Water-oxygen barrier film and preparation method and application thereof
Patent Information
- Application Number
- CN202210629164.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-06
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-06-06
AI Technical Summary
文献中也有采用石墨烯作为阻隔层的研究,但主要通过真空方法沉积,不利于大面积制备
Smart Images

Figure CN117241593B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a water-oxygen barrier film, specifically to a water-oxygen barrier film prepared by solution method for packaging flexible electronic devices and its application, belonging to the field of flexible electronic device fabrication technology. Background Technology
[0002] With the rapid development of flexible electronics technologies such as organic photovoltaics (OPV), organic light-emitting diodes (OLED), organic thin-film transistors (OTFT), and printed radio frequency identification (RFID), flexible electronics technology is undergoing a technological revolution. Flexible electronics technology has broad application prospects in many fields, but the lifespan of devices remains one of the biggest challenges hindering its development. Among these challenges, water and oxygen corrosion in the environment is the most significant factor leading to performance degradation in flexible electronic devices.
[0003] To achieve high water and oxygen barrier properties, there are currently two main packaging solutions for flexible electronic devices. One is cover encapsulation, which uses adhesives to bond flexible, high-barrier commercial barrier films. The other is thin film encapsulation, which involves directly depositing a thin film with alternating organic and inorganic structures onto the flexible electronic device. In this case, the inorganic layer is mainly used to block water vapor and extend its path, while the organic layer is mainly used to interrupt defects in the inorganic layer and provide flexibility.
[0004] However, cover encapsulation requires high-quality adhesives, suffers from delamination, and is prone to lateral water vapor penetration. Furthermore, the weight of the high-barrier barrier film used is many times that of the flexible organic electronic device itself, limiting some potential applications. Thin-film encapsulation primarily employs vacuum deposition methods such as physical vapor deposition (PVD), plasma-enhanced chemical vapor deposition (PECVD), and atomic layer deposition (ALD) to prepare barrier films. Vacuum deposition methods are time-consuming and require stringent conditions, potentially damaging device performance and hindering large-area, low-cost encapsulation of flexible electronic devices. Lina Sun et al. proposed a solution-based low-temperature barrier film preparation method for OLED encapsulation, mainly using UV-converted PDMS and PHPS to prepare organic and inorganic multilayer barrier films. However, this method does not involve interlayer reactions and does not fully utilize the flexibility of the barrier film. Some studies in the literature have used graphene as a barrier layer, but these are mainly deposited using vacuum methods, which are not suitable for large-area fabrication. Summary of the Invention
[0005] The main objective of this invention is to provide a water-oxygen barrier membrane, its preparation method, and its application, in order to overcome the shortcomings of the prior art.
[0006] Another object of the present invention is to provide the application of the water-oxygen barrier membrane in the fabrication of flexible electronic devices.
[0007] To achieve the aforementioned objectives, the technical solution adopted by this invention includes:
[0008] This invention provides a method for preparing a water-oxygen barrier membrane, comprising:
[0009] (1) A first solution containing polysilazane is coated onto a flexible substrate or electronic device and cured;
[0010] (2) The second solution containing graphene oxide is coated onto the flexible substrate or electronic device obtained in step (1) and dried. Then, the first solution containing polysilazane is coated on and cured, so that the polysilazane is transformed into dense SiO2. x N y Simultaneously, the graphene oxide is reduced;
[0011] (3) Repeat steps (1) to (2) at least once to obtain a water-oxygen barrier membrane with a multi-layered structure.
[0012] In some embodiments, the preparation method includes: performing the curing using at least one of vacuum ultraviolet light, ammonia treatment, or heating.
[0013] This invention also provides a water-oxygen barrier membrane prepared by the aforementioned method, which comprises at least one SiO₂. x N y / Reduced graphene oxide composite stacked structure, where x and y are used to describe the elements contained in the barrier film.
[0014] This invention also provides the application of the water-oxygen barrier membrane in the fabrication of electronic devices.
[0015] Accordingly, embodiments of the present invention also provide an electronic device, including a barrier layer comprising the aforementioned water and oxygen barrier film.
