Method for manufacturing sintered body
By heat-treating the zirconia sintered body, the problem of excessively long sintering time under normal pressure was solved, achieving color consistency and meeting aesthetic requirements.
Patent Information
- Application Number
- CN202280031078.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-28
- Filing Date
- 2022-04-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-04-25
AI Technical Summary
Existing technologies require more than 5 hours for atmospheric pressure sintering, resulting in excessively long production times for zirconia sintered bodies containing coloring elements. Furthermore, the color tone differs from that of bodies sintered in shorter times, making it difficult to meet aesthetic requirements.
By heat-treating the zirconia sintered body containing coloring elements at temperatures above 600℃ and below 1200℃, combined with short-time atmospheric pressure sintering in an oxidizing atmosphere, the color tone is ensured to be consistent with that of the long-time sintered body.
It achieves the same color tone effect as long-time sintered bodies while shortening the sintering time, thus meeting aesthetic requirements.
Smart Images

Figure BDA0004514008380000231 
Figure BDA0004514008380000261 
Figure BDA0004514008380000271
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing a sintered body of zirconium oxide containing coloring elements, and more particularly to a method for manufacturing a sintered body of zirconium oxide containing coloring elements obtained by sintering under atmospheric pressure. Background Technology
[0002] Sintered bodies of zirconium oxide containing coloring elements are rapidly expanding beyond their existing applications, such as structural materials, into aesthetically pleasing applications, such as decorative parts for the exterior of portable electronic devices and dental materials for dental restorations.
[0003] From the perspective of ease of composition control and manufacturing cost, the manufacture of sintered bodies containing coloring elements of zirconia, except in cases of manufacturing difficulties, is carried out by a sintering method that involves heating to the sintering temperature (maximum reached temperature) under atmospheric atmosphere and atmospheric pressure, holding at that temperature for several hours, and then cooling to near room temperature, i.e., atmospheric pressure sintering (e.g., Patent Documents 1 and 2). Since the sintering of zirconia requires a temperature of 1400°C to 1600°C, the sintering cycle for atmospheric pressure sintering typically requires more than 5 hours.
[0004] In recent years, sintering furnaces (sintering kilns) capable of maintaining the sintering temperature (maximum reached temperature) at atmospheric pressure for a period of ten minutes to less than one hour (hereinafter also referred to as "short-time sintering") have begun to be commercialized in the manufacture of zirconia sintered bodies (e.g., Patent Document 3). Existing technical documents Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-026990 Patent Document 2: International Publication No. 2020 / 196650 Patent Document 3: International Publication No. 2012 / 057829 Summary of the Invention The technical problem that the invention aims to solve
[0006] The purpose of this invention is to provide a manufacturing method for producing a sintered body based on atmospheric pressure sintering under atmospheric atmosphere, which can shorten the sintering time required, and can obtain a sintered body that is visually recognized as having the same color tone as a sintered body obtained by atmospheric pressure sintering (hereinafter also referred to as "long-time sintering") that requires a sintering time of more than 5 hours. Technical solutions for solving technical problems
[0007] The inventors discovered the following technical problem: Although both long-time sintering and short-time sintering are performed under the same atmospheric atmosphere, if the zirconium oxide composition used in long-time sintering is directly used in short-time sintering, the aesthetics, especially the color tone, of the resulting sintered body are significantly different from those obtained in long-time sintering. Furthermore, it was discovered that by subjecting specific treatments to the sintered body of colored zirconium oxide obtained by short-time sintering, a sintered body can be obtained that, despite having a significantly shorter production time than conventional long-time sintering, exhibits the same visual aesthetics as the sintered body of colored zirconium oxide obtained through long-time sintering.
[0008] That is, the present invention is as described in the claims, and the gist of the present invention is as follows. [1] A method for manufacturing a sintered body, characterized in that it includes a step of heat-treating a sintered body containing a coloring element, which is at a temperature of 600°C or higher and 1200°C or lower. [2] According to the manufacturing method described in [1] above, the sintered body containing the coloring element is a sintered body in the state after sintering under normal pressure. [3] According to the manufacturing method described in [1] or [2] above, the sintered body containing the coloring element is a sintered body in the state after sintering under an oxidizing atmosphere. [4] The manufacturing method according to any one of [1] to [3] above, wherein the heat treatment is a heat treatment performed at any heat treatment temperature of 600°C or higher and 1200°C or lower. [5] The manufacturing method according to any one of [1] to [4] above, wherein the temperature range of the heat treatment temperature is ±50°C. [6] The manufacturing method according to any one of [1] to [5] above, wherein the holding time at the heat treatment temperature is less than 2 hours. [7] The manufacturing method according to any one of [1] to [6] above, wherein the atmosphere of the heat treatment is an oxidizing atmosphere. [8] The manufacturing method according to any one of [1] to [7] above, wherein the heat treatment step is to place a sintered body containing a coloring element of zirconium oxide in a sintering furnace heated to a heat treatment temperature and heat treat it. [9] The manufacturing method according to any one of [1] to [7] above, wherein, prior to the heat treatment step, there is a step of sintering colored zirconium oxide in an oxidizing atmosphere to obtain a sintered body containing a coloring element of zirconium oxide.
[10] The manufacturing method according to any one of [1] to [7] and [9] above, wherein the heat treatment step is a step of holding at a sintering temperature, cooling to a heat treatment temperature and holding at that heat treatment temperature to perform heat treatment.
[11] The manufacturing method according to any one of [1] to
[10] above, wherein the sintered body obtained in the heat treatment step is a colored zirconia sintered body that has a lightness difference of 5 or less and a chroma difference of 0.3 or more compared with the zirconia sintered body containing coloring elements supplied to the step, or a lightness difference of more than 5 and a chroma difference of 10 or less.
[12] The manufacturing method according to any one of [1] to
[11] above, wherein the coloring element is selected from one or more of the group consisting of iron (Fe), cobalt (Co), manganese (Mn), nickel (Ni), copper (Cu), titanium (Ti), chromium (Cr), cerium (Ce), praseodymium (Pr), neodymium (Nd), erbium (Er), terbium (Tb) and ytterbium (Yb).
[13] The manufacturing method according to any one of [1] to
[12] above, wherein the zirconium oxide contains a stabilizing element.
[14] In the manufacturing method described in
[13] above, the stabilizing element comprises at least yttrium.
[15] The manufacturing method according to any one of [1] to
[14] above, wherein the zirconium oxide contains at least yttrium.
[16] The manufacturing method according to any one of [1] to
[15] above, wherein the sintered body of the zirconium oxide containing the coloring element comprises aluminum oxide (Al2O3). Invention Effects
[0009] According to the present invention, a manufacturing method is provided for manufacturing a sintered body based on atmospheric pressure sintering under an atmospheric atmosphere, which can shorten the sintering time required, and can obtain a sintered body that is visually recognized as having the same color tone as a sintered body obtained by long-term sintering. Detailed Implementation
[0010] The present invention will now be described with reference to an example of an embodiment. The main terms used in this embodiment are as follows.
[0011] "Zirconium oxide containing coloring elements" refers to a composition that essentially contains coloring elements and zirconium oxide (zirconia, ZrO2), for example, one or more of the following are selected from the group consisting of powder, granular powder, shaped body, pre-sintered body and sintered body containing coloring elements and zirconium oxide, preferably one or more of the following are selected from the group consisting of powder, granular powder, shaped body, pre-sintered body and sintered body containing coloring elements and using zirconium oxide as matrix (masterbatch).
[0012] "Composition" means a substance having a specific composition, for example, one or more selected from the group consisting of powder, particulate powder, shaped body, pre-sintered body and sintered body. "Zirconium oxide composition" means a composition that essentially contains zirconium oxide, and further means a composition with zirconium oxide as a matrix (masterbatch). "Colored zirconium oxide composition" means a zirconium oxide composition containing coloring elements.
[0013] "Powder" refers to an aggregate of multiple powder particles and is a fluid composition. "Zirconium oxide powder" refers to powder that essentially contains zirconium oxide, and further refers to powder with zirconium oxide as a matrix (masterbatch). "Colored zirconium oxide powder" refers to zirconium oxide powder containing coloring elements.
[0014] "Particulate powder" refers to an aggregate of powder particles and is a composition with flowability, particularly a composition with higher flowability than powder. "Zirconium oxide granular powder" refers to granular powder that essentially contains zirconium oxide, and further refers to granular powder with zirconium oxide as a matrix (masterbatch). "Colored zirconium oxide granular powder" refers to zirconium oxide granular powder containing coloring elements.
[0015] "Formed body" refers to a composition with a certain shape, consisting of powder particles agglomerated by physical force, especially a composition in a state without heat treatment. "Zirconium oxide formed body" refers to a formed body that essentially contains zirconium oxide, and further refers to a formed body with zirconium oxide as a matrix (masterbatch). "Colored zirconium oxide formed body" refers to a zirconium oxide formed body containing coloring elements. In addition, "formed body" can be used interchangeably with "powder compact".
[0016] "Pre-sintered body" refers to a composition with a specific shape made of molten particles, which is a composition that has undergone heat treatment at a temperature below the sintering temperature. "Zirconium oxide pre-sintered body" refers to a pre-sintered body that essentially contains zirconium oxide, and further refers to a pre-sintered body with zirconium oxide as the matrix (masterbatch). "Colored zirconium oxide pre-sintered body" refers to a zirconium oxide pre-sintered body containing coloring elements. In addition, pre-sintered body can be used interchangeably with "pre-sintered body" and "semi-sintered body".
[0017] "Sintered body" refers to a composition consisting of grains, and is a composition that has undergone heat treatment at a temperature above the sintering temperature. "Zirconium oxide sintered body" refers to a sintered body that essentially contains zirconium oxide, and further refers to a sintered body with zirconium oxide as the matrix (master material). "Colored zirconium oxide sintered body" refers to a zirconium oxide sintered body containing coloring elements.
[0018] "Stabilizing element" refers to an element that can stabilize the crystalline phase of zirconium oxide by dissolving it in zirconium oxide, while "coloring element" refers to an element that can color zirconium oxide. In addition, an element that has both stabilizing and coloring functions is also called a "coloring and stabilizing element".
[0019] In the zirconia composition, "stabilizing element amount" is the molar ratio of stabilizing element relative to the total amount of zirconia and stabilizing element converted to oxide [mol%], "coloring element amount" is the ratio of the mass [g] of coloring element converted to oxide to the mass [g] of zirconia composition converted to oxide [mass%], and "additive amount" is the ratio of the mass [g] of additive component converted to oxide to the mass [g] of zirconia composition converted to oxide [mass%]. For example, in a zirconium oxide composition containing alumina as an additive, iron and titanium as coloring elements, terbium as a color stabilizing element, and yttrium as a stabilizing element, the amount of stabilizing element can be calculated by {(Tb4O7+Y2O3)[mol] / (Tb4O7+Y2O3+ZrO2)[mol]}×100, the amount of coloring element can be calculated by {(Fe2O3+Tb4O7+TiO2)}[g] / (Fe2O3+Tb4O7+Y2O3+ZrO2+Al2O3+TiO2)[g]}×100, and the amount of additive can be calculated by {(Al2O3)[g] / (Fe2O3+Tb4O7+Y2O3+ZrO2+Al2O3+TiO2)[g]}×100. It should be noted that in the calculation of the composition of the zirconium oxide composition, hafnium oxide (HfO2), which is an unavoidable impurity, can be regarded as zirconium oxide (ZrO2).
[0020] "BET specific surface area" is a value obtained by the BET method (one-point method) according to JIS Z 8830, by setting the adsorbate as nitrogen (N2).
