A method for manufacturing a diamond logic integrated device

By fabricating hydrogen- and silicon-terminated diamond logic integrated devices on high-quality single-crystal diamond, the problems of lack of normally closed enhancement-mode devices and poor process compatibility in diamond logic integrated devices have been solved. This has resulted in diamond semiconductor logic integrated devices with high mobility and low interface state density, exhibiting high stability and logic functionality.

CN117238757BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311194564.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-09-04
Filing Date
2023-09-15
Publication Date
2026-11-24
Estimated Expiration
2043-09-15

AI Technical Summary

Technical Problem

Existing diamond logic integrated devices lack normally closed enhancement-mode devices, the integration scheme is immature, the carrier mobility is low, the dielectric layer quality affects the device performance, and the process compatibility is poor.

Method used

High-quality single-crystal diamond growth, photolithography masking, silicon film deposition, ICP-RIE etching, and diamond hydrogenation techniques are used to fabricate hydrogen- and silicon-terminated diamond logic integrated devices on high-quality single-crystal diamond. Through localized terminal diamond semiconductor processes, combined with depletion-mode and enhancement-mode device characteristics, channels with high mobility and low interface state density are formed.

Benefits of technology

A diamond semiconductor logic integrated device with high mobility and low interface state density has been realized, which has high stability and logic function and is suitable for the fabrication of diamond semiconductor logic circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117238757B_ABST
    Figure CN117238757B_ABST
Patent Text Reader

Abstract

A method for fabricating diamond logic integrated devices belongs to the field of semiconductor electronic device fabrication. The process steps are as follows: a. Processing and growth of an undoped diamond substrate; b. Polishing, acid washing, and ultrasonic cleaning of the epitaxially grown undoped diamond layer, followed by ozone ultraviolet irradiation to form an oxygen-terminated diamond surface; c. Photolithography, Ti / Au mask deposition, vacuuming, and room temperature Si film deposition; d. In-situ vacuum high-temperature annealing, and inductively coupled plasma-reactive ion etching; e. Ti / Au mask stripping, cleaning, and diamond surface hydrogenation; f. Photolithography, source and drain deposition, and device isolation using oxygen plasma; g. Deposition of gate oxide to complete the fabrication of the diamond logic integrated device. This invention utilizes high-quality single-crystal diamond growth, photolithography mask processing, silicon film deposition, inductively coupled plasma etching, and diamond hydrogenation techniques to efficiently and conveniently preserve the channel performance of the diamond interface, thus realizing the fabrication of diamond logic integrated devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention pertains to the field of semiconductor electronic device fabrication processes. It provides a method for fabricating diamond high-logic integrated devices on a high-quality single-crystal diamond surface using techniques such as high-quality single-crystal diamond growth, photolithography masking, silicon film deposition, ICP-RIE etching, and diamond hydrogenation. This invention effectively avoids interface problems present in other fabrication methods, achieving channels with high mobility and low interface state density, exhibiting high thermal stability. Furthermore, it provides an effective means for advancing diamond integrated logic circuit fabrication processes. Technical Background

[0002] With the development of the information society, semiconductor integration technology continues to shrink chip size along Moore's Law, leading to a bottleneck in the development of traditional semiconductor devices. These devices are no longer adequate for ultra-high frequency and ultra-high power information transmission, reception, and storage. In contrast, diamond is a promising semiconductor material due to its wide bandgap (5.5 eV), high carrier mobility, high breakdown electric field (>20 MV / cm), and high thermal conductivity, making it highly anticipated in next-generation high-frequency, high-power power electronic devices. However, the wide bandgap of intrinsic diamond presents a significant challenge: how to semiconductorize it and utilize it effectively. To address this, researchers have discovered that appropriate surface modification of diamond can generate two-dimensional hole gas (2DHG), providing an effective method for the development of diamond electronic power devices.

[0003] Through methods such as hydrogenation or plasma modification of the diamond surface, a high-density 2DHG channel can be generated on the diamond subsurface. Hydrogen-terminated diamond metal-oxide field-effect transistors (MOSFETs) prepared in this way exhibit depletion characteristics. Furthermore, by depositing an aluminum layer on the diamond surface at high temperature and then annealing and self-oxidizing to form an aluminum oxide gate oxide dielectric layer, the channel conductivity can be effectively controlled, achieving normal pinch-off operation and a high drain current density (Reference: "Wide temperature (10K-700K) and high voltage (~1000V) operation of CH diamondMOSFETs for power electronics application", IEEE International ElectronDevices Meeting. San Francisco, CA, USA. IEEE, 2015: 11.2.1-11.2.4).