[0016] Compared with existing technologies, the method for preparing water-oxygen barrier membranes provided by this invention has good repeatability, simple preparation process, and effectively avoids damage to devices caused by solvents and high temperatures during preparation. The prepared water-oxygen barrier membrane has advantages such as high transparency, high flexibility and high water-oxygen barrier properties, and has good application prospects in the field of electronic devices. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a schematic diagram illustrating the preparation of a barrier film and its application in electronic devices in a typical embodiment of the present invention. Detailed Implementation
[0019] In view of the shortcomings of existing technologies, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention. Its main feature is the selection of polysilazane and graphene oxide as barrier layers, and the preparation of a water-oxygen barrier film via a solution method. The following will further explain and illustrate this technical solution, its implementation process, and its principles.
[0020] One aspect of this invention provides a method for preparing a water-oxygen barrier membrane, comprising:
[0021] (1) A first solution containing polysilazane is coated onto a flexible substrate or electronic device and cured;
[0022] (2) The second solution containing graphene oxide is coated onto the flexible substrate or electronic device obtained in step (1) and dried. Then, the first solution containing polysilazane is coated on and cured, so that the polysilazane is transformed into dense SiO2. x N y Simultaneously, the graphene oxide is reduced;
[0023] (3) Repeat steps (1) to (2) at least once to obtain a water-oxygen barrier membrane with a multi-layered structure.
[0024] In some embodiments, in step (1), the polysilazane includes perhydropolysilazane and / or organopolysilazane, preferably a polymer with Si-N as the main chain, but not limited thereto.
[0025] In some embodiments, the preparation method includes coating the first solution containing polysilazane onto a flexible substrate or electronic device using at least one of spin coating, blade coating, or slot coating.
[0026] In some embodiments, the preparation method includes curing using at least one of vacuum ultraviolet light, ammonia treatment, or heating. Vacuum ultraviolet light curing is preferred as it accelerates the reduction of graphene oxide. Vacuum ultraviolet light generally refers to ultraviolet light with wavelengths below 200 nm. The vacuum ultraviolet conversion of this invention can be performed in nitrogen or air.
[0027] The ammonia treatment specifically includes: placing the spin-coated polysilazane film in an ammonia vapor atmosphere for a time depending on the specific thickness, until the polysilazane is completely converted.
[0028] Furthermore, the heating temperature is generally above 180°C, and the time depends on the specific thickness, until the polysilazane is completely converted.
[0029] In some preferred embodiments, the present invention selects polysilazane and graphene oxide as the barrier layer, prepares the barrier film by solution method, and converts the polysilazane (perhydropolysilazane, organopolysilazane, etc.) into dense SiO2 by vacuum ultraviolet conversion. x N y Graphene oxide was reduced using vacuum ultraviolet light and polysilazane. Please refer to [link / reference]. Figure 1 As shown, the specific preparation steps of the water-oxygen barrier membrane (also referred to as "water-oxygen barrier film") can be as follows:
[0030] 1. A certain concentration of polysilazane is coated onto a flexible substrate or electronic device by means of spin coating, blade coating or slot coating, and cured by means of vacuum ultraviolet or ammonia treatment or heating;
[0031] 2. After coating with a certain concentration of graphene oxide and drying, a certain concentration of polysilazane is then coated onto a flexible substrate or electronic device to form a structure such as... Figure 1 The polysilazane / graphene oxide stacked structure shown is cured by methods such as vacuum ultraviolet light, ammonia treatment, or heating, wherein vacuum ultraviolet light can accelerate the reduction of graphene oxide.
[0032] 3. Repeat the above steps to prepare a water-oxygen barrier membrane with a multi-layered structure.
[0033] The preparation mechanism of this invention may lie in the following: It cleverly utilizes the reaction between polysilazane and graphene oxide (GO) to directly form r-GO, thereby improving barrier properties. Simultaneously, it can also utilize vacuum ultraviolet light to accelerate the reaction between polysilazane and graphene oxide, converting polysilazane into SiO₂. x N y At the same time, it reduces graphene oxide and forms a strong bond at the interface between the two, which is beneficial for stress release and improved barrier properties.
[0034] Furthermore, the present invention also includes: firstly coating the device surface with an organic material, such as organosilicon, polyurethane, polyacrylate, epoxy resin, etc., as a buffer layer to provide flexibility and prevent solvent damage to the device.