[0021] "Measured density" refers to the ratio (g / cm³) of the volume obtained through dimensional measurement to the mass obtained through mass measurement for both shaped and pre-sintered bodies. 3 On the other hand, for sintered bodies, it is the ratio of the volume determined by the Archimedes method to the mass determined by mass measurement (g / cm³). 3 ).
[0022] "XRD pattern" refers to the powder X-ray diffraction pattern of colored zirconia measured under the following conditions. X-ray source: CuKα rays (λ = 0.15418 nm) Measurement mode: Continuous scanning Scanning speed: 4° / minute Measurement range: 2θ = 26°~33° Accelerating voltage and current: 40mA·40kV Longitudinal diverging slit: 10mm Diverging / Incident Slit: 1° Light-receiving slit: open Detector: Semiconductor detector (D / teX Ultra) Filter: Ni filter Goniometer radius: 185mm
[0023] XRD measurements can be performed using a standard X-ray diffraction apparatus (e.g., Ultima IV, manufactured by RIGAKU). The area intensity of each crystal plane is determined by curve fitting of the smoothed and background-removed XRD pattern using a separate pseudo-Voigt function. Analysis of the XRD pattern, including smoothing, background removal, and area intensity calculations, can be performed using analysis programs included with the X-ray diffraction apparatus (e.g., PDXL Ver.2.2, a comprehensive powder X-ray analysis software manufactured by RIGAKU).
[0024] As equivalent to the XRD peaks of each crystal plane of zirconium oxide as measured in the above-mentioned XRD determination, XRD peaks with peak positions in the following 2θ can be cited. The XRD peak corresponding to the (111) plane of a monoclinic crystal is: 2θ = 31 ± 0.5° The XRD peak corresponding to the (11-1) plane of a monoclinic crystal is: 2θ = 28 ± 0.5° The XRD peak corresponding to the (111) plane of a tetragonal crystal is: 2θ = 30 ± 0.5° XRD peaks corresponding to the (111) plane of a cubic crystal: 2θ = 30 ± 0.5°
[0025] The XRD peaks corresponding to the tetragonal (111) plane and the XRD peaks corresponding to the cubic (111) plane were measured as an overlapping peak.
[0026] "Hue" refers to the CIE L value measured against a black background under the following conditions for a test specimen with a thickness of 1 mm and a surface roughness (Ra) ≤ 0.02 μm: using a spectrophotometer (e.g., CM-700d, manufactured by Konica Minolta) equipped with an illumination and receiving optical system according to geometric condition c of JIS Z 8722. * a * b * Colorimetric system (CIE 1976 (L) * a * b * In a color space, lightness (L) is used as the unit of measurement.* Hue a * and b * The color tone of the expression. Light source: D65 light source Angle of view: 10° Measurement method: SCI Measurement background: black plate
[0027] "Saturation" is one of the indicators of the vividness of a hue, determined by hue a. * and b * The value is obtained by the following formula. C * =(a *2 +b *2 ) 0.5
[0028] In the above formula, C * For chroma, a * and b * Hue a * and b * .
[0029] "Color difference" refers to the difference between the hue of the base colored zirconia and the hue of the object colored zirconia, and is a value obtained by the following formula. △E * ={(L1) * -L2 * ) 2 +(a1 * -a2 * ) 2 +(b1 * -b2 * ) 2} 0.5
[0030] In the above formula, △E * For color difference, L1 * a1 * and b1 * The lightness L of the colored zirconium oxide used as a reference is respectively. * Hue a * and b * Additionally, L2 * a2 * and b2 * The lightness L of the colored zirconium oxide as the object * Hue a * and b * .
[0031] "Total transmittance" refers to the ratio of the transmittance of the transmitted light to the incident light (the total value of diffuse transmittance and linear transmittance) for a test sample with a thickness of 1 mm and a surface roughness (Ra) ≤ 0.02 μm, measured using a conventional turbidimeter (haze meter; for example, NDH4000, manufactured by NIPPON DENSHOKU), through which light from the CIE standard light source D65 is transmitted as incident light and focused using an integrating sphere.
[0032] "Transmittance difference" refers to the ratio of the difference between the total transmittance of the colored zirconia as the object and the total transmittance of the colored zirconia as the reference, and is a value obtained by the following formula. △T={(T1-T2) 2} 0.5
[0033] In the above formula, △T is the transmittance difference, T1 is the total transmittance of the colored zirconia used as the reference, and T2 is the total transmittance of the colored zirconia used as the object.
[0034] "Atmospheric pressure sintering" refers to sintering in which no external force is applied to the sintered material (shaped body, pre-sintered body, etc.) during sintering, especially sintering under atmospheric pressure.
[0035] "Pressure sintering" refers to sintering processes such as hot pressing (HP process) and hot isostatic pressing (HIP process), in which external force is applied to the material being sintered while it is heated.
[0036] This embodiment is a method for manufacturing a sintered body (hereinafter, in this embodiment, for convenience, the sintered body containing coloring elements of zirconium oxide supplied to the heat treatment process is also referred to as a "precursor sintered body"), characterized by a step of heat-treating the sintered body containing coloring elements of zirconium oxide at a temperature of 600°C or higher and 1200°C or lower (hereinafter also referred to as the "heat treatment process"). Conventional sintering involves holding the sintering temperature to densify the zirconium oxide containing coloring elements (colored zirconium oxide) while simultaneously forming a desired hue. In contrast, this embodiment focuses on achieving densification of the colored zirconium oxide in the same way as long-term sintering through short-time sintering, while maintaining a different hue change compared to long-term sintering. Furthermore, it has been found that in this embodiment, by performing heat treatment on the sintered colored zirconium oxide without densification, it is easier to promote the color development of the colored zirconium oxide, resulting in a sintered body that can be visually recognized as having the same aesthetic appeal as a sintered body of colored zirconium oxide obtained through long-term sintering.
[0037] As the primary sintering atmosphere for zirconia, oxidizing atmospheres, reducing atmospheres, or vacuum atmospheres are known. Conventionally, it is known that during zirconia sintering, to remove residual carbon, reduced metal elements, and other reducing substances, the sintered body sintered in a reducing atmosphere is subjected to heat treatment (so-called tempering) in an oxidizing atmosphere. Unlike tempering, which involves sintering in an atmosphere different from the sintering atmosphere of at least one of the shaped body and the pre-sintered body, the heat treatment in this embodiment is a heat treatment that performs a different function than tempering. Preferably, it is heat treatment based on the same atmosphere as the sintering atmosphere, and more preferably, it is heat treatment of the sintered body of colored zirconia sintered in an atmospheric atmosphere. It is believed that by performing such heat treatment, the color development of the colored zirconia is further promoted.
[0038] <Colored Zirconia Sintered Body> In the heat treatment process, a sintered body containing coloring elements of zirconium oxide (colored zirconium oxide sintered body; precursor sintered body) is provided. The precursor sintered body is preferably a sintered body in the state after sintering in an oxidizing atmosphere, and more preferably a sintered body in the state after sintering at atmospheric pressure, i.e., an atmospheric pressure sintered body. The precursor sintered body is further preferably a sintered body in the state after atmospheric pressure sintering in an atmospheric atmosphere (atmospheric pressure sintered body in the state after sintering in an atmospheric atmosphere), and even further preferably a sintered body in the state after atmospheric pressure sintering in an atmospheric atmosphere with a holding time of less than 2 hours at the sintering temperature, and even further preferably a sintered body in the state after atmospheric pressure sintering in an atmospheric atmosphere with a holding time of less than 2 hours at the sintering temperature.
[0039] The precursor sintered body is preferably free of ceramic material on its surface.
[0040] It should be noted that the colored zirconia sintered body shown below is characterized in that, in the manufacturing method of this embodiment, the colored zirconia sintered body (precursor sintered body) supplied for the heat treatment process and the sintered body (colored zirconia sintered body; hereinafter, for convenience, also referred to as "heat-treated sintered body") obtained after the heat treatment process can be used interchangeably.
[0041] Coloring elements may include at least one of transition metal elements and lanthanide rare earth elements, and further examples include transition metal elements other than zirconium (Zr) and hafnium (Hf), as well as lanthanide rare earth elements. Preferred coloring elements include one or more selected from the group consisting of iron (Fe), cobalt (Co), manganese (Mn), nickel (Ni), copper (Cu), titanium (Ti), chromium (Cr), cerium (Ce), praseodymium (Pr), neodymium (Nd), erbium (Er), terbium (Tb), and ytterbium (Yb), further selected from one or more selected from the group consisting of iron, cobalt, titanium, manganese, praseodymium, erbium, and terbium, and even further selected from one or more selected from the group consisting of iron, cobalt, titanium, erbium, and terbium, preferably containing at least iron or terbium, more preferably containing at least terbium.
[0042] The coloring element contained in colored zirconia can be in any form. The coloring element may be contained in at least one of the forms of ions and compounds. Alternatively, the coloring element may be contained therein by being dissolved in zirconia.
[0043] The colored zirconia preferably comprises one or more elements selected from the group consisting of iron, terbium, and praseodymium (hereinafter also referred to as "yellow coloring elements"), and at least one element selected from neodymium and erbium (hereinafter also referred to as "red coloring elements"); more preferably, it comprises yellow coloring elements, red coloring elements, and one or more elements selected from the group consisting of cobalt, titanium, and manganese (hereinafter also referred to as "gray coloring elements"). By combining these coloring elements, the colored zirconia easily gives the impression of being close to natural teeth when visually identified.
[0044] In addition, colored zirconia can include yellow and gray coloring elements as coloring elements, or it can include gray and red coloring elements as coloring elements.
[0045] Zirconia preferably contains a stabilizing element. The stabilizing element is preferably one or more selected from the group consisting of yttrium (Y), calcium (Ca), cerium, magnesium (Mg), praseodymium, ytterbium, erbium, and terbium; more preferably, one or more selected from the group consisting of yttrium, cerium, erbium, and terbium; even more preferably, one or more selected from the group consisting of yttrium, erbium, and terbium; even more preferably, one or more selected from the group consisting of yttrium and terbium; and even more preferably, yttrium. Furthermore, the stabilizing element preferably contains at least yttrium.
[0046] Zirconia preferably contains a stabilizing element, more preferably contains one or more selected from the group consisting of yttrium, calcium, cerium, magnesium, praseodymium, ytterbium, erbium and terbium, even more preferably contains one or more selected from the group consisting of yttrium, erbium and terbium, even more preferably contains at least one of yttrium and terbium, and particularly preferably contains at least yttrium.
[0047] The stabilizing element (color stabilizing element) is selected from one or more of the group consisting of cerium, praseodymium, ytterbium, terbium, and erbium, further including at least one of terbium and erbium, or further including terbium as a coloring element. Colored zirconia may contain only the color stabilizing element as a coloring element, or it may contain coloring elements other than the color stabilizing element. In order to stabilize the crystalline phase of zirconia, in order to achieve the desired hue of the sintered colored zirconia obtained through a heat treatment process, colored zirconia may also contain both the color stabilizing element and a stabilizing element that does not function as a coloring element (hereinafter also referred to as "non-color stabilizing element"). Examples of non-color stabilizing elements include, for example, one or more of the group consisting of yttrium, calcium, and magnesium, and further including yttrium.