[0004] Currently, diamond logic integrated devices mainly lack normally closed enhancement-mode devices. The main fabrication methods for enhancement-mode devices include local modification of hydrogen-terminated diamond (IEEE Electron Device Letters, 2017, 38(3):363-366), modulation of different types of dielectric layers (IEEE Electron Device Letters, 2017, 38(7):922-925; Applied Physics Letters, 2013, 103(9):092905), and impurity compensation methods (Advanced Electronic Materials. 2023, 2201122). The fabrication of diamond logic integrated circuits mainly relies on modulation of different types of dielectric layers (IEEE Electron Device Letters, 2017, 38(7):922-925), but its integration scheme is not mature, its process compatibility is poor, its carrier mobility is low, and the quality of the dielectric layer significantly affects the overall performance of the device. Summary of the Invention

[0005] To address the aforementioned problems in the fabrication of traditional diamond semiconductor logic integrated devices, this invention proposes a method for fabricating hydrogen- and silicon-terminated diamond logic integrated devices on high-quality single-crystal diamond using techniques such as high-quality single-crystal diamond growth, photolithography masking, silicon film deposition, ICP-RIE etching, and diamond hydrogenation. This invention effectively avoids interface problems present in other fabrication methods, achieving channels with high mobility and low interface state density. Its aim is to achieve terminal integration on high-quality diamond through a localized diamond semiconductor fabrication process, utilizing its depletion-mode and enhancement-mode device characteristics to form diamond semiconductor logic integrated devices with high channel carrier mobility, low interface state density, and high stability.

[0006] A method for fabricating diamond logic integrated devices is characterized by using high-quality undoped diamond as a foundation, and employing techniques such as high-quality single-crystal diamond growth, photolithography masking, silicon film deposition, inductively coupled plasma-reactive ion etching (ICP-RIE), and diamond hydrogenation to fabricate diamond high-logic integrated devices on high-quality single-crystal diamond. This method is efficient and convenient, effectively avoiding interface problems present in other fabrication methods, obtaining channels with high mobility and low interface state density, and utilizing its depletion-mode and enhancement-mode device characteristics to realize the logic functions of diamond semiconductors, forming NOR gate characteristics, exhibiting high thermal stability, and providing a foundation for the fabrication of diamond semiconductor logic circuits. The method specifically includes the following steps:

[0007] Step 1: Deposition and growth of undoped diamond

[0008] 1.1 Pretreatment of diamond substrate: A high-quality diamond film is used as the substrate. First, it is polished. Then, it is ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10-20 minutes respectively and dried to remove metal impurity particles and diamond powder generated during polishing.

[0009] 1.2 Growth of undoped diamond: After the substrate is processed, undoped diamond film is deposited and grown by microwave plasma chemical vapor deposition.

[0010] Step 2: Treatment of undoped diamond epitaxy

[0011] 2.1 Surface treatment of undoped diamond grown epitaxially: After the undoped diamond layer is grown epitaxially on the diamond substrate, the sample is polished and heated in sulfuric acid / nitric acid solution to remove non-carbon crystals and impurities on the diamond surface. Then, it is ultrasonically cleaned with acetone, anhydrous ethanol and deionized water respectively and dried.

[0012] 2.2 Ozone UV irradiation: The cleaned and dried diamond sample was irradiated with ultraviolet light in an ozone atmosphere to form oxygen-terminated diamond surface. Oxygen termination helps to improve the adhesion to Si atomic layer and Ti / Au mask.

[0013] Step 3: Photolithography deposition of Ti / Au mask.

[0014] 3.1 Photoresist spin coating and development: Positive photoresist spin coating is used. The rotation speed is set, and after the sample is uniformly coated by spinning, it is baked in an oven to remove solvent and moisture and improve the adhesion between the photoresist and the diamond surface. Then, the photomask is aligned with the sample surface and exposed and developed by ultraviolet light to obtain the pattern of Ti / Au mask.

[0015] 3.2 Etching and Resist Removal: Immediately after exposure and development, the photoresist is heated for hardening treatment to enhance the adhesion between the photoresist and diamond and improve the photoresist's resistance to etching. Then, the photoresist is removed by immersion in photoresist stripping solution, leaving the Ti / Au mask deposition area.

[0016] 3.3 Ti / Au mask deposition and photoresist stripping: Ti and Au layers were deposited on the diamond surface after photolithography using vacuum electron beam evaporation. Then, the photoresist was stripped by immersing the diamond in tetrahydrofuran solution for 30-40 minutes, leaving the silicon-terminated diamond preparation area.

[0017] Step 4: Introduction of Silicon Terminals

[0018] 4.1 Magnetron sputtering deposition of silicon layer: After photoresist stripping, surface cleaning is performed, and a Si film is deposited using magnetron sputtering; First, the magnetron sputtering chamber is evacuated and heated in a high vacuum environment to desorb impurities and some oxygen adsorbed on the surface of the oxygen-rich diamond; then, the temperature is lowered to room temperature, and a Si film is deposited using magnetron sputtering.