[0035] In summary, the preparation process of this invention is simple, and the in-situ preparation will not damage the device; it has the advantages of good repeatability, high transparency of the obtained film, good flexibility, and high water and oxygen barrier properties, and effectively avoids damage to the device caused by solvents and high temperatures during the preparation process.
[0036] Another aspect of the present invention provides a water-oxygen barrier membrane prepared by the aforementioned preparation method, which comprises at least one SiO₂. x N y / Reduced graphene oxide (r-GO) composite stacked structure, where x and y are used to describe the elements contained in the barrier film.
[0037] Furthermore, the barrier layer prepared by the solution method in this invention exhibits high transparency, high flexibility, and high barrier properties. Specifically, the transparency of the water-oxygen barrier film is above 95%, and the water-oxygen barrier properties increase with the number of layers, with a minimum water vapor permeability of 10%. -3 g / m 2 For applications under / day, flexibility can be adjusted according to the ratio of organic to inorganic layers, depending on the specific flexibility requirements of the electronic device.
[0038] Another aspect of the present invention provides the application of the water-oxygen barrier membrane in the fabrication of electronic devices.
[0039] Accordingly, another aspect of the present invention provides an electronic device including a barrier layer comprising the aforementioned water and oxygen barrier film.
[0040] The invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the invention are disclosed herein; however, it should be understood that the disclosed embodiments are merely exemplary of the invention, which may be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims and as intended to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.
[0041] Example 1
[0042] For electronic devices requiring water and oxygen protection, in-situ encapsulation is performed by first coating the device surface with an organic material, such as silicone, polyurethane, polyacrylate, or epoxy resin, as a buffer layer to provide flexibility and prevent solvent damage. Then, a perhydropolysilazane solution is coated on top, dried at room temperature for 1 hour, and then converted to SiO2 by vacuum ultraviolet irradiation at 172 nm in nitrogen atmosphere. x An N-type barrier layer is then applied, followed by a coating of graphene oxide solution, which is then allowed to evaporate and dry at room temperature. This process is repeated until the polysilazane is converted into dense SiO₂. x N y Simultaneously, graphene oxide is reduced to prepare 2-3 layers for encapsulation. Testing shows that the prepared water-oxygen barrier film has a transparency of over 95% and a water vapor permeability of over 10%. -3 g / m 2 / day or less.
[0043] Example 2
[0044] For electronic devices requiring water and oxygen protection, in-situ encapsulation is performed by first coating the device surface with an organic material, such as silicone, polyurethane, polyacrylate, or epoxy resin, as a buffer layer to provide flexibility and prevent solvent damage. Then, a perhydropolysilazane solution is coated on top, dried at room temperature for 1 hour, and then placed in ammonia vapor for 4 hours to convert it into SiO₂. x An N-layer barrier is then applied, followed by a coating of graphene oxide solution, which is then allowed to evaporate and dry at room temperature. The above steps are repeated to prepare 2-3 layers, completing the encapsulation process.
[0045] Example 3
[0046] For electronic devices requiring water and oxygen protection, in-situ encapsulation is performed by first coating the device surface with an organic material, such as silicone, polyurethane, polyacrylate, or epoxy resin, as a buffer layer to provide flexibility and prevent solvent damage. Then, a solution of perhydropolysilazane is coated on top and heated in air at above 180°C to convert it into SiO₂. x An N-layer barrier is then applied, followed by coating with a graphene oxide solution, which is then allowed to evaporate and dry. The above steps are repeated to prepare 2-3 layers, completing the encapsulation process.
[0047] Example 4
[0048] For electronic devices requiring water and oxygen protection, in-situ encapsulation is performed by first coating the device surface with an organic material, such as silicone, polyurethane, polyacrylate, or epoxy resin, as a buffer layer to provide flexibility and prevent solvent damage. Then, a perhydropolysilazane solution is coated on top, dried at room temperature for 1 hour, and then converted to SiO2 by vacuum ultraviolet irradiation at 172 nm wavelength in air. xAn N-layer barrier is then applied, followed by a coating of graphene oxide solution, which is then allowed to evaporate and dry at room temperature. The above steps are repeated to prepare 2-3 layers, completing the encapsulation process.