[0048] In colored zirconia, the content of the stabilizing element in zirconia is only required to stabilize the crystalline phase of zirconia, and can be 0.1 mol% or more and 10 mol% or less. When the stabilizing element is yttrium, the content of the stabilizing element (hereinafter, when the stabilizing element is yttrium, etc., it will also be referred to as "yttrium content", etc.) can be 2.5 mol% or more, 3 mol% or more, 3.5 mol% or more, 4 mol% or more, or 5 mol% or more, and can also be 8 mol% or less, 7 mol% or less, 6 mol% or less, or 5.5 mol% or less. Similarly, the erbium content can be 0 mol% or more, 0.03 mol% or more, or 0.1 mol% or more, and can also be 0.62 mol% or less or 0.41 mol% or less. Terbium content can be 0 mol% or more, 0.001 mol% or more, or 0.002 mol% or more, or less than 0.04 mol%, less than 0.02 mol% or less.
[0049] Colored zirconia sintered bodies may also contain components with functions other than coloring and stabilization (hereinafter also referred to as "additives") as needed. Examples of additives include alumina (Al2O3).
[0050] Because sintered bodies tend to be less prone to degradation, colored zirconia sintered bodies may contain alumina. Examples of alumina content in such sintered bodies (hereinafter, the amount of added component, such as alumina, will be referred to as "alumina content") include 0% by mass or more, more than 0% by mass, 0.01% by mass or more, or 0.02% by mass or more; alternatively, it may be 0.1% by mass or less, or 0.06% by mass or less. Colored zirconia sintered bodies may also not contain alumina (i.e., the alumina content may be 0% by mass).
[0051] Colored zirconia sintered bodies can also contain unavoidable impurities. One example of an unavoidable impurity in zirconia is hafnium oxide (HfO2).
[0052] The colored zirconia sintered body preferably does not contain oxides of stabilizing elements, i.e., undissolved stabilizing elements, and more preferably does not contain undissolved yttrium oxide (Y₂O₃). Whether the sintered body contains undissolved stabilizing elements can be confirmed by its XRD pattern. That is, if the XRD pattern of the colored zirconia sintered body contains XRD peaks of oxides of stabilizing elements (e.g., yttrium oxide; Y₂O₃), it can be considered that the sintered body contains undissolved stabilizing elements. In order not to have a substantial impact on the properties of the colored zirconia sintered body, in this embodiment, the colored zirconia sintered body is allowed to contain undissolved stabilizing elements to a degree that cannot be confirmed by the XRD pattern.
[0053] The shape of the colored zirconia sintered body can be any shape that corresponds to the purpose and use, such as circular plate, cylindrical, polyhedral, spherical, and conical shapes.
[0054] <Sintering Process> The colored zirconia sintered body (precursor sintered body) supplied for the heat treatment process can be any sintered body obtained by any manufacturing method. Preferably, it is a sintered body obtained by sintering colored zirconia in an oxidizing atmosphere. More preferably, it is a sintered body obtained by sintering colored zirconia under atmospheric pressure. Even more preferably, it is a sintered body obtained by sintering colored zirconia under atmospheric pressure in an atmospheric atmosphere. More preferably, it is a sintered body containing coloring elements obtained by sintering colored zirconia at a sintering temperature of 1400°C or higher for less than 2 hours.
[0055] In other words, before the heat treatment process, the manufacturing method of this embodiment may include a process of sintering zirconia containing coloring elements (colored zirconia) (hereinafter also referred to as the "sintering process"). Further, it may include a process of sintering zirconia in an oxidizing atmosphere to obtain a sintered body of zirconia. Further, it may include a process of sintering zirconia under atmospheric pressure to obtain a sintered body of zirconia. In addition, it may include a process of sintering zirconia under atmospheric pressure in an atmospheric atmosphere to obtain a sintered body of zirconia. Further, it may include a process of sintering zirconia at a sintering temperature of 1400°C or higher for less than 2 hours to obtain a sintered body of zirconia containing coloring elements.
[0056] As the sintering temperature increases, there is a tendency to promote densification of colored zirconia. The sintering temperature need only be the temperature at which densification of colored zirconia is achieved, preferably 1400°C or higher, 1450°C or higher, 1500°C or higher, or 1550°C or higher. If densification of colored zirconia is to be promoted, the sintering temperature does not need to be as high as necessary; examples of sintering temperatures include 1650°C or lower, or 1600°C or lower.
[0057] The holding time at the sintering temperature is preferably less than 2 hours, less than 1 hour, less than 30 minutes, or less than 20 minutes; in addition, it is preferably more than 1 minute, more than 5 minutes, or more than 10 minutes.
[0058] The sintering atmosphere is preferably an oxidizing atmosphere, and more preferably an atmospheric atmosphere.
[0059] The sintering method is arbitrary and can be selected from one or more of the group consisting of vacuum sintering, pressure sintering, and atmospheric pressure sintering. It is preferably at least one of pressure sintering and atmospheric pressure sintering, more preferably atmospheric pressure sintering, and even more preferably atmospheric pressure sintering only. The sintering process preferably does not include pressure sintering and vacuum sintering, and more preferably does not include pressure sintering.
[0060] The heating rate to the sintering temperature is arbitrary. From the viewpoint of shortening the time required for sintering, a heating rate where the time required to reach the sintering temperature (heating time) is less than 2 hours is preferred. More preferably, the heating time is less than 1 hour, less than 30 minutes, less than 15 minutes, or less than 10 minutes. When using a general-purpose sintering furnace, the heating time can be exemplified as more than 3 minutes or more than 5 minutes. Examples of heating rates to reach the sintering temperature include: 5°C / min or more, 10°C / min or more, 50°C / min or more, 100°C / min or more, or 150°C / min or more. Additionally, rates less than 300°C / min, less than 200°C / min, or less than 190°C / min are also possible. The heating rate can vary, for example, in each temperature range from room temperature to around 1000°C, from 1000°C to around 1200°C, and from 1200°C to the sintering temperature. Furthermore, the heating rate can also be a different rate than the cooling rate described later.
[0061] The colored zirconia supplied for the sintering process can be any colored zirconia composition that can serve as a precursor of a sintered body (precursor sintered body), particularly selected from one or more of the group consisting of colored zirconia powder, granular powder, shaped body and pre-sintered body, and further selected from at least one of the shaped body and pre-sintered body of colored zirconia.
[0062] For simplicity, any colored zirconia supplied for the sintering process can be a shaped colored zirconia body. On the other hand, if the shape of the shaped body differs from the desired shape of the sintered body, the colored zirconia supplied for the sintering process is preferably a pre-sintered colored zirconia body. This pre-sintered body can be machined into any shape using CAD / CAM or similar processing methods before the sintering process. Therefore, the pre-sintered body supplied for the sintering process can be a pre-sintered body in its processed state.
[0063] The method for manufacturing colored zirconia molded articles for the sintering process is arbitrary. For example, at least one of colored zirconia powder and particulate powder can be mixed with a binder as needed and shaped by a known method. The colored zirconia molded article is preferably a molded article containing a mixture of powder containing coloring elements and zirconia powder, and more preferably a molded article in the state after the mixture of powder containing coloring elements and zirconia powder has been shaped.
[0064] Examples of molding methods include one or more selected from the group consisting of uniaxial pressing, cold isostatic pressing, slide casting, and injection molding. For simplicity, the molding method is preferably at least one of uniaxial pressing and cold isostatic pressing, and more preferably a molding method in which cold isostatic pressing is performed after uniaxial pressing. The pressure of uniaxial pressing is exemplified as 15 MPa or more and 150 MPa or less, and the pressure of cold isostatic pressing is exemplified as 90 MPa or more and 400 MPa or less. The higher the pressure during molding, the easier it is to increase the density of the resulting molded article.
[0065] The zirconium oxide contained in the colored zirconium oxide molded body is preferably zirconium oxide in the state after heat treatment of zirconium oxide sol, more preferably zirconium oxide in the state after heat treatment of zirconium oxide sol obtained by hydrolysis of zirconium compounds, and even more preferably zirconium oxide in the state after heat treatment of zirconium oxide sol obtained by hydrolysis of zirconium oxychloride.
[0066] A binder is a substance that has the function of physically bonding powder particles together or granular powder together. Any binder used for ceramic molding and capable of improving the shape retention of the molded body is acceptable. The binder is preferably a substance removed from colored zirconia by heat treatment at 1200°C or below. Examples include: organic binders; further, one or more selected from the group consisting of polyvinyl alcohol, polyvinyl butyral, wax, and acrylic resin; further, at least one of polyvinyl alcohol and acrylic resin; and further, acrylic resin.
[0067] Prior to sintering, it is preferable to remove the binder contained in the shaped body. The method of binder removal is arbitrary, and examples include firing in an atmospheric atmosphere at a temperature above 400°C and below 900°C.
[0068] Colored zirconia supplied for the sintering process can be a pre-sintered colored zirconia body. The method for manufacturing the pre-sintered colored zirconia body for the sintering process is arbitrary; for example, the colored zirconia shaped body can be pre-sintered using a known method.
[0069] Pre-sintering is simply a heat treatment under conditions where the powder particles of colored zirconia become molten particles, for example, heat treatment at a temperature below the sintering temperature of zirconia.
[0070] The pre-sintering temperature can be exemplified as above 800°C, above 900°C, or above 950°C. Alternatively, it can be exemplified as below 1200°C, below 1150°C, or below 1100°C.
[0071] The holding time at the pre-sintering temperature is preferably 0.5 hours or more and 5 hours or less, and more preferably 0.5 hours or more and 3 hours or less.
[0072] The pre-sintering atmosphere is preferably an atmosphere other than a reducing atmosphere, more preferably an oxidizing atmosphere, and even more preferably an atmospheric atmosphere. It should be noted that the pre-sintering atmosphere can be the same as the atmosphere used in the sintering process and the heat treatment process, or it can be a different atmosphere.
[0073] <Heat Treatment Process> In the manufacturing method of this embodiment, the sintered body (precursor sintered body) of colored zirconia is heat-treated at a temperature of 600°C or higher and 1200°C or lower. In order to facilitate the coloring of zirconia, the heat treatment is preferably performed at a temperature of 700°C or higher, 750°C or higher, 800°C or higher, or 850°C or higher. In addition, it is more preferably performed at a temperature of 1150°C or lower, 1100°C or lower, or 1050°C or lower, and more preferably at a temperature of more than 700°C and less than 1100°C.
[0074] When the coloring element is a transition metal element, the heat treatment is preferably performed at 700°C or above, or 800°C or above, and 1200°C or below, or 1150°C or below. For example, the heat treatment of iron-containing precursor sintered bodies is performed at 800°C or above, or 900°C or above, and 1200°C or below, or 1150°C or below; the heat treatment of cobalt-containing precursor sintered bodies is performed at 700°C or above, or 800°C or above, and 1150°C or below, or 1100°C or below; and the heat treatment of manganese-containing precursor sintered bodies is performed at 900°C or above, or 1000°C or above, and 1200°C or below, or 1150°C or below.
[0075] When the coloring element is a lanthanide rare earth element, the heat treatment is preferably performed at 650°C or above, or 700°C or above, and below 1200°C or 1100°C. For example, the heat treatment of terbium-containing precursor sintered bodies is performed at 650°C or above, or 700°C or above, and below 1150°C or 1100°C; the heat treatment of praseodymium-containing precursor sintered bodies is performed at 800°C or above, or 900°C or above, and below 1200°C or 1100°C.