[0019] 4.2 High-temperature in-situ annealing: After the silicon film is deposited, in-situ annealing is performed; after the Si layer is deposited on the diamond surface, the vacuum degree is maintained and in-situ annealing is performed by heating. The oxygen atoms on the oxygen-terminated diamond surface are replaced by silicon atoms, and carbon-silicon bonding is completed.

[0020] 4.3I CP-RI E etching: Etching the SiO2 on the deposited surface removes the thick SiO2 layer on the surface of the silicon-terminated diamond, leaving a silicon atom layer on the diamond surface;

[0021] Step 5: Hydrogen terminal introduction

[0022] 5.1Ti / Au mask removal: The sample was placed in a sulfuric acid / nitric acid (3:1) solution and heated to remove the Ti / Au mask. Then, it was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water respectively and dried to prevent TiC residue.

[0023] 5.2 Hydrogenation of diamond surface: After mask removal, cleaning and drying, hydrogen termination is introduced by MPCVD hydrogen plasma;

[0024] Step 6: Source / drain electrode fabrication and device isolation

[0025] 6.1 Photoresist spin coating, development, and stripping: Positive photoresist spin coating is used. After setting the rotation speed and spinning to evenly coat the sample, the sample is baked in an oven. Then, the photomask is aligned with the sample surface, and the photoresist is exposed and developed by ultraviolet light to obtain the electrode deposition pattern. Then, hardening treatment is performed by soaking in photoresist stripping solution to remove the photoresist from the surface, leaving the Ti / Pt / Au electrode deposition area.

[0026] 6.2 Ti / Pt / Au electrode deposition: Ti, Pt, and Au layers were deposited on the diamond surface after photolithography using vacuum electron beam evaporation. After deposition, the surface was annealed and then immersed in tetrahydrofuran solution to remove the photoresist.

[0027] 6.3 Device isolation: Photolithography is used to protect the active region and the channel region with photoresist; then the sample is subjected to oxygen plasma treatment to form oxygen terminals on the diamond surface in addition to the photoresist-protected area, thus completing device isolation;

[0028] Step 7: Gate Deposition Annealing

[0029] The isolated diamond sample was immersed in acetone to remove the photoresist; then, an Al film was deposited at 450°C using ALD and annealed to complete the fabrication of hydrogen- and silicon-terminated diamond logic integrated devices.

[0030] Furthermore, in the undoped diamond deposition process described in step 1.2, the vacuum level is first reduced to below 1 Pa using a mechanical pump, and then the vacuum level in the reaction chamber is evacuated to 10 Pa using a molecular pump. -3 To ensure the cleanliness of the chamber, the Pa level is kept below 100 Pa, thereby reducing the impact of impurities on the growth of undoped diamond and promoting the preparation of high-quality diamond.

[0031] Further, the undoped diamond deposition growth process described in step 1.3 is as follows: the flow rates of hydrogen, methane, and carbon dioxide are set to 200-500, 2-4, and 2-4 sccm, respectively; the reaction chamber pressure is 5-9 kPa; the growth temperature is 550-850℃; the microwave power is 800-1600 W; the growth time is 10-15 h; and the growth thickness is 2-5 μm.

[0032] Furthermore, the specific operation of ozone ultraviolet irradiation in step 2.2 is as follows: the treated diamond sample is irradiated with ultraviolet light in an ozone atmosphere for 2-4 hours to form an oxygen-terminated diamond surface.

[0033] Further, in step 3.1, the photoresist spin coating and development is carried out by using positive photoresist spin coating at a speed of 3000-4000 r / min. After spinning and homogenizing the photoresist for 2-4 min, the sample is baked in an oven at 80-100℃ for 3-4 min to remove solvent and moisture and improve the adhesion between the photoresist and the diamond surface.

[0034] Furthermore, the specific process parameters for the magnetron sputtering deposition of the Si film in step 4.1 are as follows: the vacuum level of the magnetron sputtering chamber is evacuated to 10... -4 Below Pa, heat to 450-550℃ in a high vacuum environment for high-temperature annealing for 3-5 hours; then, cool to room temperature and deposit Si film using magnetron sputtering with RF power of 75-95W, pulse bias of 100V, cavity pressure of 0.5-0.8Pa, sputtering time of 2-4min, and sputtered Si film thickness of 15-45nm.

[0035] Furthermore, the specific process parameters for forming the silicon-terminated diamond in step 4.2 are as follows: maintain its 10 -4 Under a vacuum of less than Pa, the diamond is heated to 850-950℃ for in-situ annealing for 3-4 hours, and the thick SiO2 layer is etched with ICP-RI E to form a silicon atom layer on the diamond surface.

[0036] Furthermore, the specific process parameters for introducing hydrogen terminals through hydrogenation on the diamond surface in step 5.2 are as follows: microwave power: 60-80W, H2 flow rate: 90-110sccm, hydrogenation temperature: 500-700℃, and time: 25-45min.

