above-mentioned self-supporting carbon nanofiber-based electrode.

[0005] A further objective of this invention is to provide the application of a self-supporting carbon nanofiber-based electrode or a self-supporting carbon nanofiber-based electrode prepared by the above-described method in the electrocatalytic hydrogen evolution reaction.

[0006] The above-mentioned objective of this invention is achieved through the following technical solution:

[0007] A self-supporting carbon nanofiber-based electrode includes a carbon nanofiber membrane and a phosphide loaded on the surface of the carbon nanofibers of the carbon nanofiber membrane.

[0008] The diameter of the cross-section of the carbon nanofibers is 400-500 nm; the carbon nanofibers are cross-linked by zirconium boride.

[0009] The phosphide has a layered structure with a thickness of 10–20 nm and a sheet diameter of 100–200 nm; the phosphide is cobalt phosphide.

[0010] Loading active materials (such as nickel phosphide) onto a support surface is a common and effective strategy for designing electrocatalysts. Common supports include nickel foam, cobalt foam, elemental metal sheets, and carbon cloth. These supports themselves have a certain strength, which can achieve the loading and support of active materials, making them convenient for use as electrodes. However, due to their inherent characteristics, these common supports have a small specific surface area, limiting the amount of active material that can be loaded, thus resulting in a small electrochemical active area and restricting catalytic activity.

[0011] In existing technologies, carbon nanofibers generally do not have active substances directly loaded onto their surface; instead, the active substances are embedded in the carbon nanofibers or are part of the carbon nanofibers. The inventors of this invention attempted to load phosphides onto the surface of carbon nanofibers; however, carbon nanofibers themselves have low strength and are prone to breakage when loading active substances, making it difficult to achieve effective loading.

[0012] Through extensive research, the inventors of this invention discovered that by controlling the diameter of carbon nanofibers within a specific range and achieving cross-linking between carbon nanofibers using zirconium boride, a carbon nanofiber membrane can be formed. This not only improves the strength of the carbon nanofiber membrane, making it suitable as a direct electrode substrate, but also enables the effective loading of cobalt phosphide with a specific lamellar structure onto the surface of the carbon nanofibers. Furthermore, due to the large specific surface area of ​​carbon nanofibers, they can load a large amount of cobalt phosphide with a specific lamellar structure, thereby giving the material a large electrochemically active area. This, combined with the synergistic effect of cobalt phosphide, results in a self-supporting carbon nanofiber-based electrode exhibiting excellent hydrogen evolution catalytic performance and stability. Specifically, the self-supporting carbon nanofiber-based electrode of this invention exhibits good performance in the hydrogen evolution reaction when j = 10 mA / cm². 2 The overpotential relative to the standard hydrogen electrode is below 43 mV, and the Tafel slope is 47 V dec. -1 Furthermore, the self-supporting carbon nanofiber-based electrode of the present invention has low charge transfer resistance and a large electrochemical active area.

[0013] That is, the self-supporting carbon nanofiber-based electrode of the present invention can be directly used as an electrode and has good hydrogen evolution catalytic activity and hydrogen evolution catalytic stability.

[0014] Preferably, the sheet structure is perpendicular to the surface of the carbon nanofibers.

[0015] The above-mentioned method for preparing the self-supporting carbon nanofiber-based electrode includes the following steps:

[0016] S1. Polyacrylonitrile and zirconium boride are prepared into a spinning solution, and electrospinning is performed to obtain a nanofiber membrane;

[0017] S2. The nanofiber membrane is pre-oxidized and carbonized to obtain a carbon nanofiber membrane;

[0018] S3. Place the carbon nanofiber membrane in a cobalt source solution and perform electrodeposition to obtain the precursor;

[0019] S4. Phosphate the precursor to obtain the self-supporting carbon nanofiber-based electrode.

[0020] The electrodeposition time was 280–350 s, and the current density was -0.4–-0.8 A / cm². 2 .

[0021] By adjusting the electrodeposition time and current density within this range, phosphide can be better loaded onto the surface of the carbon nanofiber membrane without damaging the carbon nanofibers, thereby improving the hydrogen evolution catalytic activity and stability of the self-supporting carbon nanofiber-based electrode.

[0022] Preferably, the electrodeposition time is 280–300 s, and the current density is -0.4–-0.6 A / cm². 2 .

[0023] Preferably, the concentration of polyacrylonitrile in the spinning solution in step S1 is 10-14 wt%, and the concentration of zirconium boride is 2-3 wt%.