[0076] The heat treatment is preferably performed and held at any heat treatment temperature (hereinafter also referred to as "heat treatment temperature") between 600°C and 1200°C. The heat treatment temperature can be a specific temperature, but it can also have a temperature range, for example, the temperature range of the heat treatment temperature can be ±0°C, ±2°C, ±5°C, ±10°C, ±30°C or ±50°C. Examples of heat treatment include: heat treatment performed at a temperature selected from the group consisting of 1150℃, 1100℃, 1050℃, 1000℃, 950℃, 900℃, 850℃, 800℃, 750℃, 700℃, 650℃, and 600℃, wherein the range of the heat treatment temperature is ±50℃ or less, ±30℃ or less, or ±5℃ or less; further, heat treatment performed at a temperature selected from the group consisting of 1000℃, 900℃, 800℃, and 700℃, wherein the range of the heat treatment temperature is ±50℃ or less, ±30℃ or less, ±10℃ or less, or ±5℃ or less; and still further, heat treatment performed at a temperature selected from the group consisting of 1000℃, 900℃, and 800℃, wherein the range of the heat treatment temperature is ±30℃ or less, ±10℃ or less, or ±5℃ or less.
[0077] This heat treatment can also be a heat treatment in which the precursor sintered body is held at two or more heat treatment temperatures. Examples of heat treatments in which the body is held at two or more heat treatment temperatures include: holding at any heat treatment temperature above 1000°C and below 1200°C, and then holding at any heat treatment temperature above 600°C and below 1000°C; holding at any heat treatment temperature above 600°C and below 1000°C, and then holding at any heat treatment temperature above 1000°C and below 1200°C.
[0078] The heat treatment time is arbitrary, but the holding time at the heat treatment temperature can be the same as the heat treatment time. For example, the holding time at the heat treatment temperature can be more than 1 minute, more than 3 minutes, more than 5 minutes, or more than 10 minutes. From the viewpoint of shortening the time required for sintering, the holding time is preferably less than 2 hours, less than 1 hour, less than 30 minutes, less than 25 minutes, or less than 20 minutes.
[0079] The atmosphere for heat treatment is preferably an oxidizing atmosphere, and more preferably an atmospheric atmosphere.
[0080] The heat treatment method is arbitrary and can be selected from one or more of the group consisting of firing under vacuum, firing under pressure, and firing under atmospheric pressure. It is preferred to be at least one of firing under pressure and firing under atmospheric pressure, more preferably firing under atmospheric pressure, and even more preferably firing under atmospheric pressure only. Firing under atmospheric pressure is particularly preferred to be firing under atmospheric pressure in an atmospheric atmosphere.
[0081] The heat treatment process is preferably performed using a sintering procedure with the heat treatment temperature and holding time controlled as described above.
[0082] One preferred heat treatment process is to heat-treat a colored zirconia sintered body placed in a sintering furnace heated to a heat treatment temperature. This allows for the production of a colored zirconia sintered body with the desired hue in a shorter time. To produce the sintered body in a shorter time, the heat treatment process is preferably as follows: the zirconia sintered body containing coloring elements, after being held at the sintering temperature, is removed from the sintering furnace at a temperature cooled to either 1000°C or 1200°C, and then placed in a sintering furnace at 600°C or 1200°C for heat treatment.
[0083] As another preferred heat treatment process, one can exemplify is a process in which the sintering temperature is held, then cooled to a heat treatment temperature, and held at that temperature to perform heat treatment. This allows for the production of colored zirconia sintered bodies that exhibit the desired hue without requiring multiple sintering furnaces.
[0084] In conventional sintering methods, the cooling process aims to cool the sintered zirconia to its removal temperature (e.g., near room temperature). Therefore, from the viewpoint of shortening the sintering time, it is preferable to shorten the cooling process. In contrast, by extending the time required for the heat treatment process during cooling and designating it as heat treatment during cooling, it is possible to control the hue of the sintered colored zirconia while simultaneously cooling the sintered body of the colored zirconia. As a result, compared to the case where the sintered body is cooled to near room temperature and then subjected to heat treatment again, the time and energy required for heat treatment are reduced, making the manufacturing method of this embodiment a more suitable manufacturing method for industrial applications.
[0085] In this embodiment, during the cooling process, it is preferable to hold the sintered body in a temperature range of 600°C or higher and 1200°C or lower for at least 5 minutes. By satisfying this condition, it is considered that the coloring elements contained in the sintered body are close to the state of the coloring elements contained in the sintered body obtained by long-term sintering, and it is easy to obtain a sintered body with the desired hue.
[0086] During the cooling process, the residence time (hereinafter also referred to as "residence time") of the precursor sintered body in a temperature range of 600°C to 1200°C can be, for example, 5 minutes or more, 8 minutes or more, or 10 minutes or more, and can also be 90 minutes or less, 80 minutes or less, 70 minutes or less, or 60 minutes or less. From the viewpoint of approximating the color tone of the sintered body obtained by long-term sintering, a longer residence time is preferred, but in order to shorten the total time required for the sintering process and the heat treatment process, a residence time of 50 minutes or less or 40 minutes or less is preferred.
[0087] During the cooling process, the temperature range in which the precursor sintered body remains (hereinafter also referred to as the "retention temperature range") can be exemplified as 600°C or higher and 1200°C or lower, 700°C or higher and 1150°C or lower, and more specifically, 700°C or higher and 1100°C or lower. When the coloring element is a transition metal element, the retention temperature range is preferably 700°C or higher and 1200°C or lower. For example, when the precursor sintered body contains iron, the retention temperature range is preferably 800°C or higher and 1200°C or lower; when the precursor sintered body contains cobalt, the retention temperature range is preferably 700°C or higher and 1150°C or lower; and when the precursor sintered body contains manganese, the retention temperature range is 900°C or higher and 1200°C or lower. When the precursor sintered body contains lanthanide rare earth elements, the retention temperature range is preferably 650°C or higher and 1200°C or lower. For example, when used as a terbium-containing precursor sintered body, the retention temperature range is 650°C or higher and 1150°C or lower; when used as a praseodymium-containing precursor sintered body, the retention temperature range is 800°C or higher and 1200°C or lower.
[0088] In this embodiment, the cooling process refers to the cooling rate (hereinafter also referred to as "cooling rate from 1200°C to the heat treatment temperature") in the temperature range from 1200°C to the heat treatment temperature, which may be 10°C / min or more, 15°C / min or more, or 20°C / min or more. Alternatively, it may be 100°C / min or less, 80°C / min or less, or 60°C / min or less.
[0089] In cases where heat treatment is performed by holding the sintering temperature, then cooling to a heat treatment temperature, and holding at that temperature, the holding time at the heat treatment temperature is arbitrary, for example: more than 1 minute, more than 4 minutes, more than 8 minutes, or more than 10 minutes; and less than 1 hour, less than 50 minutes, less than 40 minutes, or less than 30 minutes. A longer residence time during cooling, even with a shorter holding time at the heat treatment temperature, tends to more easily promote the desired color development of the zirconia. For example, if a sintered body is cooled for 30 minutes in a temperature range above 600°C and below 1200°C and then heat-treated at 600°C for 5 minutes, compared with a sintered body cooled for 5 minutes in a temperature range above 1000°C and below 1200°C and then heat-treated at 1000°C for 10 minutes, the color difference of these sintered bodies is the same as that of sintered bodies obtained through long-term sintering.
[0090] In cases where the precursor sintered body is held at a sintering temperature and then cooled to a heat treatment temperature and held thereafter, the heat treatment can also involve holding the precursor sintered body at two or more heat treatment temperatures. Examples of heat treatments involving holding at two or more heat treatment temperatures include holding at any heat treatment temperature between 1000°C and 1200°C, followed by holding at any heat treatment temperature between 600°C and 1000°C.
[0091] The colored zirconia sintered body (heat-treated sintered body) after the heat treatment process can be removed from the sintering furnace or firing furnace in a manner that does not produce defects. The cooling method after heat treatment is arbitrary and can be exemplified by: cooling to near room temperature (e.g., 20°C to 30°C) in the sintering furnace while controlling the cooling rate; allowing it to cool naturally to near room temperature in the sintering furnace; or removing the colored zirconia (heat-treated sintered body) from the firing furnace while maintaining the heat treatment temperature and cooling it at room temperature, etc.
[0092] The total time required for the sintering and heat treatment processes is preferably shorter than that required for long-term sintering, preferably less than 5 hours, less than 3 hours, less than 1 hour, or less than 45 minutes. Alternatively, it can be more than 10 minutes, more than 15 minutes, or more than 30 minutes.
[0093] The heat-treated sintered body is a colored zirconia sintered body containing the same constituent elements as the precursor sintered body, and is a colored zirconia sintered body with higher chroma than the colored zirconia sintered body supplied for the heat treatment process (precursor sintered body). The lightness L of the precursor sintered body and the sintered body obtained through long-time sintering (hereinafter also referred to as "long-time sintered body") are considered to be... * For the same degree (e.g., brightness L of each other)* The difference is ±5), on the other hand, due to the chroma C * They are very different, therefore the color difference △E * As the size increases, the two colors are visually perceived as different hues. On the other hand, based on the type of coloring element, the chroma C of the precursor sintered body and the long-term sintered body is considered to be different. * To the same degree, on the other hand, due to the brightness L * They are very different, therefore the color difference △E * They are quite different, and sometimes the two shades are visually perceived as different shades.
[0094] Therefore, in the manufacturing method of this embodiment, the heat-treated sintered body is preferably a colored zirconia sintered body with a chroma that is 0.3 or more higher than that of the precursor sintered body, more preferably 0.6 or more higher, and even more preferably 0.8 or more higher. Furthermore, the heat-treated sintered body is preferably a lightness (L) sintered body compared to the precursor sintered body. * The difference between the two values is less than 5 and the chroma (C) is less than 5. * The sintered body is colored zirconia with a lightness difference of 0.3 or more, a further lightness difference of 0.6 or more, a further further lightness difference of 0.8 or more, or a lightness difference of more than 5 and a chroma difference of less than 10; more preferably, it is a lightness difference of L. * The difference is less than 5 and the chroma C * Colored zirconia sintered bodies with a color intensity of 0.3 or higher, further 0.6 or higher, and even further 0.8 or higher. The heat-treated sintered body is preferably a chroma C higher than the precursor sintered body. * A value of 0.3 or higher, 0.6 or higher, 0.8 or higher, 1.0 or higher, 1.5 or higher, or 2.0 or higher with a lightness level of L. * The values are 5 or less, 4.5 or less, and 4 or less. Therefore, it is considered that heat-treated sintered bodies and long-term sintered bodies can be visually identified as having the same hue. Examples of chroma differences are 8.0 or less, 5.0 or less, or 4.5 or less. In other words, the manufacturing method of this embodiment can also be considered a method for manufacturing a sintered body, characterized by a step of heat-treating a sintered body containing zirconium oxide containing coloring elements at 600°C or higher and 1200°C or lower, wherein the chroma of the heat-treated sintered body is 0.6 or more higher, and further 0.8 or more higher, than the chroma of the sintered body before heat treatment.
[0095] A heat-treated sintered body is a sintered body whose hue is visually perceived to be the same as that of a sintered body obtained through long-term sintering. For example, in the case of sintering colored zirconia with the same composition, the color difference (ΔE) between the hue of the heat-treated sintered body (the sintered body obtained by the manufacturing method of this embodiment) and the hue of the long-term sintered body obtained by long-term sintering under the following conditions is... * () can be exemplified as 5 or less, 3 or less, or 2 or less. In addition, it can be exemplified as 0 or more, or 0.5 or more. Heating rate: 600℃ / hour Sintering temperature: 1500℃ Duration: 2 hours Cooling rate: 500℃ / hour
[0096] Similarly, the difference in light transmittance (ΔT) of the heat-treated sintered body compared to the light transmittance of the long-term sintered body can be exemplified as 0.15 or less or 0.10 or less, or 0 or more or 0.01 or more.