[0037] Furthermore, in the fabrication method of the diamond logic integrated device, the Al film deposition can be replaced by other materials suitable for magnetron sputtering and conforming to the dielectric layer structure.

[0038] The key to implementing this invention lies in:

[0039] 1. To ensure the quality of undoped diamond growth and the excellent performance of the fabricated devices, a high-quality diamond substrate is used and mirror polished. Then, it is ultrasonically cleaned for 20-30 minutes each with acetone, anhydrous ethanol and deionized water and dried to remove metal impurity particles and diamond powder generated during polishing, ensuring the cleanliness of the growth substrate.

[0040] 2. Undoped diamond is deposited and grown using a high-quality diamond substrate, which has a low defect density and impurity concentration. This ensures the growth quality of single-crystal diamond and provides a foundation for performance development in subsequent device fabrication processes.

[0041] 3. To ensure high-quality growth of undoped diamond, a molecular pump was used to reduce the chamber vacuum to 10. -3 At a pressure of Pa, a high vacuum is maintained to remove impurities and contaminants from the preparation of undoped diamond and finished diamond.

[0042] 4. Undoped diamond was deposited and grown on high-quality diamond substrates using microwave plasma technology and homoepitaxial growth. The diamond deposition rate was 0.1-4 μm / h, and the growth temperature was 550-850℃. The deposition rate increased with increasing temperature, but excessively high temperatures led to pyramidal morphology in the diamond growth, reducing the surface quality of the single-crystal diamond. Lower growth temperatures resulted in pits and a rough surface on the single-crystal diamond growth surface, which was detrimental to the preparation of silicon-terminated diamonds.

[0043] 5. After cleaning and drying the grown undoped diamond sample, it is irradiated with ultraviolet light in an ozone atmosphere for 2-4 hours to form an oxygen-terminated diamond surface. The preparation of oxygen-terminated diamond helps to improve the bonding force with the Ti / Au mask and Si atomic layer, and greatly improves the channel quality of the diamond surface.

[0044] 6. After exposure and development, the photoresist is immediately heated at 120-180℃ for 20-30 minutes to perform a hardening treatment, which enhances the adhesion between the photoresist and diamond and improves the photoresist's resistance to etching.

[0045] 7. Before performing magnetron sputtering, use a molecular pump to evacuate the magnetron sputtering chamber to a vacuum level of 10. -4 Below Pa, the diamond is heated to 450-550℃ in a high vacuum environment for high-temperature annealing for 3-5 hours to desorb impurities and some oxygen from the surface of the diamond, avoid contamination during sputtering, and ensure the quality of the silicon-terminated diamond interface.

[0046] 8. After Si film deposition, maintain the vacuum level and heat to 850-950℃ for in-situ annealing for 3-4 hours. The high-temperature environment induces bonding between Si and C atoms on the sample surface, and the vacuum environment prevents graphitization of the sample during heating. Oxygen atoms on the oxygen-terminated diamond surface are replaced by Si atoms, completing the preparation of silicon-terminated diamond. Furthermore, it is thinned using ICP-RIE etching with the following parameters: ICP: 500W, RIE: 12W, etching time 2.5-3.5 min.

[0047] 9. After the diamond hydrogenation is completed, the chamber temperature is reduced to room temperature while maintaining the vacuum. An Al film with a thickness of about 95-125 nm is deposited at 250-350℃ using the ALD method, and then annealed at 350-550℃ for 2-3 hours. The deposited Al has strong bonding force and high density, and through the self-oxidation of Al, an Al2O3 dielectric layer structure is formed.

[0048] The beneficial effects of this invention and the prior art are as follows:

[0049] 1. This invention prepares high-quality undoped single-crystal diamond by microwave plasma method and diamond homoepitaxial method. Due to the surface characteristics of high-quality diamond, the silicon-terminated diamond prepared in this way has high dipole density and high hole carrier concentration, which enhances the overall performance of silicon-terminated diamond semiconductor.

[0050] 2. In this invention, high-quality single-crystal diamond surfaces are irradiated with ultraviolet light in an ozone atmosphere for 2-4 hours to form oxygen-terminated diamond surfaces. The preparation of oxygen-terminated diamond helps to improve the bonding force with the Si atomic layer, increase the bonding density of the silicon-terminated diamond surface, and improve the channel quality of the silicon-terminated diamond.

[0051] 3. This invention combines photolithography masking technology to deposit masks and electrodes on the diamond surface, thereby enabling the localized preparation of hydrogen-terminated and silicon-terminated diamonds, ensuring the quality of the diamond surface and the terminal integration performance during the preparation process.

[0052] 4. This invention employs ICP-RIE etching technology to deposit a Si atomic layer on the diamond surface, followed by thinning treatment. ICP-RIE etching has advantages such as high etching rate, high selectivity, and low damage, thereby avoiding the problems existing in other fabrication methods and obtaining high-performance diamond integrated circuits. Attached Figure Description

[0053] To more clearly illustrate the preparation technology of the present invention, the accompanying drawings used in the implementation process will be briefly introduced below. The accompanying drawings are only a brief introduction to the present invention.