[0024] Preferably, the voltage of electrospinning in step S1 is 12-18kV, the distance from the spinning needle to the receiver is 12-20cm, and the flow rate of the spinning solution is 0.009-0.012mL / min.

[0025] More preferably, the voltage for electrospinning in step S1 is 12-14 kV.

[0026] Preferably, the pre-oxidation temperature in step S2 is 250–280°C, and the time is 2–4 hours.

[0027] Preferably, the carbonization process in step S2 is as follows: first, heat at 500-600°C for 2-4 hours, and then heat at 700-1000°C for 1-2 hours.

[0028] More preferably, the carbonization process in step S2 is as follows: first, keep at 500-600°C for 2-4 hours, and then keep at 700-800°C for 1-2 hours.

[0029] Preferably, the cobalt ion concentration of the cobalt solution in step S3 is 0.05–0.2 mol / L.

[0030] More preferably, the cobalt ion concentration of the cobalt solution in step S3 is 0.05–0.1 mol / L.

[0031] Preferably, the phosphorus source used in step S4 for phosphating is sodium hypophosphite.

[0032] Application of the above-mentioned self-supporting carbon nanofiber-based electrode or the self-supporting carbon nanofiber-based electrode prepared by the above method in the electrocatalytic hydrogen evolution reaction.

[0033] Compared with the prior art, the beneficial effects of the present invention are:

[0034] The self-supporting carbon nanofiber-based electrode of the present invention can be used directly as an electrode and has good hydrogen evolution catalytic activity and hydrogen evolution catalytic stability. Attached Figure Description

[0035] Figure 1 This is a SEM image of the carbon nanofiber membrane obtained in step 2 of Example 1.

[0036] Figure 2 This is a photograph of the carbon nanofiber membrane obtained in step 2 of Example 1.

[0037] Figure 3 and Figure 4 The images shown are SEM images of the self-supporting carbon nanofiber-based electrode of Example 1 at different magnifications.

[0038] Figure 5 This is a photograph of the self-supporting carbon nanofiber-based electrode from Example 1.

[0039] Figure 6 The graphs show the polarization curves of the electrodes of Example 1 and Comparative Example 1 in 1M KOH solution.

[0040] Figure 7 The image shows the Tafel slope of the electrodes of Example 1 and Comparative Example 1 in 1M KOH solution.

[0041] Figure 8 and Figure 9 The images shown are SEM images of the carbon-based electrode of Comparative Example 1 at different magnifications.

[0042] Figure 10 The EIS curves of the electrodes of Example 1 and Comparative Example 1 in 1M KOH solution are shown.

[0043] Figure 11 The graph shows the slope of the double-layer capacitance of the electrodes in Example 1 and Comparative Example 1 in 1M KOH solution. Detailed Implementation

[0044] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.

[0045] Example 1

[0046] This embodiment provides a self-supporting carbon nanofiber-based electrode, the preparation method of which is as follows:

[0047] 1. Dissolve 0.6 g of polyacrylonitrile in 6 ml of DMF (NN dimethylformamide) at 60 °C with slow stirring. After complete dissolution, add 0.15 g of ZrB and stir for 1 h to obtain a gray, viscous spinning solution. Load the spinning solution into a syringe and electrospin in an electrospinning machine to obtain nanofiber membranes. The electrospinning parameters were: voltage 14 kV, temperature 30 °C, push speed 0.001 mm / s, and distance from the syringe to the receiving plate 15 cm.

[0048] 2. The obtained nanofiber membrane was pre-oxidized in air with the following parameters: heating to 260℃ at 5℃ / min and holding for 4 hours. The pre-oxidized nanofiber membrane was then carbonized at high temperature in an argon atmosphere with the following carbonization temperature curve: heating to 500℃ at 5℃ / min and holding for 2 hours, then heating to 800℃ at 2℃ / min and holding for 2 hours, followed by natural cooling. After removal, the membrane was washed with deionized water and dried to obtain the carbon nanofiber membrane.

[0049] 3. Using the carbon nanofiber membrane obtained in step 2 as the working electrode and a high-purity cobalt sheet as the counter electrode, the electrolyte was 2M NH4Cl and 0.1M CoCl2. Constant current electrodeposition was performed under an electrochemical workstation. After completion, the membrane was washed with deionized water and dried to obtain the precursor. The electrodeposition current density was set to -0.6 A cm⁻¹. -2 The electrodeposition time was set to 300s.