[0097] <Heat-treated sintered body> Next, regarding the sintered body obtained by the manufacturing method of this embodiment (hereinafter also referred to as "the sintered body of this embodiment"), as an example, a sintered body containing zirconium oxide selected from the group consisting of terbium, iron and praseodymium as a coloring element will be described.
[0098] The sintered body of this embodiment is a sintered body of yellow zirconium oxide with a yellow hue. An example of the hue of the sintered body in this embodiment is L... * a * b * The lightness (L) represented by the color system * Chroma a * and b * The values are as follows. Brightness L * 66 or above or 70 or above, and, 80 or below or 75 or below Hue a * 0.1 or higher, 0.2 or higher, or 0.3 or higher, and, Below 2.0, below 1.8, below 1.0, or below 0.8 Hue b * 10 or above, 12 or above, 20 or above, or 24 or above, and, 30 or under or 28
[0099] The sintered body of this embodiment is preferably translucent. The total light transmittance of the sintered body of this embodiment (the total light transmittance relative to a D65 light source when the sample thickness is 1 mm) can be 25% or more, 30% or more, 35% or more, or 36% or more. Alternatively, it can be 41% or less or 40% or less.
[0100] The sintered body of this embodiment preferably contains at least one of tetragonal (T-phase) and cubic (C-phase) crystalline phases of zirconium oxide, more preferably at least one tetragonal-dominant zirconium oxide, and even more preferably zirconium oxide containing both tetragonal and cubic crystalline phases. It should be noted that in this embodiment, the "dominant phase" refers to the crystalline phase with the highest proportion (the proportion of the integrated intensity of the XRD peak) among the crystalline phases of zirconium oxide. This proportion can be determined from the XRD pattern on the surface of the sintered body.
[0101] Furthermore, in this embodiment, the sintered body is a zirconia sintered body containing yellow and red coloring elements as coloring elements, and further, in the case of a zirconia sintered body containing yellow, red, and gray coloring elements as coloring elements, the sintered body of this embodiment preferably has the same hue as the dental hue sample, and more preferably has a hue of A1, A2, A3, A3.5, A4, B1, B2, B3, B4, C1, C2, C3, C4, D2, D3, or D4 of VITA Classical Shade.
[0102] As a representative color tone in this embodiment, L in Table 1 can be cited as an example. * a * b * The hue of a color system. However, due to the different light transmittance of sintered bodies, the hue perceived visually varies, so even sintered bodies belonging to the same hue category may sometimes have different hue values.
[0103] [Table 1]
[0104] The method for manufacturing sintered bodies according to this embodiment can be provided as a method for manufacturing sintered bodies used in the known applications of zirconia, such as structural materials and optical materials; it can also be provided as a method for manufacturing sintered bodies used in dental materials, such as exterior and decorative parts for portable electronic devices, dental restorations such as crowns, bridges, inlays, high-mounted inlays, and veneers, dental implant materials such as abutments and implant bridges, and dental orthodontic materials such as brackets; in particular, it can be used as a method for manufacturing sintered bodies for dental use, further as a method for manufacturing sintered bodies for dental restorations, and even further as a method for adjusting the color of sintered bodies for dental restorations. Example
[0105] The following describes this embodiment in detail through examples. However, this embodiment is not limited thereto.
[0106] (BET specific surface area) The BET specific surface area of the samples was determined using a standard BET specific surface area measuring apparatus (TriStar II 3020, manufactured by Shimadzu Corporation) and nitrogen as the adsorbent gas, according to the BET 1-point method of JIS Z 8830. The samples were pretreated by degassing at 250°C in atmospheric air for 30 minutes.
[0107] (Average particle size) The average particle size can be determined by feeding a particulate powder sample into a Microtrac particle size analyzer (device name: MT 3100II, manufactured by MicrotracBEL). The particle size at 50% of the cumulative volume is taken as the average particle size.
[0108] (Total light transmittance) The total transmittance of the sample was determined according to the method in JIS K 7361. The sample was illuminated with a standard light source D65, and the total transmittance was determined by detecting the light beam transmitted through the sample using an integrating sphere. A conventional haze meter (device name: NDH 4000, manufactured by NIPPON DENSHOKU) was used in the measurement.
[0109] The test sample was a circular plate with a diameter of 20 mm and a thickness of 1 mm, and its two surfaces were mirror-polished to a surface roughness of Ra≤0.02 μm to form a sintered body.
[0110] (tone) Hue was determined using a standard spectrophotometer (instrument name: CM-700d, manufactured by Konica Minolta) by placing the test sample against a black background on a black plate. The measurement conditions are as follows.
[0111] Light source: D65 light source Angle of view: 10° Measurement method: SCI Effective area for tone evaluation: 10mm in diameter The test sample was a circular plate with a diameter of 20 mm and a thickness of 1 mm, and its two surfaces were mirror-polished to a surface roughness of Ra≤0.02 μm to form a sintered body.
[0112] (Color difference) The color difference between the hue of the colored zirconia sintered body (heat-treated sintered body) obtained from the examples and comparative examples and the hue of the colored zirconia sintered body (reference example) having the same composition as the sintered body and manufactured by long-term sintering is calculated by the following formula.
[0113] △E * ={(L1) * -L2 * )2 +(a1 * -a2 * ) 2 +(b1 * -b2 * ) 2} 0.5 In the above formula, △E * For color difference, L1 * a1 * and b1 * The lightness L of the colored zirconia sintered body in the reference example are respectively. * Hue a * and b * Additionally, L2 * a2 * and b2 * The lightness L of the sample was measured respectively. * Hue a * and b * .
[0114] Refer to Example 1 (Fabrication of sintered bodies based on long-term sintering) A slurry containing terbium and yttrium-stabilized zirconium oxide (0.034 mol% terbium and 4.0 mol% yttrium), α-alumina, and pure water was mixed in a 2.3 L container and spray-dried at 180 °C to obtain a granular powder containing terbium and yttrium-stabilized zirconium oxide with 0.05 mol% alumina and the remainder being terbium and yttrium-stabilized zirconium oxide granules (alumina-containing terbium and yttrium-stabilized zirconium oxide granules). The BET specific surface area of the obtained granular powder was 10.2 m² / s. 2 / g and an average particle size of 43μm.
[0115] 3g of the powder was filled into a mold with an inner diameter of 25mm and then uniaxially pressed at a pressure of 49MPa. After molding, the powder was subjected to CIP treatment at a pressure of 196MPa to obtain a molded body (powder compact).
[0116] The shaped body was heated to 1000°C at a heating rate of 50°C / hour and held at 1000°C for 1 hour to obtain a pre-sintered body of terbium and yttrium-stabilized zirconium oxide containing 0.05% by mass of alumina, with the remainder being 0.034 mol% terbium and 4.0 mol% yttrium.
[0117] The obtained pre-sintered body was heated to a sintering temperature of 1500°C at a heating rate of 10°C / min, held at this sintering temperature for 2 hours, and then cooled to room temperature at a cooling rate of 500°C / hour (=8.3°C / min). It was then removed from the sintering furnace, yielding a sintered body containing terbium and yttrium-stabilized zirconium oxide with an alumina content of 0.05% by mass, and the remaining portion consisting of 0.034 mol% terbium and 4.0 mol% yttrium. This sintered body was used as the sintered body of Reference Example 1. The hue of the sintered body of Reference Example 1 is L. * a * and b * The figures are 73.6, 1.77, and 27.90, respectively. Examples 1 to 4, Comparative Examples 1 and 2 The pre-sintered body obtained by the same method as in Reference Example 1 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes to form a sintered body. Then, it was cooled to 1200°C at a cooling rate of 240°C / min and removed from the sintering furnace. Next, the removed sintered body (precursor sintered body) was placed in another firing furnace preheated to the heat treatment temperatures shown in Table 2 and held for 5 minutes for heat treatment. After being removed from the firing furnace, the following results were obtained: a sintered body containing terbium and yttrium-stabilized zirconium oxide with an alumina content of 0.05% by mass, containing alumina, and the remaining portion consisting of 0.034 mol% terbium and 4.0 mol% yttrium. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment was 30.1 minutes, and the heat treatment time was 5 minutes. It should be noted that, for Comparative Example 1, no heat treatment was performed, and the sintered body (precursor sintered body) taken out of the sintering furnace was used as the sintered body of Comparative Example 1.
[0118] [Table 2]
[0119] A comparison between the examples and Comparative Example 2 confirms that the heat treatment process △E * The decrease can be further confirmed by a 5-minute heat treatment ΔE. * The decrease confirms that ΔE is lower at 900℃ (above 700℃ but below 1100℃). * The value is significantly reduced. Furthermore, Comparative Examples 1 and 2 confirm that when heat treatment is performed at a temperature of 500°C, ΔE is not obtained. * The effect of reduction. Furthermore, compared to Comparative Example 1, in Comparative Example 2, which underwent heat treatment at 500°C, the chroma C... * The chroma C was reduced; in contrast, the examples all confirmed that the chroma C was reduced.* Increase to 1.5 or higher and 5.0 or lower.
[0120] Examples 5 to 7 The sintered bodies were placed in another firing furnace preheated to 800°C and heat-treated for the holding times shown in Table 3. Afterward, they were removed from the firing furnace. Otherwise, using the same method as in Example 1, sintered bodies containing terbium and yttrium-stabilized zirconium (terbium and yttrium-stabilized zirconium oxide sintered bodies containing 0.05% by mass of alumina, with the remainder being 0.034 mol% terbium and 4.0 mol% yttrium) were obtained. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment and the heat treatment time were: 35.1 minutes and 10 minutes in Example 5, 40.1 minutes and 15 minutes in Example 6, and 45.1 minutes and 20 minutes in Example 7.
[0121] [Table 3]
[0122] Examples 8 to 10 The sintered bodies were placed in another firing furnace preheated to 950°C and heat-treated for the holding times shown in Table 4. Afterward, they were removed from the firing furnace. Otherwise, using the same method as in Example 1, sintered bodies containing terbium and yttrium-stabilized zirconium (terbium and yttrium-stabilized zirconium sintered bodies containing alumina of 0.05 mol% and terbium of 0.034 mol% remaining) were obtained. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment and the heat treatment time were: 35.1 minutes and 10 minutes in Example 8, 40.1 minutes and 15 minutes in Example 9, and 45.1 minutes and 20 minutes in Example 10.
[0123] [Table 4]
[0124] Examples 5 to 10 confirm that the longer the holding time at the heat treatment temperature, the higher the chroma C. * The greater the tendency, the larger △E becomes. * The more it tends to decrease, the more likely it is to be visually recognized as having the same hue as a long-sintered body.
[0125] Example 11 The pre-sintered body obtained by the same method as in Reference Example 1 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled to 1000°C and held at this temperature for 10 minutes to perform heat treatment. It was then removed from the sintering furnace to obtain a sintered body of this embodiment containing terbium and yttrium-stabilized zirconium oxide with an alumina content of 0.05 mol% by mass, and the remainder being terbium with a terbium content of 0.034 mol% and yttrium with a yttrium content of 4.0 mol%. The results are shown in the table below. The time required from heating the pre-sintered body to the end of the heat treatment was 50.1 minutes, and the heat treatment time was 15 minutes.
[0126] [Table 5]
[0127] Even when heat treatment is performed during the cooling process after holding at the sintering temperature, ΔE can be confirmed. * The temperature is reduced. This confirms that even when heating, sintering, heat treatment, and cooling are set as a single sintering cycle, it is possible to produce sintered bodies that are visually recognizable as having the same color tone as those sintered over a long period.