[0054] Figure 1This is a process flow diagram for the fabrication of a hydrogen- and silicon-terminated diamond logic integrated device.

[0055] Figure 2 This is a schematic diagram of a hydrogen-silicon terminal diamond logic integrated device. Detailed Implementation

[0056] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0057] A fabrication process flow diagram of a hydrogen- and silicon-terminated integrated diamond semiconductor with an alumina dielectric layer structure is shown below. Figure 1 As shown, the process mainly includes the growth of undoped diamond, epitaxial undoped diamond treatment, photolithography mask deposition, silicon film deposition, ICP-RIE etching, mask lift-off and cleaning, diamond hydrogenation, and the fabrication of an alumina dielectric layer. The main idea is to grow high-quality undoped single-crystal diamond using a high-quality diamond growth process, then perform Ti / Au mask deposition using photolithography to locally fabricate silicon and hydrogen terminals. Finally, a Si film is deposited on the diamond using the ALD method, followed by ICP-RIE etching and annealing to deposit an Al film. This avoids a series of performance defects caused by interface state issues in the fabrication of diamond logic integrated devices, resulting in high-quality diamond integrated circuits.

[0058] Example 1

[0059] A (110) Ib type diamond sheet was selected as the substrate, polished, and then ultrasonically cleaned for 15 min each with acetone, anhydrous ethanol, and deionized water, and dried. Subsequently, the pretreated diamond substrate was placed in a microwave chemical vapor deposition apparatus for the deposition and growth of an undoped intrinsic diamond film. First, a vacuum pump was used to evacuate the reaction chamber, reducing its vacuum level to below 6 Pa. Then, a molecular pump was used to evacuate the reaction chamber to 10 Pa. -3Below Pa, the molecular pump was turned off, and undoped diamond films were grown via microwave plasma chemical vapor deposition. The flow rates of hydrogen, methane, and carbon dioxide were set to 150, 4, and 3 sccm, respectively. The reaction chamber pressure was 6 kPa, the growth temperature was 850 °C, the microwave power was 1500 W, the growth time was 13 h, and the growth thickness was 4 μm. After epitaxial growth of the undoped diamond layer on the diamond substrate, the sample was polished and heated in a sulfuric acid / nitric acid (3:1) solution for 40 min. Then, it was ultrasonically cleaned for 20 min each with acetone, anhydrous ethanol, and deionized water, and dried. The cleaned and dried diamond sample was irradiated with ultraviolet light in an ozone atmosphere for 3 h to form an oxygen-terminated diamond surface. Then, positive photoresist spin coating was performed at 3000 r / min for 4 min, followed by baking in a 90 °C oven for 4 min to remove solvent and moisture. Finally, a photomask was aligned with the sample surface and exposed and developed by UV irradiation to obtain the Ti / Au mask pattern. After exposure and development, the photoresist is immediately heated at 150°C for 25 minutes for hardening. Then, it is immersed in photoresist stripping solution for 30 minutes to remove the photoresist from the surface, leaving the Ti / Au mask deposition area. Ti and Au layers are then deposited on the photolithographically etched diamond surface using vacuum electron beam evaporation at a vacuum level of 10. -6 The deposition temperature was 800℃, and the deposition time was 15 min, resulting in a thickness of 85 nm. After deposition, the photoresist was stripped by immersion in tetrahydrofuran solution for 40 min. After photoresist stripping, the sample was cleaned with acetone, anhydrous ethanol, and deionized water for 20 min each. Then, the vacuum level in the magnetron sputtering chamber was evacuated to 1000 nm using a vacuum pump. -4Below Pa, the silicon film was heated to 500℃ in a high vacuum environment for high-temperature annealing for 4 hours, then cooled to room temperature. A silicon film was deposited using magnetron sputtering with an RF power of 85W, a pulse bias of 100V, a cavity pressure of 0.7Pa, and a sputtering time of 3 minutes, resulting in a silicon film thickness of 35nm. After silicon film deposition, the vacuum level was maintained, and the film was heated to 950℃ for in-situ annealing for 4 hours to complete the diamond-silicon carbide bonding. Subsequently, ICP-RIE etching was performed for 3 minutes in an ICP-RIE etching system with 500W ICP and 12W RIE to remove the thick SiO2 layer on the silicon-terminated diamond surface. The sample was removed and heated in a sulfuric acid / nitric acid (3:1) solution for 30 min to remove the Ti / Au mask. It was then ultrasonically cleaned for 25 min each with acetone, anhydrous ethanol, and deionized water, and dried. Next, it was placed in an MPCVD chamber to introduce hydrogen termination. The parameters were set as follows: microwave power: 70 W, H2 flow rate: 110 sccm, hydrogenation temperature: 600℃, and time: 30 min. Photoresist was then spin-coated again, followed by exposure and development to remove the photoresist and leave the Ti / Pt / Au deposition sites. Ti, Pt, and Au layers were then deposited on the photolithographically etched diamond surface using vacuum electron beam evaporation (PEBE) at a vacuum level of 10. -6 The deposition temperature was 800℃, and the deposition time was 15 min, with thicknesses of 20, 30, and 100 nm, respectively. After deposition, the photoresist was stripped by immersion in tetrahydrofuran solution for 40 min. After stripping, the active and channel regions were covered by photoresist spin coating. The active and channel regions were then modified by oxygen plasma treatment for 8 min using MPCVD at a pressure of 4 kPa, a temperature of 500℃, and a microwave power of 900 W for 8 min, followed by oxygen termination isolation. The photoresist was then stripped by immersion in acetone for 10 min. An Al film was then deposited using ALD at 300℃ with a thickness of approximately 110 nm, followed by annealing at 400℃ for 2 h. This completed the fabrication of hydrogen- and silicon-terminated diamond logic integrated devices. The diamond logic circuit fabricated in this manner clearly exhibited inverting characteristics, and its threshold voltage V0 was [not specified]. TH With voltages of 5.3V and -5.0V respectively, and a maximum gain of 25.1, diamond logic circuits exhibit NOR gate characteristics.