[0050] 4. Place the precursor obtained in step 2 and 0.85g of NaH2PO2 (after grinding) into a tube furnace, with NaH2PO2 at the front end and the precursor at the rear end. Heat to 300℃ at a rate of 2℃ / min in an argon atmosphere with a flow rate of 50sccm, hold for 2h, and then cool naturally to room temperature. Remove and wash with deionized water, then dry at 60℃ overnight to obtain a self-supporting carbon nanofiber-based electrode.

[0051] Morphological characteristics:

[0052] The carbon nanofiber membrane obtained in step 2 and the self-supporting carbon nanofiber-based electrode obtained in step 4 of this embodiment were photographed by SEM, and physical photographs were also taken. Figure 1 These are SEM images of carbon nanofiber membranes, from... Figure 1 It can be seen that the carbon nanofibers in the carbon nanofiber membrane are cylindrical filaments with smooth surfaces and irregular cross-linking between them. The diameter of the cross-section of the carbon nanofibers is between 400 nm and 500 nm. Figure 2 This is a photograph of a carbon nanofiber membrane.

[0053] Figure 3 and Figure 4 These are SEM images of a self-supporting carbon nanofiber-based electrode at different magnifications. Figure 3 and Figure 4 It is known that the self-supporting carbon nanofiber-based electrode includes a carbon nanofiber membrane and cobalt phosphide with a sheet structure loaded on the surface of the carbon nanofiber membrane; the thickness of the sheet structure is 10-20 nm and the sheet diameter is 100-200 nm. Figure 5 This is a photograph of a self-supporting carbon nanofiber-based electrode.

[0054] Performance testing:

[0055] Test Method: A traditional three-electrode system was used, with a carbon rod as the counter electrode, Ag-AgCl as the reference electrode, and a self-supporting carbon nanofiber-based electrode as the working electrode. Electrochemical performance was tested in a 1M potassium hydroxide aqueous solution, with hydrogen gas introduced before testing to saturate the solution. Linear sweep voltammetry (LSV, 5 mV / s) without infrared correction was used to characterize the polarization curve in the 1M potassium hydroxide solution. The Tafel slope was derived from the LSV curve η = a + b * log|i|, where η is the overpotential, b is the Tafel slope, and i is the measured current density.

[0056] Figure 6 This is the polarization curve of the electrode in 1M KOH solution, from... Figure 6 It is evident that the self-supporting carbon nanofiber-based electrode (Co-P-CNF-300s) of the present invention possesses excellent hydrogen evolution electrocatalytic performance. Specifically, when j = 10 mA / cm 2 At that time, the overpotential of the self-supporting carbon nanofiber-based electrode in this embodiment relative to the standard hydrogen electrode is 27mV. Figure 7 It is the Tafel slope of the electrode in 1M KOH solution, from Figure 7 It can be seen that the Tafel slope of the self-supporting carbon nanofiber-based electrode (Co-P-CNF-300s) in this embodiment is 32V dec. -1 .

[0057] Example 2

[0058] This embodiment provides a self-supporting carbon nanofiber-based electrode, the preparation method of which is basically the same as that in Example 1, except that the voltage of the electrospinning parameter in step 1 is 18kV. Finally, a self-supporting carbon nanofiber-based electrode is obtained.

[0059] Morphological characteristics:

[0060] The microstructure of the self-supporting carbon nanofiber-based electrode obtained in this embodiment is similar to that of the self-supporting carbon nanofiber-based electrode in Example 1.

[0061] Performance testing:

[0062] The testing method is the same as in Example 1. The self-supporting carbon nanofiber-based electrode of this example also exhibits excellent electrocatalytic performance; specifically, when j = 10 mA / cm², [the electrocatalytic performance is achieved]. 2 The overpotential relative to the standard hydrogen electrode is 43 mV, and the Tafel slope is 45 Vdec. -1 .

[0063] Example 3

[0064] This embodiment provides a self-supporting carbon nanofiber-based electrode, the preparation method of which is basically the same as that in Example 1, except that the CoCl2 concentration of the electrolyte in step 3 is 0.15M. Finally, a self-supporting carbon nanofiber-based electrode is obtained.

[0065] Morphological characteristics:

[0066] The microstructure of the self-supporting carbon nanofiber-based electrode obtained in this embodiment is similar to that of the self-supporting carbon nanofiber-based electrode in Example 1.