[0128] Refer to Example 2 (Fabrication of sintered bodies based on long-term sintering) A slurry containing 4.0 mol% yttrium-stabilized zirconium oxide, α-alumina, iron hydroxide, and pure water was mixed in a 2.3 L container and spray-dried at 180 °C to obtain granular powder containing 0.05 wt% alumina and 0.2 wt% iron, with the remainder being 4.0 mol% yttrium-stabilized zirconium oxide (granular powder containing alumina and iron hydroxide). The BET specific surface area of the obtained granular powder was 10.2 m². 2 / g and an average particle size of 45μm.
[0129] In addition to using the obtained particulate powder, the pre-sintered body of yttrium-stabilized zirconia (containing alumina and iron oxide) was obtained by molding and pre-sintering in the same manner as in Reference Example 1.
[0130] In addition to using the obtained pre-sintered body, a sintered body of yttrium-stabilized zirconia containing 0.05 wt% alumina and 0.2 wt% iron, comprising alumina and iron oxide, and with the remainder being 4.0 mol% yttrium, was obtained by the same method as in Reference Example 1 (a sintered body of yttrium-stabilized zirconia containing alumina and iron oxide). The hue L of the sintered body in Reference Example 2... * a * and b * The values are 68.2, 3.52, and 20.70, respectively.
[0131] Examples 12 and 13, Comparative Example 3 Using a pre-sintered body obtained by the same method as in Reference Example 2, and a sintered body taken out and placed in another firing furnace preheated to 900°C, both were heat-treated by holding for the holding times shown in Table 6, and then taken out of the firing furnace. Otherwise, by the same method as in Example 1, a sintered body of yttrium-stabilized zirconium oxide containing 0.05% by mass of alumina and 0.2% by mass of iron, comprising alumina and iron oxide, and with the remainder being 4.0 mol% of yttrium was obtained (yttrium-stabilized zirconium oxide sintered body containing alumina and iron oxide). It should be noted that for Comparative Example 3, no heat treatment was performed, and the sintered body taken out of the firing furnace was used as the sintered body of Comparative Example 3.
[0132] [Table 6]
[0133] Even in sintered bodies of colored zirconia containing iron (iron oxide) that is not dissolved in zirconia, it can be confirmed that the heat treatment process ΔE * The lower the temperature, and the longer the heat treatment time, the better. * The lower it is. It should be noted that L in Example 2... * The value is 68.2, therefore it can be confirmed that in sintered bodies of colored zirconia containing iron (iron oxide), the lightness L can be increased through heat treatment. * Similar to long-sintered bodies, this results in a color difference ΔE * It gets smaller.
[0134] Examples 14 and 15 The pre-sintered body obtained by the same method as in Reference Example 2 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min, held at this sintering temperature for 15 minutes to form a sintered body, and then cooled to 1000°C and removed from the sintering furnace. Next, the removed sintered body was placed in another firing furnace preheated to the heat treatment temperatures shown in Table 7, held for 5 minutes for heat treatment, and then removed from the firing furnace to obtain: a sintered body of yttrium-stabilized zirconium oxide containing 0.05% by mass of alumina, 0.2% by mass of iron, and 4.0 mol% by mass of yttrium (a sintered body of yttrium-stabilized zirconium oxide containing alumina and iron oxide). In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment was 39.0 minutes, and the heat treatment time was 5 minutes.
[0135] [Table 7]
[0136] Even with short holding times, a heat treatment process exceeding 900°C can confirm an increase in ΔE compared to heat treatment at 900°C. * Furthermore, it can be confirmed that ΔE decreases at 1100℃ (above 900℃ but below 1200℃). * It has been significantly reduced.
[0137] Refer to Example 3 (Fabrication of sintered bodies based on long-term sintering) A slurry containing 4.0 mol% yttrium-stabilized zirconium oxide, α-alumina, titanium dioxide, cobalt tetroxide, and pure water was mixed in a 2.3 L container and spray-dried at 180 °C to obtain a granular powder containing 0.05 wt% alumina, 0.2 wt% titanium dioxide, and 0.04 wt% cobalt oxide, with the remainder being 4.0 mol% yttrium-stabilized zirconium oxide granules (granular powder containing alumina, titanium dioxide, and cobalt tetroxide). The BET specific surface area of the obtained granular powder was 10.2 m². 2 / g and an average particle size of 45μm.
[0138] In addition to using the obtained particulate powder, the same molding and pre-sintering method as in Reference Example 1 was used to obtain a pre-sintered body of yttrium-stabilized zirconium oxide containing alumina, titanium oxide, and cobalt tetroxide, with the following composition: 0.05 wt% alumina, 0.2 wt% titanium, and 0.04 wt% cobalt, and the remainder being 4.0 mol% yttrium.
[0139] In addition to using the obtained pre-sintered body, a sintered body containing alumina, titanium oxide, and cobalt tetroxide, with a content of 0.05 wt%, titanium oxide, and cobalt tetroxide, and the remainder being 4.0 mol% yttrium-stabilized zirconium oxide (a sintered body containing alumina, titanium oxide, and cobalt tetroxide), was obtained by the same method as in Reference Example 1. The hue of the sintered body in Reference Example 3 is L. * a * and b * The values are 61.8, 3.33, and -4.96, respectively.
[0140] Example 16, Comparative Example 4 Using the pre-sintered body obtained in Reference Example 3, and a sintered body taken out and preheated to 900°C in another firing furnace, both were heat-treated by holding for the holding times shown in Table 8, and then taken out of the firing furnace. Otherwise, by the same method as in Example 1, a sintered body containing 0.05% by mass of alumina, 0.2% by mass of titanium, and 0.04% by mass of cobalt, comprising alumina, titanium oxide, and cobalt tetroxide, with the remainder being 4.0 mol% yttrium-stabilized zirconium oxide (a sintered body containing alumina, titanium oxide, and cobalt tetroxide) was obtained. It should be noted that for Comparative Example 4, no heat treatment was performed, and the sintered body taken out of the firing furnace was used as the sintered body of Comparative Example 4.
[0141] [Table 8]
[0142] Even in sintered bodies of colored zirconium oxide containing both titanium (Ti) dissolved in zirconium oxide and cobalt insoluble in zirconium oxide, it can be confirmed that the heat treatment process ΔE * The sintering process reduces the color intensity and produces a sintered body that is visually recognized as having the same hue as a long-sintered body.
[0143] Refer to Example 4 (Fabrication of sintered bodies based on long-term sintering) A slurry containing 4.0 mol% yttrium-stabilized zirconium oxide, α-alumina, manganese tetroxide, and pure water was mixed in a 2.3 L container and spray-dried at 180 °C to obtain granular powder containing 0.05 wt% alumina and 0.01 wt% manganese, with the remainder being 4.0 mol% yttrium-stabilized zirconium oxide (granular powder containing alumina and manganese tetroxide). The BET specific surface area of the obtained granular powder was 10.2 m². 2 / g and an average particle size of 45μm.
[0144] In addition to using the obtained particulate powder, the pre-sintered body of yttrium-stabilized zirconium oxide (containing alumina and manganese tetroxide) was obtained by molding and pre-sintering in the same manner as in Reference Example 1.
[0145] In addition to using the obtained pre-sintered body, a sintered body of yttrium-stabilized zirconium oxide (containing alumina and manganese tetroxide) was obtained by the same method as in Reference Example 1, comprising alumina and manganese tetroxide, with the remainder being 4.0 mol% yttrium. The sintered body of Reference Example 4 had a color tone L. * a * and b * The values are 62.4, 2.63, and -1.88, respectively.
[0146] Examples 17 to 19, Comparative Example 5 Using a pre-sintered body obtained by the same method as in Reference Example 4, and a sintered body taken out and preheated in another firing furnace at the temperatures shown in Table 9, both were heat-treated by holding for the holding times shown in Table 9, and then taken out of the firing furnace. Otherwise, by the same method as in Example 14, a sintered body of yttrium-stabilized zirconium oxide with an alumina content of 0.05 wt%, a manganese content of 0.01 wt%, and a remaining yttrium content of 4.0 mol% was obtained (yttrium-stabilized zirconium oxide sintered body containing alumina and manganese tetroxide). It should be noted that for Comparative Example 5, no heat treatment was performed, and the sintered body taken out of the firing furnace was used as the sintered body of Comparative Example 5.
[0147] [Table 9]
[0148] Even in sintered bodies of colored zirconia containing manganese, the presence of heat treatment process ΔE can be confirmed. * The temperature was lowered, resulting in a sintered body with a color tone visually recognized as the same as that of a long-sintered body. Furthermore, it was confirmed that when the heat treatment temperature is above 1000°C and below 1100°C, ΔE... * It has been significantly reduced.
[0149] Refer to Example 5 (Fabrication of sintered bodies based on long-term sintering) Terbium, erbium, and yttrium-stabilized zirconium oxide (0.002 mol%, erbium 0.050 mol%, and yttrium 4.0 mol%), α-alumina, cobalt tetroxide, titanium oxide, and pure water were placed in a 2.3 L container and mixed using a ball mill to obtain a slurry. The slurry was then spray-dried at 180 °C to obtain a granular powder containing 0.05 mol% alumina, 0.003 mol% cobalt, and 0.015 mol% titanium oxide, with the remainder being 0.002 mol% terbium, 0.050 mol% erbium, and 4.0 mol% yttrium stabilized zirconium oxide particles (granular powder containing alumina, cobalt tetroxide, and titanium oxide). The obtained particulate powder has a BET specific surface area of 10.2 m². 2 / g and an average particle size of 43μm.
[0150] In addition to using the obtained particulate powder, a sintered body was obtained by molding, pre-sintering, and sintering in the same manner as in Reference Example 1, and this was used as the sintered body of Reference Example 5. The hue L of the sintered body of Reference Example 5 is... * a * and b * The values are 76.1, -0.24, and 3.95, respectively.
[0151] Refer to Example 6 (Fabrication of sintered bodies based on long-term sintering) Terbium, erbium, and yttrium-stabilized zirconium oxide (0.007 mol%, erbium 0.050 mol%, and yttrium 4.0 mol%), α-alumina, cobalt tetroxide, titanium oxide, and pure water were placed in a 2.3 L container and mixed using a ball mill to obtain a slurry. The slurry was then spray-dried at 180 °C to obtain a granular powder containing 0.05 mol% alumina, 0.007 mol% cobalt, and 0.035 mol% titanium oxide, with the remainder being 0.007 mol% terbium, 0.050 mol% erbium, and 4.0 mol% yttrium stabilized zirconium oxide particles (granular powder containing alumina, cobalt tetroxide, and titanium oxide). The obtained granular powder has a BET specific surface area of 10.1 m². 2 / g and an average particle size of 44μm.
[0152] In addition to using the obtained particulate powder, a sintered body was obtained by molding, pre-sintering, and sintering in the same manner as in Reference Example 1, and this was used as the sintered body of Reference Example 6. The hue L of the sintered body of Reference Example 6... * a * and b * The values are 71.9, -0.23, and 10.46, respectively.
[0153] Refer to Example 7 (Fabrication of sintered bodies based on long-term sintering) Terbium, erbium, and yttrium-stabilized zirconium oxide (0.016 mol%, erbium 0.254 mol%, and yttrium 3.8 mol%), α-alumina, cobalt tetroxide, titanium oxide, and pure water were placed in a 2.3 L container and mixed using a ball mill to obtain a slurry. The slurry was then spray-dried at 180 °C to obtain a granular powder containing terbium, erbium, and yttrium-stabilized zirconium oxide with 0.05 wt% alumina, 0.007 wt% cobalt, and 0.035 wt% titanium oxide, containing alumina, cobalt tetroxide, and titanium oxide, with the remainder being 0.016 mol% terbium, 0.254 mol% erbium, and 3.8 mol% yttrium. The obtained particulate powder has a BET specific surface area of 10.1 m². 2 / g and an average particle size of 44μm.