[0060] Example 2

[0061] A (110) Ib type diamond sheet was selected as the substrate, polished, and then ultrasonically cleaned for 15 min each with acetone, anhydrous ethanol, and deionized water, and dried. Subsequently, the pretreated diamond substrate was placed in a microwave chemical vapor deposition apparatus for the deposition and growth of an undoped intrinsic diamond film. First, a vacuum pump was used to evacuate the reaction chamber, reducing its vacuum level to below 6 Pa. Then, a molecular pump was used to evacuate the reaction chamber to 10 Pa. -3Below Pa, the molecular pump was turned off, and undoped diamond films were grown via microwave plasma chemical vapor deposition. The flow rates of hydrogen, methane, and carbon dioxide were set to 300, 4, and 3 sccm, respectively. The reaction chamber pressure was 6 kPa, the growth temperature was 850 °C, the microwave power was 1500 W, the growth time was 14 h, and the growth thickness was 5 μm. After epitaxial growth of the undoped diamond layer on the diamond substrate, the sample was polished and heated in a sulfuric acid / nitric acid (3:1) solution for 40 min. Then, it was ultrasonically cleaned for 20 min each with acetone, anhydrous ethanol, and deionized water, and dried. The cleaned and dried diamond sample was irradiated with ultraviolet light in an ozone atmosphere for 3 h to form an oxygen-terminated diamond surface. Then, positive photoresist spin coating was performed at a speed of 4000 r / min for 3 min, followed by baking in a 90 °C oven for 4 min to remove solvent and moisture. Finally, a photomask was aligned with the sample surface and exposed and developed by UV irradiation to obtain the Ti / Au mask pattern. After exposure and development, the photoresist is immediately heated at 150°C for 25 minutes for hardening. Then, it is immersed in photoresist stripping solution for 30 minutes to remove the photoresist from the surface, leaving the Ti / Au mask deposition area. Ti and Au layers are then deposited on the photolithographically etched diamond surface using vacuum electron beam evaporation at a vacuum level of 10. -6 The deposition temperature was 850℃, and the deposition time was 20 min, resulting in a thickness of 90 nm. After deposition, the photoresist was stripped by immersion in tetrahydrofuran solution for 40 min. After photoresist stripping, the sample was cleaned with acetone, anhydrous ethanol, and deionized water for 20 min each. Then, the vacuum level in the magnetron sputtering chamber was evacuated to 1000 nm using a vacuum pump. -4Below Pa, the silicon film was heated to 500℃ in a high vacuum environment for high-temperature annealing for 4 hours, then cooled to room temperature. A silicon film was deposited using magnetron sputtering with an RF power of 90W, a pulse bias of 100V, a cavity pressure of 0.7Pa, and a sputtering time of 4 minutes, resulting in a silicon film thickness of 40nm. After silicon film deposition, the vacuum level was maintained, and the film was heated to 950℃ for in-situ annealing for 4 hours to complete the diamond-silicon carbide bonding. Subsequently, ICP-RIE etching was performed for 3 minutes in an ICP-RIE etching system with 500W ICP and 12W RIE to remove the thick SiO2 layer on the silicon-terminated diamond surface. The sample was removed and heated in a sulfuric acid / nitric acid (3:1) solution for 30 min to remove the Ti / Au mask. It was then ultrasonically cleaned for 25 min each with acetone, anhydrous ethanol, and deionized water, and dried. Next, it was placed in an MPCVD chamber to introduce hydrogen termination. The parameters were set as follows: microwave power: 80 W, H2 flow rate: 100 sccm, hydrogenation temperature: 600℃, and time: 30 min. Photoresist was then spin-coated again, followed by exposure and development to remove the photoresist and leave the Ti / Pt / Au deposition sites. Ti, Pt, and Au layers were then deposited on the photolithographically etched diamond surface using vacuum electron beam evaporation (PEBE) at a vacuum level of 10. -6 The deposition temperature was 800℃, and the deposition time was 15 min, with thicknesses of 20, 30, and 100 nm, respectively. After deposition, the photoresist was stripped by immersion in tetrahydrofuran solution for 40 min. After stripping, the active and channel regions were covered by photoresist spin coating. The active and channel regions were then modified by oxygen plasma treatment for 8 min using MPCVD at a pressure of 4 kPa, a temperature of 500℃, and a microwave power of 900 W for 8 min, followed by oxygen termination isolation. The photoresist was then stripped by immersion in acetone for 10 min. An Al film was then deposited using ALD at 300℃ with a thickness of approximately 110 nm, followed by annealing at 400℃ for 2 h. This completed the fabrication of hydrogen- and silicon-terminated diamond logic integrated devices. The diamond logic circuit fabricated in this manner clearly exhibited inverting characteristics, and its threshold voltage V0 was [not specified]. TH With voltages of 5.4V and -5.1V respectively, and a maximum gain of 25.2, diamond logic circuits exhibit NOR gate characteristics.