[0067] Performance testing:

[0068] The testing method is the same as in Example 1. The self-supporting carbon nanofiber-based electrode of this example also exhibits excellent electrocatalytic performance; specifically, when j = 10 mA / cm², [the electrocatalytic performance is achieved]. 2 The overpotential relative to the standard hydrogen electrode is 40 mV, and the Tafel slope is 42 Vdec. -1 .

[0069] Example 4

[0070] This embodiment provides a self-supporting carbon nanofiber-based electrode, the preparation method of which is basically the same as that of Example 1, except that: in step 2, the carbonization temperature curve is set as follows: the temperature is increased to 500℃ at 5℃ / min and held for 2 hours, then increased to 1000℃ at 2℃ / min and held for calcination for 2 hours, and then cooled naturally. Finally, the self-supporting carbon nanofiber-based electrode is obtained.

[0071] Morphological characteristics:

[0072] The microstructure of the self-supporting carbon nanofiber-based electrode obtained in this embodiment is similar to that of the self-supporting carbon nanofiber-based electrode in Example 1.

[0073] Performance testing:

[0074] The testing method is the same as in Example 1. The self-supporting carbon nanofiber-based electrode of this example also exhibits excellent electrocatalytic performance; specifically, when j = 10 mA / cm², [the electrocatalytic performance is achieved]. 2 The overpotential relative to the standard hydrogen electrode is 42 mV, and the Tafel slope is 47 Vdec. -1 .

[0075] Comparative Example 1

[0076] This comparative example provides a carbon-based electrode, the preparation method of which is basically the same as that of Example 1, except that in step 3, the electrodeposition time is set to 500s.

[0077] Morphological characteristics:

[0078] The carbon-based electrode of this comparative example was photographed using SEM, and the results are as follows: Figure 8 and Figure 9 As shown. Figure 8 and Figure 9 These are SEM images of a carbon-based electrode at different magnifications, from... Figure 8 and Figure 9 It can be seen that the carbon-based electrode no longer exhibits a fibrous shape because the active material has grown excessively on the carbon nanofibers.

[0079] Performance testing:

[0080] The testing method is the same as in Example 1. The electrocatalytic performance of the carbon-based electrode in this comparative example is poor; specifically, when j = 10 mA / cm², the electrocatalytic performance is poor. 2 The overpotential relative to the standard hydrogen electrode is 72 mV. Figure 6 Co-P-CNF-500s), Tafel slope is 80Vdec -1 ( Figure 7 Co-P-CNF-500s).

[0081] Figure 10 The EIS curves of the electrodes in 1M KOH solution for Examples 1 and Comparative Example 1 show that the semi-circular diameter of the low-frequency region of the self-supporting carbon nanofiber-based electrode of Example 1 is significantly smaller than that of Comparative Example 1, indicating that the self-supporting carbon nanofiber-based electrode of the present invention has a smaller charge transfer resistance and better electrocatalytic performance.

[0082] Figure 11The graphs are fitting plots of the double-layer capacitance slopes of the electrodes in 1M KOH solution for Examples 1 and Comparative Example 1. It can be seen that the Cdl slope of the self-supporting carbon nanofiber-based electrode of Example 1 is significantly greater than that of Comparative Example 1, indicating that the self-supporting carbon nanofiber-based electrode of the present invention has a larger electrochemical active area.

[0083] Comparative Example 2

[0084] This comparative example provides a carbon-based electrode, the preparation method of which is basically the same as that of Example 1, except that in step 3, the electrodeposition current density is set to -2A cm⁻¹. -2 At this current density, the carbon nanofiber membrane is damaged, making it impossible to successfully fabricate a carbon-based electrode.

[0085] Comparative Example 3

[0086] This comparative example provides a carbon-based electrode, the preparation method of which is basically the same as that of Example 1, except that in step 3, the electrodeposition current density is set to -0.1 A cm⁻¹. -2 Finally, a carbon-based electrode was obtained.

[0087] Performance testing:

[0088] The testing method is the same as in Example 1. The electrocatalytic performance of the carbon-based electrode in this comparative example is poor, possibly because the low current density makes it difficult for the active material to grow on the carbon nanofibers, thus affecting the electrocatalytic hydrogen evolution performance. Specifically, when j = 10 mA / cm 2 The overpotential relative to the standard hydrogen electrode is 65 mV, and the Tafel slope is 91 V dec. -1 .