[0154] In addition to using the obtained particulate powder, a sintered body was obtained by molding, pre-sintering, and sintering in the same manner as in Reference Example 1, and this was used as the sintered body of Reference Example 7. The hue L of the sintered body of Reference Example 7... * a * and b * The values are 67.8, -1.81, and 12.93, respectively. Refer to Example 8 (Fabrication of sintered bodies based on long-term sintering) Erbium and yttrium stabilized zirconium oxide (0.033 mol% erbium and 3.9 mol% yttrium), α-alumina, iron hydroxide, cobalt tetroxide, and pure water were placed in a 2.3 L container and mixed using a ball mill to obtain a slurry. The slurry was then spray-dried at 180 °C to obtain a granular powder containing 0.05 wt% alumina, 0.047 wt% iron, and 0.003 wt% cobalt, as well as alumina, iron hydroxide, and cobalt tetroxide, with the remainder being erbium and yttrium stabilized zirconium oxide granules (containing alumina, iron hydroxide, and cobalt tetroxide). The BET specific surface area of the obtained granular powder was 10.2 m². 2 / g and an average particle size of 44μm.
[0155] In addition to using the obtained particulate powder, a sintered body was obtained by molding, pre-sintering, and sintering in the same manner as in Reference Example 1, and this was used as the sintered body of Reference Example 8. The hue L of the sintered body of Reference Example 8... * a * and b *The values are 75.2, -0.97, and 7.09, respectively. Refer to Example 9 (Fabrication of sintered bodies based on long-term sintering) Erbium and yttrium stabilized zirconium oxide (0.033 mol% erbium and 3.8 mol% yttrium), α-alumina, iron hydroxide, cobalt tetroxide, and pure water were placed in a 2.3 L container and mixed using a ball mill to obtain a slurry. The slurry was then spray-dried at 180 °C to obtain a granular powder containing 0.05 wt% alumina, 0.128 wt% iron, and 0.006 wt% cobalt, as well as alumina, iron hydroxide, and cobalt tetroxide, with the remainder being erbium and yttrium stabilized zirconium oxide granules (containing alumina, iron hydroxide, and cobalt tetroxide). The BET specific surface area of the obtained granular powder was 10.2 m². 2 / g and an average particle size of 44μm.
[0156] In addition to using the obtained particulate powder, a sintered body was obtained by molding, pre-sintering, and sintering in the same manner as in Reference Example 1, and this was used as the sintered body of Reference Example 9. The hue L of the sintered body of Reference Example 9... * a * and b * The figures are 68.5, 1.76, and 14.00, respectively.
[0157] Examples 20 to 22 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled from 1200°C to a heat treatment temperature of 600°C at a cooling rate of 20°C / min and held at this temperature for the holding times shown in Table 10 to perform heat treatment. After being removed from the sintering furnace, the sintered body of this embodiment (containing alumina, cobalt tetroxide, and titanium oxide) was obtained, which has an alumina content of 0.05 mol%, a cobalt content of 0.003 mol%, and a titanium content of 0.015 mol%, and the remainder is terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.002 mol%, an erbium content of 0.050 mol%, and a yttrium content of 4.0 mol%. The time required from heating the pre-sintered body to the end of the heat treatment was 65.0 minutes in Example 20, 70.0 minutes in Example 21, and 80.0 minutes in Example 22. Furthermore, the residence time during the cooling process after holding at the sintering temperature was 31.0 minutes in all examples.
[0158] Examples 23 and 24 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled from 1200°C to a heat treatment temperature of 900°C at a cooling rate of 35.0°C / min and held at this temperature for the holding times shown in Table 10 to perform heat treatment. After being removed from the sintering furnace, the sintered body of this embodiment (containing alumina, cobalt tetroxide, and titanium oxide) was obtained, which has an alumina content of 0.05 mol%, a cobalt content of 0.003 mol%, and a titanium content of 0.015 mol%, and the remainder is terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.002 mol%, an erbium content of 0.050 mol%, and a yttrium content of 4.0 mol%. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment is 41.8 minutes in Example 23 and 46.8 minutes in Example 24. Furthermore, during the cooling process after holding at the sintering temperature, the residence time is 10.0 minutes in both embodiments.
[0159] Examples 25 and 26 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled from 1200°C to a heat treatment temperature of 1000°C at a cooling rate of 40.0°C / min and held at this temperature for the holding times shown in Table 10 to perform heat treatment. After being removed from the sintering furnace, the sintered body of this embodiment (containing alumina, cobalt tetroxide, and titanium oxide) was obtained, which has an alumina content of 0.05 mol%, a cobalt content of 0.003 mol%, and a titanium content of 0.015 mol%, and the remainder is terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.002 mol%, an erbium content of 0.050 mol%, and a yttrium content of 4.0 mol%. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment is 39.0 minutes in Example 25 and 44.0 minutes in Example 26. Furthermore, during the cooling process after holding at the sintering temperature, the residence time is 5.0 minutes in both embodiments.
[0160] Examples 27 and 28 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled to 1200°C and held at this temperature for the holding times shown in Table 10 to perform heat treatment. Then, it was cooled to 1000°C in the furnace and removed from the sintering furnace to obtain a sintered body of this embodiment containing 0.05 mol% alumina, 0.003 mol% cobalt, and 0.015 mol% titanium, and containing alumina, cobalt tetroxide, and titanium oxide, with the remainder being 0.002 mol% terbium, 0.050 mol% erbium, and 4.0 mol% yttrium stabilized zirconium oxide (a sintered body containing alumina, cobalt tetroxide, and titanium oxide). In any of the embodiments, the time required from the heating of the pre-sintered body to the end of the heat treatment process is 39.0 minutes in Example 27 and 44.0 minutes in Example 28.
[0161] Comparative Example 6 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled to 1000°C and removed from the sintering furnace to obtain a sintered body containing alumina, cobalt tetroxide, and titanium oxide with a content of 0.05 mol% alumina, 0.003 mol% cobalt, and 0.015 mol% titanium oxide, and the remainder being terbium, erbium, and yttrium stabilized zirconium oxide (a sintered body containing alumina, cobalt tetroxide, and titanium oxide). This body was used as the sintered body of Comparative Example 6.
[0162] Comparative Example 7 The pre-sintered body obtained by the same method as in Reference Example 5 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled to 1300°C and held at this temperature for heat treatment. Then, it was cooled to 1000°C in the furnace and removed from the sintering furnace to obtain a sintered body containing alumina, cobalt tetroxide, and titanium oxide with a content of 0.05 mol% alumina, 0.003 mol% cobalt, and 0.015 mol% titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a content of 0.002 mol% terbium, 0.050 mol% erbium, and 4.0 mol% yttrium. The time required from heating to the end of the heat treatment was 44.0 minutes.
[0163] Examples 29 to 31 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered and heat-treated by the same method as in Examples 20 to 22 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 mol%, a cobalt content of 0.007 mol%, and a titanium content of 0.035 mol%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.007 mol%, an erbium content of 0.050 mol%, and yttrium content of 4.0 mol%.
[0164] Examples 32 and 33 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered and heat-treated by the same method as in Examples 23 and 24 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 mol%, a cobalt content of 0.007 mol%, and a titanium content of 0.035 mol%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.007 mol%, an erbium content of 0.050 mol%, and yttrium content of 4.0 mol%.
[0165] Examples 34 and 35 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered and heat-treated by the same method as in Examples 25 and 26 to obtain: a terbium, erbium and yttrium stabilized zirconium oxide containing alumina, cobalt tetroxide and titanium oxide, with the remaining portion being terbium, erbium and yttrium stabilized zirconium oxide containing alumina, cobalt tetroxide and titanium oxide.
[0166] Examples 36 and 37 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered by the same method as in Examples 27 and 28 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 mol%, a cobalt content of 0.007 mol%, and a titanium content of 0.035 mol%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.007 mol%, an erbium content of 0.050 mol%, and yttrium content of 4.0 mol%.
[0167] Comparative Example 8 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered by the same method as in Comparative Example 6 to obtain a sintered body containing alumina, cobalt tetroxide and titanium oxide with a content of 0.05 mol% alumina, 0.007 mol% cobalt and 0.035 mol% titanium oxide, and the remainder being a terbium, erbium and yttrium stabilized zirconium oxide sintered body (a terbium, erbium and yttrium stabilized zirconium oxide sintered body containing alumina, cobalt tetroxide and titanium oxide), which was used as the sintered body of Comparative Example 8.
[0168] Comparative Example 9 The pre-sintered body obtained by the same method as in Reference Example 6 was sintered and heat-treated by the same method as in Comparative Example 7 to obtain a sintered body containing alumina, cobalt tetroxide and titanium oxide with a content of 0.05 mol% alumina, 0.007 mol% cobalt and 0.035 mol% titanium oxide, and the remainder being terbium, erbium and yttrium stabilized zirconium oxide (a sintered body containing alumina, cobalt tetroxide and titanium oxide). This body was used as the sintered body of Comparative Example 9.
[0169] Examples 38 to 40 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered and heat-treated by the same method as in Examples 20 to 22 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 wt%, a cobalt content of 0.007 wt%, and a titanium content of 0.035 wt%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.016 mol%, an erbium content of 0.254 mol%, and yttrium content of 3.8 mol%.
[0170] Examples 41 and 42 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered and heat-treated by the same method as in Examples 23 and 24 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 wt%, a cobalt content of 0.007 wt%, and a titanium content of 0.035 wt%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.016 mol%, an erbium content of 0.254 mol%, and yttrium content of 3.8 mol%.
[0171] Examples 43 and 44 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered and heat-treated by the same method as in Examples 25 and 26 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 wt%, a cobalt content of 0.007 wt%, and a titanium content of 0.035 wt%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.016 mol%, an erbium content of 0.254 mol%, and yttrium content of 3.8 mol%.
[0172] Examples 45 and 46 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered and heat-treated by the same method as in Examples 27 and 28 to obtain a sintered body of this embodiment containing terbium, erbium, and yttrium-stabilized zirconium oxide with an alumina content of 0.05 wt%, a cobalt content of 0.007 wt%, and a titanium content of 0.035 wt%, containing alumina, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium-stabilized zirconium oxide with a terbium content of 0.016 mol%, an erbium content of 0.254 mol%, and yttrium content of 3.8 mol%.
[0173] Comparative Example 10 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered by the same method as in Comparative Example 6 to obtain a sintered body containing alumina, cobalt tetroxide and titanium oxide with a content of 0.05 mol% alumina, 0.007 mol% cobalt and 0.035 mol% titanium oxide, and the remainder being a terbium, erbium and yttrium stabilized zirconium oxide sintered body (a terbium, erbium and yttrium stabilized zirconium oxide sintered body containing alumina, cobalt tetroxide and titanium oxide), which was used as the sintered body of Comparative Example 10.
[0174] Comparative Example 11 The pre-sintered body obtained by the same method as in Reference Example 7 was sintered and heat-treated by the same method as in Comparative Example 7 to obtain a sintered body containing alumina, cobalt tetroxide and titanium oxide with a content of 0.05 mol% by mass, cobalt tetroxide and titanium oxide, and the remainder being terbium 0.016 mol% by mass, erbium 0.254 mol% by mass and yttrium 3.8 mol% by mass. This sintered body was used as the sintered body of Comparative Example 11.