Claims

1. A method for fabricating a diamond logic integrated device, characterized by using high-quality undoped diamond as a basis, and fabricating the diamond logic integrated device on high-quality single-crystal diamond through high-quality single-crystal diamond growth, photolithography masking, silicon film deposition, inductively coupled plasma-reactive ion etching, and diamond hydrogenation technology; specifically including the following steps: Step 1: Deposition and growth of undoped diamond 1.1 Pretreatment of diamond substrate: A high-quality diamond film is used as the substrate. First, it is polished. Then, it is ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 10-20 minutes respectively and dried to remove metal impurity particles and diamond powder generated during polishing. 1.2 Growth of undoped diamond: After the substrate is processed, undoped diamond film is deposited and grown by microwave plasma chemical vapor deposition. Step 2: Treatment of undoped diamond epitaxy 2.1 Surface treatment of undoped diamond grown epitaxially: After the undoped diamond layer is grown epitaxially on the diamond substrate, the sample is polished and heated in sulfuric acid / nitric acid solution to remove non-carbon crystals and impurities on the diamond surface. Then, it is ultrasonically cleaned with acetone, anhydrous ethanol and deionized water respectively and dried. 2.2 Ozone UV irradiation: The cleaned and dried diamond sample was irradiated with ultraviolet light in an ozone atmosphere to form oxygen-terminated diamond surface. Oxygen termination helps to improve the adhesion to Si atomic layer and Ti / Au mask. Step 3: Photolithography deposition of Ti / Au mask. 3.1 Photoresist spin coating and development: Positive photoresist spin coating is used. The rotation speed is set, and after the photoresist is uniformly coated by spinning, the sample is baked in an oven to remove solvent and moisture and improve the adhesion between the photoresist and the diamond surface. Then, the photomask is aligned with the sample surface and exposed and developed by ultraviolet light to obtain the pattern of the Ti / Au mask; 3.2 Etching and Resin Removal: After exposure and development, the photoresist is immediately heated for hardening treatment to enhance the adhesion between the photoresist and diamond and improve the photoresist's resistance to etching. Then, the surface photoresist is removed by soaking in a photoresist stripping solution, leaving the Ti / Au mask deposition area. 3.3 Ti / Au mask deposition and photoresist stripping: Ti and Au layers were deposited on the diamond surface after photolithography using vacuum electron beam evaporation. Then, the photoresist was stripped by immersing the surface in tetrahydrofuran solution for 30-40 minutes, leaving the Ti / Au mask-covered area. Step 4: Introduction of Silicon Terminals 4.1 Magnetron sputtering deposition of silicon layer: After photoresist stripping, surface cleaning is performed, and a Si film is deposited using magnetron sputtering; First, the magnetron sputtering chamber is evacuated and heated in a high vacuum environment to desorb impurities and some oxygen adsorbed on the surface of the oxygen-rich diamond; then, the temperature is lowered to room temperature, and a Si film is deposited using magnetron sputtering. 4.2 High-temperature in-situ annealing: After the silicon film is deposited, in-situ annealing is performed; after the Si layer is deposited on the diamond surface, the vacuum degree is maintained and in-situ annealing is performed by heating. The oxygen atoms on the oxygen-terminated diamond surface are replaced by silicon atoms, and carbon-silicon bonding is completed. 4.3 ICP-RIE etching: Etching the SiO2 on the deposited surface removes the thick SiO2 layer on the surface of the silicon-terminated diamond, leaving a silicon atom layer on the diamond surface; Step 5: Hydrogen terminal introduction 5.1Ti / Au mask removal: The sample was placed in a sulfuric acid / nitric acid solution with a volume ratio of 3:1 and heated to remove the Ti / Au mask. Then, it was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water respectively and dried to prevent TiC residue. 5.2 Hydrogenation of diamond surface: After mask removal, cleaning and drying, hydrogen termination is introduced by MPCVD hydrogen plasma; Step 6: Source / drain electrode fabrication and device isolation 6.1 Photoresist spin coating, development and stripping: Positive photoresist spin coating is used. The rotation speed is set, and after the sample is uniformly coated by spinning, it is baked in an oven. Then, the photomask is aligned with the sample surface, and the photoresist is exposed and developed by ultraviolet light to obtain the electrode deposition pattern; Then, a hard film treatment is performed by soaking the surface in a photoresist stripping solution to remove the photoresist, leaving the Ti / Pt / Au electrode deposition area. 6.2 Ti / Pt / Au electrode deposition: Ti, Pt, and Au layers were deposited on the diamond surface after photolithography using vacuum electron beam evaporation. After deposition, the surface was annealed and then immersed in tetrahydrofuran solution to remove the photoresist. 6.3 Device isolation: Photolithography is used to protect the active region and the channel region with photoresist; then the sample is subjected to oxygen plasma treatment to form oxygen terminals on the diamond surface in addition to the photoresist-protected area, thus completing device isolation; Step 7: Gate Deposition Annealing The isolated diamond sample was immersed in acetone to remove the photoresist; then, an Al film was deposited at 450°C using ALD and annealed to complete the fabrication of hydrogen- and silicon-terminated diamond logic integrated devices.