[0089] Comparative Example 4

[0090] This comparative example provides a carbon-based electrode, the preparation method of which is basically the same as that of Example 1, except that zirconium boride is not added to the spinning solution in step 1. After pre-oxidation and carbonization, a carbon nanofiber membrane similar to that of Example 1 is obtained. However, when the carbon nanofiber membrane is used for electrodeposition in step 3, the carbon nanofiber membrane is damaged and the active material cannot be electrodeposited, so the carbon-based electrode cannot be successfully prepared.

[0091] Comparative Example 5

[0092] This comparative example provides a self-supporting carbon nanofiber-based electrode, the preparation method of which is basically the same as that of Example 1, except that in step 3, the counter electrode is a high-purity nickel sheet, the electrolyte is 2M NH4Cl and 0.1M NiCl2, and finally a self-supporting carbon nanofiber-based electrode is obtained, the surface of which is loaded with nickel phosphide.

[0093] Morphological characteristics:

[0094] The microstructure of the self-supporting carbon nanofiber-based electrode obtained in this comparative example is similar to that of the self-supporting carbon nanofiber-based electrode in Example 1.

[0095] Performance testing:

[0096] The testing method is the same as in Example 1. The electrocatalytic performance of the self-supported carbon nanofiber-based electrode in this comparative example is poor; specifically, when j = 10 mA / cm², the electrocatalytic performance is poor. 2 The overpotential relative to the standard hydrogen electrode is 58 mV, and the Tafel slope is 70 V dec. -1 .

[0097] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A self-supporting carbon nanofiber-based electrode, characterized in that, Including carbon nanofiber membranes and phosphides loaded on the surface of carbon nanofibers in the carbon nanofiber membranes; The diameter of the cross-section of the carbon nanofibers is 400-500 nm; the carbon nanofibers are cross-linked by zirconium boride. The phosphide has a layered structure with a thickness of 10–20 nm and a sheet diameter of 100–200 nm; the phosphide is cobalt phosphide.

2. The self-supporting carbon nanofiber-based electrode according to claim 1, characterized in that, The sheet structure is perpendicular to the surface of the carbon nanofibers.

3. The method for preparing the self-supporting carbon nanofiber-based electrode according to any one of claims 1 to 2, characterized in that, Includes the following steps: S1. Polyacrylonitrile and zirconium boride are prepared into a spinning solution, and electrospinning is performed to obtain a nanofiber membrane; S2. The nanofiber membrane is pre-oxidized and carbonized to obtain a carbon nanofiber membrane; S3. Place the carbon nanofiber membrane in a cobalt source solution and perform electrodeposition to obtain the precursor; S4. Phosphate the precursor to obtain the self-supporting carbon nanofiber-based electrode. The electrodeposition time was 280–350 s, and the current density was -0.4–-0.8 A / cm². 2 .

4. The preparation method according to claim 3, characterized in that, In step S1, the concentration of polyacrylonitrile in the spinning solution is 10-14 wt%, and the concentration of zirconium boride is 2-3 wt%.

5. The preparation method according to claim 3, characterized in that, In step S1, the voltage for electrospinning is 12-18 kV, the distance from the spinning needle to the receiver is 12-20 cm, and the flow rate of the spinning solution is 0.009-0.012 mL / min.

6. The preparation method according to claim 3, characterized in that, The pre-oxidation temperature in step S2 is 250–280°C, and the time is 2–4 hours.

7. The preparation method according to claim 3, characterized in that, The carbonization process described in step S2 is as follows: first, keep at 500-600℃ for 2-4 hours, and then keep at 700-1000℃ for 1-2 hours.

8. The preparation method according to claim 3, characterized in that, The cobalt ion concentration of the cobalt source solution in step S3 is 0.05–0.2 mol / L.

9. The preparation method according to claim 3, characterized in that, The phosphorus source selected for phosphating in step S4 is sodium hypophosphite.

10. The application of the self-supporting carbon nanofiber-based electrode according to any one of claims 1 to 2 or the self-supporting carbon nanofiber-based electrode prepared by any one of claims 3 to 9 in the electrocatalytic hydrogen evolution reaction.

Citation Information

Patent Citations

  • Method for preparing electrostatic spinning liquid of zirconium boride nano ceramic fiber

    CN102351539A

  • Nano cobalt phosphide-porous carbon nanofiber flexible membrane and preparation method thereof

    CN107715899A