[0175] [Table 10]
[0176] As can be confirmed from Examples and Comparative Examples 6, 8 and 10, sintered bodies containing terbium, erbium, cobalt and titanium as coloring elements, after heat treatment, ΔE * The temperature decreases. Furthermore, as confirmed by Comparative Examples 7, 9, and 11, when the heat treatment temperature is set to 1300°C, ΔE is not obtained. * The effect of reduction. Furthermore, compared to Comparative Example 6, the chroma C of Examples 20 to 28... * All were above 0.7; compared to Comparative Example 8, the chroma C of Examples 29 to 37 was... * All were above 1.6; compared to Comparative Example 10, the chroma C of Examples 38 to 46 were... * All values are above 2.3; chroma C can be confirmed. * It gets bigger.
[0177] In addition, it can be confirmed that the sintered bodies of Examples 20 to 28 have a hue equivalent to C1 of VITA Classical Shade, the sintered bodies of Examples 29 to 37 have a hue equivalent to C3 of VITA Classical Shade, and the sintered bodies of Examples 38 to 46 have a hue equivalent to C4 of VITA Classical Shade.
[0178] Examples 47 and 48 The pre-sintered body obtained by the same method as in Reference Example 8 was heated to a sintering temperature of 1560°C at a heating rate of 177°C / min and held at this sintering temperature for 15 minutes. After holding at the sintering temperature, it was cooled from 1200°C to a heat treatment temperature of 600°C at a cooling rate of 20.0°C / min and held at this temperature for the holding times shown in Table 11 to perform heat treatment. After being removed from the sintering furnace, the sintered body of this embodiment (containing alumina, iron oxide, and cobalt tetroxide) was obtained, which has an alumina content of 0.05 mol%, an iron content of 0.047 mol%, and a cobalt content of 0.003 mol%, and contains erbium and yttrium stabilized zirconium oxide of 0.033 mol% and yttrium of 3.9 mol%. In any embodiment, the time required from heating the pre-sintered body to the end of the heat treatment is 65.0 minutes in Example 47 and 70.0 minutes in Example 48. Furthermore, during the cooling process after holding at the sintering temperature, the residence time is 31.0 minutes in all embodiments.
[0179] Examples 49 and 50 The pre-sintered body obtained by the same method as in Reference Example 8 was sintered and heat-treated by the same method as in Examples 27 and 28 to obtain the sintered body of this embodiment containing 0.05 mol% alumina, 0.047 mol% iron, and 0.003 mol% cobalt, containing alumina, iron oxide, and cobalt tetroxide, with the remainder being 0.033 mol% erbium and 3.9 mol% yttrium stabilized zirconium oxide.
[0180] Comparative Example 12 The pre-sintered body obtained by the same method as in Reference Example 8 was sintered by the same method as in Comparative Example 6 to obtain a sintered body of erbium and yttrium stabilized zirconium oxide containing alumina, iron oxide, and cobalt tetroxide, with the remainder being erbium 0.033 mol% and yttrium 3.9 mol% (erbium and yttrium stabilized zirconium oxide sintered body containing alumina, iron oxide, and cobalt tetroxide). This was used as the sintered body of Comparative Example 12.
[0181] Comparative Example 13 The pre-sintered body obtained by the same method as in Reference Example 8 was sintered and heat-treated by the same method as in Comparative Example 7 to obtain a sintered body of erbium and yttrium stabilized zirconium oxide containing alumina, iron oxide and cobalt tetroxide, with the remainder being erbium 0.033 mol% and yttrium 3.9 mol% (erbium and yttrium stabilized zirconium oxide sintered body containing alumina, iron oxide and cobalt tetroxide). This was used as the sintered body of Comparative Example 13.
[0182] Examples 51 and 52 The pre-sintered body obtained by the same method as in Reference Example 9 was sintered and heat-treated by the same method as in Examples 47 and 48 to obtain the sintered body of this embodiment containing 0.05 mol% alumina, 0.128 mol% iron, and 0.006 mol% cobalt, containing alumina, iron oxide, and cobalt tetroxide, with the remainder being 0.033 mol% erbium and 3.8 mol% yttrium stabilized zirconium oxide.
[0183] Examples 53 and 54 The pre-sintered body obtained by the same method as in Reference Example 9 was sintered and heat-treated by the same method as in Examples 27 and 28 to obtain the sintered body of this embodiment containing 0.05 mol% alumina, 0.128 mol% iron, and 0.006 mol% cobalt, containing alumina, iron oxide, and cobalt tetroxide, with the remainder being 0.033 mol% erbium and 3.8 mol% yttrium stabilized zirconium oxide.
[0184] Comparative Example 14 The pre-sintered body obtained by the same method as in Reference Example 9 was sintered by the same method as in Comparative Example 6 to obtain a sintered body of erbium and yttrium stabilized zirconium oxide containing alumina, iron oxide, and cobalt tetroxide, with the remainder being erbium 0.033 mol% and yttrium 3.8 mol%. This body was used as the sintered body of Comparative Example 14.
[0185] Comparative Example 15 The pre-sintered body obtained by the same method as in Reference Example 9 was sintered and heat-treated by the same method as in Comparative Example 7 to obtain a sintered body containing alumina (0.05 mol% by mass), iron (0.128 mol% by mass), cobalt (0.006 mol% by mass), containing alumina, iron oxide, and cobalt tetroxide, with the remainder being erbium and yttrium stabilized zirconium oxide (0.033 mol% by mass and 3.8 mol% by mass). This was used as the sintered body of Comparative Example 15.
[0186] [Table 11]
[0187] As can be confirmed from Examples and Comparative Examples 12 and 14, sintered bodies containing iron, erbium, cobalt, and titanium as coloring elements, after heat treatment, ΔE * The temperature decreases. Furthermore, as confirmed by Comparative Examples 13 and 15, when heat treatment is performed at a temperature of 1300°C, ΔE is not obtained. * The effect of reduction. Furthermore, compared to Comparative Example 12, the chroma C of Examples 47 to 50... * All were above 1.0; compared to Comparative Example 14, the chroma C of Examples 51 to 54 was 1.0 or higher. * All values are above 2.0; chroma C can be confirmed. * It gets bigger.
[0188] In addition, it can be confirmed that the sintered bodies of Examples 47 to 50 have a hue equivalent to C1 of VITA Classical Shade, and the sintered bodies of Examples 51 to 54 have a hue equivalent to C4 of VITA Classical Shade.
[0189] Comparative Example 16 After mirror polishing both surfaces of the sintered body obtained in Comparative Example 10 until the surface roughness Ra≤0.02μm, a commercially available polishing agent (product name: CERABIEN ZR, manufactured by Kuraray Noritake Dental) was applied to one side of the body. The sintered body was placed in a firing furnace preheated to 900°C and held for 10 minutes for heat treatment. After being removed from the firing furnace, a sintered body containing alumina, cobalt tetroxide, and titanium oxide with a content of 0.05 wt%, cobalt tetroxide, and titanium oxide, and the remainder being terbium, erbium, and yttrium stabilized zirconium oxide with a content of 0.016 mol%, erbium tetroxide, and 3.8 mol% yttrium was obtained. The surface of the sintered body was coated with a polishing agent on one side.
[0190] Comparative Example 17 In addition to using the sintered body obtained in Comparative Example 14, a sintered body containing alumina, iron oxide, and cobalt tetroxide, with the following composition (a sintered body containing alumina, iron oxide, and cobalt tetroxide) and the remainder being erbium and yttrium stabilized zirconium oxide with a content of 0.05 mol% alumina, 0.128 mol% iron, and 0.006 mol% cobalt, and the remainder being erbium and yttrium stabilized zirconium oxide with a content of 0.033 mol% erbium and 3.8 mol% yttrium, was obtained by the same method as in Comparative Example 16. One side of the sintered body was covered with a polishing agent.
[0191] By mirror polishing the surfaces of the sintered bodies of Comparative Examples 16 and 17 covered with polishing agent to remove the polishing agent, sintered bodies with a surface roughness Ra≤0.02μm were prepared, and the hue of the surface coated with glaze was measured.
[0192] [Table 12]
[0193] Comparative Examples 16 and 17 confirm that colored zirconia sintered bodies with a surface coating of polishing agent cannot obtain ΔE after heat treatment. * The effect of reduction.
[0194] The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2021-076347, filed on April 28, 2021, are incorporated herein by reference and are incorporated as a disclosure of this disclosure.
Claims
1. A method for manufacturing a sintered body, characterized in that, It has a process for heat-treating sintered bodies containing coloring elements of zirconium oxide at a temperature above 600°C and below 1200°C under an oxidizing atmosphere. The heat treatment time is between 5 and 20 minutes. Prior to the heat treatment step, a sintering step is performed to sinter the colored zirconium oxide at a temperature below 1600°C under an oxidizing atmosphere to obtain the sintered body containing the coloring element. The sintering process does not involve pressure sintering. The total time required for the sintering process and the heat treatment process is less than 3 hours, and, The coloring element is selected from one or more of the group consisting of iron, cobalt, manganese, nickel, copper, titanium, chromium, cerium, praseodymium, neodymium, erbium, terbium and ytterbium.
2. The manufacturing method according to claim 1, wherein, The sintered body containing the coloring element, zirconium oxide, is a sintered body in the state after sintering under normal pressure.
3. The manufacturing method according to claim 1 or 2, wherein, The sintered body containing the coloring element, zirconium oxide, is a sintered body in the state after sintering under an oxidizing atmosphere.
4. The manufacturing method according to claim 1 or 2, wherein, The heat treatment is a heat treatment that is carried out and held at any heat treatment temperature above 600°C and below 1200°C.
5. The manufacturing method according to claim 4, wherein, The temperature range for the heat treatment is ±50℃.
6. The manufacturing method according to claim 1 or 2, wherein, The atmosphere for the heat treatment is atmospheric.
7. The manufacturing method according to claim 1 or 2, wherein, The heat treatment process involves placing a sintered body containing coloring elements of zirconium oxide in a firing furnace heated to the heat treatment temperature and then heat-treating it.
8. The manufacturing method according to claim 1 or 2, wherein, The heat treatment is performed at a temperature above 700°C and below 1100°C.
9. The manufacturing method according to claim 8, wherein, The sintering process in the sintering step is: sintering colored zirconium oxide at a sintering temperature of above 1400°C and below 1600°C for less than 2 hours.
10. The manufacturing method according to claim 1 or 2, wherein, The heat treatment process involves holding the sample at a sintering temperature, then cooling it to a heat treatment temperature and holding it thereafter.
11. The manufacturing method according to claim 1 or 2, wherein, The sintered body obtained in the heat treatment process is a colored zirconia sintered body that has a lightness difference of 5 or less and a chroma difference of 0.3 or more compared with the zirconia sintered body containing coloring elements supplied to the process, or a lightness difference of more than 5 and a chroma difference of 10 or less.
12. The manufacturing method according to claim 1 or 2, wherein, The coloring element contains at least iron or erbium.
13. The manufacturing method according to claim 1 or 2, wherein, The zirconium oxide contains stabilizing elements.
14. The manufacturing method according to claim 1 or 2, wherein, The zirconium oxide contains at least yttrium.
15. The manufacturing method according to claim 1 or 2, wherein, The sintered zirconium oxide containing coloring elements comprises aluminum oxide (Al2O3).
Citation Information
Patent Citations
Color ceramic
JP2016026990A
Refrigeration cycle device
JP2021076347A
Method of rapid sintering of ceramics
WO2012057829A2
Zirconia powder, method for producing zirconia powder, method for producing zirconia sintered body, and zirconia sintered body
WO2020196650A1
Colored light transmissive zirconia sintered body, manufacturing method therefor, and application therefor
JP2018002495A