2. The method of claim 1, wherein in the growing of the undoped diamond of step 1.2, a mechanical pump is first used to reduce the vacuum degree to below 1 Pa, and then a molecular pump is used to reduce the vacuum degree of the reaction chamber to below 10 Pa, so as to ensure the cleanliness of the chamber and reduce the influence of impurities on the growth of the undoped diamond and promote the preparation of high-quality diamond. -3 Pa, and then a molecular pump is used to reduce the vacuum degree of the reaction chamber to below 10 Pa, so as to ensure the cleanliness of the chamber and reduce the influence of impurities on the growth of the undoped diamond and promote the preparation of high-quality diamond.

3. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The undoped diamond growth process described in step 1.2 is as follows: the flow rates of hydrogen, methane, and carbon dioxide are set to 200-500, 2-4, and 2-4 sccm, respectively; the reaction chamber pressure is 5-9 kPa; the growth temperature is 550-850℃; the microwave power is 800-1600 W; the growth time is 10-15 h; and the growth thickness is 2-5 µm.

4. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The specific operation of ozone ultraviolet irradiation in step 2.2 is as follows: the treated diamond sample is irradiated with ultraviolet light in an ozone atmosphere for 2-4 hours to form an oxygen-terminated diamond surface.

5. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... Step 3.1 Photoresist spin coating and development: Use positive photoresist spin coating, set the rotation speed to 3000-4000 r / min, spin coat for 2-4 min, and then bake the sample in an 80-100℃ oven for 3-4 min to remove solvent and moisture and improve the adhesion between the photoresist and the diamond surface.

6. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The specific process parameters for magnetron sputtering deposition of Si film in step 4.1 are as follows: the vacuum level of the magnetron sputtering chamber is evacuated to 10. -4 Below Pa, heat to 450-550℃ in a high vacuum environment for high-temperature annealing for 3-5 hours; then, cool to room temperature and deposit Si film using magnetron sputtering with RF power of 75-95W, pulse bias of 100V, cavity pressure of 0.5-0.8Pa, sputtering time of 2-4min, and sputtered Si film thickness of 15-45nm.

7. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The specific process parameters for forming the silicon-terminated diamond in step 4.2 are as follows: maintain its 10 -4 Under a vacuum of less than Pa, the diamond is heated to 850-950℃ for in-situ annealing for 3-4 hours, and the thick SiO2 layer is etched by ICP-RIE to form a silicon atom layer on the diamond surface.

8. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The specific process parameters for introducing hydrogen terminals through hydrogenation on the diamond surface in step 5.2 are as follows: microwave power: 60-80W, H2 flow rate: 90-110sccm, hydrogenation temperature: 500-700℃, and time: 25-45min.

9. The method for fabricating the diamond logic integrated device according to claim 1, characterized in that... The deposition of the Al film in step 7 can be replaced by other materials suitable for magnetron sputtering and conforming to the dielectric layer structure.

Citation Information

Patent Citations

  • Array type diamond film and method for making the same

    CN102345169A

  • Method of preparing high-performance diamond semiconductor based on low-cost single crystal diamond

    CN107275192A