[0049] Example 5
[0050] A solution of all-hydrogen polysilazane was directly coated onto transparent flexible substrates such as PET, PEN, CPI, and PVA. After drying at room temperature for 1 hour, it was converted into SiO by vacuum ultraviolet irradiation at a wavelength of 172 nm in air. x An N-layer barrier is formed, followed by coating with a graphene oxide solution and drying at room temperature. The above steps are then repeated to prepare 2-3 layers, completing the fabrication of a transparent, flexible water-oxygen barrier membrane.
[0051] Example 6
[0052] A solution of all-hydrogen polysilazane was directly coated onto transparent flexible substrates such as PET, PEN, CPI, and PVA. After drying at room temperature for 1 hour, it was converted into SiO by vacuum ultraviolet irradiation at 172 nm wavelength in nitrogen atmosphere. x An N-layer barrier is formed, followed by coating with a graphene oxide solution and drying at room temperature. The above steps are then repeated to prepare 2-3 layers, completing the fabrication of a transparent, flexible water-oxygen barrier membrane.
[0053] Example 7
[0054] A solution of all-hydrogen polysilazane was directly coated onto transparent flexible substrates such as PET, PEN, CPI, and PVA. After evaporation at room temperature for 1 hour and drying, the substrate was placed in ammonia vapor for 4 hours to convert it into SiO2. x An N-layer barrier is formed, followed by coating with a graphene oxide solution and drying at room temperature. The above steps are then repeated to prepare 2-3 layers, completing the fabrication of a transparent, flexible water-oxygen barrier membrane.
[0055] Example 8
[0056] A fully hydrogenated polysilazane solution is directly coated onto transparent flexible substrates such as PET, PEN, CPI, and PVA, and then heated in air at temperatures above 180°C to convert it into SiO₂. x An N-layer barrier is formed, followed by coating with a graphene oxide solution and allowing it to evaporate and dry. The above steps are then repeated to prepare 2-3 layers, completing the fabrication of a transparent, flexible water-oxygen barrier membrane.
[0057] The all-hydrogenated polysilazane in the above embodiments can also be replaced with an organopolysilazane with Si-N as the main chain, achieving similar results. Furthermore, the test results of Examples 2-8 are essentially the same as those of Example 1.
[0058] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the described embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims.
Claims
1. A method for preparing a water-oxygen barrier membrane, characterized in that, include: First, an organic material selected from silicone, polyurethane, polyacrylate, and epoxy resin is directly coated onto the surface of the electronic device as a buffer layer. (1) A first solution containing perhydropolysilazane is coated onto an electronic device having the buffer layer and cured using vacuum ultraviolet light with a wavelength below 200 nm; (2) The second solution containing graphene oxide is coated onto the electronic device obtained in step (1) and dried. Then, the first solution containing perhydropolysilazane is coated onto the device, and then cured using vacuum ultraviolet light with a wavelength below 200 nm, so that the perhydropolysilazane is converted into dense SiO2. x N y Meanwhile, the graphene oxide is reduced in situ by the reducing substances generated during the conversion of the polysilazane, and no external graphene oxide reducing agent is added during the curing process. (3) Repeat steps (1) to (2) at least once to obtain a water-oxygen barrier membrane with a multi-layered structure.
2. The preparation method according to claim 1, characterized in that: The polysilazane comprises polymers with Si-N as the main chain.
3. The preparation method according to claim 1, characterized in that, include: The first solution containing perhydropolysilazane is coated onto the electronic device having the buffer layer using at least one of spin coating, blade coating, or slot coating.
4. A water-oxygen barrier membrane prepared by any one of claims 1-3, comprising at least one SiO₂. x N y The reduced graphene oxide composite laminate structure provides a water-oxygen barrier film with a transparency of over 95% and a water vapor permeability of over 10%. -3 g / m 2 / day or less.
5. The application of the water-oxygen barrier membrane according to claim 4 in the preparation of electronic devices.
6. An electronic device, comprising a barrier layer, characterized in that: The barrier layer comprises the water-oxygen barrier membrane as described in claim 4.
Citation Information
Patent Citations
Moisture transmission resistant coating composition comprising graphene oxide and silicon
KR1020140120557A