A method for solving tire crown blisters and a tire

By improving the structure of the rear pressure roller and bonding differential rubber sheets to the belt layer composite, the problem of air bubbles in the tire crown was solved, improving tire quality stability and production efficiency, and reducing the scrap rate.

CN117245958BActive Publication Date: 2026-11-24SAILUN GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311303130.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-10
Publication Date
2026-11-24
Estimated Expiration
2043-10-10

AI Technical Summary

Technical Problem

Existing technologies, when addressing the issue of air bubbles in tire crowns, require repeated adjustments to the pressing process, which cannot guarantee the stability of tire quality and negatively impacts production efficiency and quality.

Method used

A rear pressure roller with a protrusion in the middle of the roller body is used to press and form the tread and belt layer composite. The belt layer composite adopts a multi-layer structure. Differential rubber sheets are attached at the thickness difference position of the two belt layers adjacent to the tread. The structure of the rear pressure roller is improved to match the shape of the tread and shoulder, and differential rubber sheets are used during the pressing process to reduce the thickness difference.

Benefits of technology

It effectively solved the problem of air bubbles in the tire crown, reduced the scrap rate, improved the stability of tire quality, and avoided the impact on production efficiency caused by repeated adjustments to the pressing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117245958B_ABST
    Figure CN117245958B_ABST
Patent Text Reader

Abstract

This invention relates to a method for resolving tire tread air bubbles and to a tire, belonging to the field of tire manufacturing technology. The method involves using a rear pressure roller with a protrusion in the middle of the roller body to press and shape the tread and the belt layer composite. The belt layer composite has a multi-layer structure, and differential rubber sheets are bonded at the thickness difference positions of the two belt layers adjacent to the tread. This invention can solve the problem in the prior art where repeated adjustments to the pressing process to resolve tread air bubbles cannot guarantee the stability of tire quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of tire manufacturing technology, and specifically relates to a method for solving tire crown air bubbles and a tire. Background Technology

[0002] During tire production, tire crown air bubbles frequently occur. To address this issue, existing technological improvements include adjusting molding and pressing parameters and pressing positions. However, these improvements have minimal effect and cannot effectively resolve tire crown air bubbles, thus affecting tire quality. Furthermore, repeatedly adjusting the pressing process can easily impact production efficiency and fail to guarantee the stability of tire quality. Summary of the Invention

[0003] In view of the various shortcomings of the existing technology, and in order to solve the above problems, a method and a tire for solving tire crown air bubbles are proposed, so as to solve the problem that repeated adjustments to the pressing process to solve tire crown air bubbles cannot guarantee the stability of tire quality in the existing technology.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] In a first aspect, the present invention provides a method for solving air bubbles in tire crowns. In the molding process, a rear pressure roller with a protrusion in the middle of the roller body is used to press and mold the tread and the belt layer composite. The belt layer composite adopts a multi-layer structure, and differential films are attached at the thickness difference positions of the two belt layers adjacent to the tread.

[0006] The technical solution is further configured such that the protrusion includes a main pressing surface and auxiliary pressing surfaces located on both sides of the main pressing surface. The main pressing surface is parallel to the central axis of the roller body, the auxiliary pressing surfaces are inclined, and the distance between the main pressing surface and the central axis of the roller body is greater than the distance between the auxiliary pressing surface and the central axis of the roller body.

[0007] The technical solution is further configured such that, during the compression molding process, the main compression surface contacts the tire tread, the auxiliary compression surface contacts the tire shoulder, and an angle of 15°-75° is formed between the main compression surface and the auxiliary compression surface.

[0008] The technical solution is further configured such that the width of the protrusion is L, and satisfies: L=L1±10mm, where L1 is the width of the belt layer adjacent to the tread, and the width direction is consistent with the width direction of the tire cross section.

[0009] The technical solution is further configured such that the protrusion also includes a side surface that is in contact with the auxiliary pressing surface, and the side surface is perpendicular to the central axis of the roller body.

[0010] The technical solution is further configured such that the height of the side is less than 1 / 2 of the radius of the protrusion.

[0011] The technical solution is further configured such that the tread is composed of multiple layers of rubber sheets, the material of the differential rubber sheets is the same as the material of the bottom layer rubber sheet of the tread, and the bottom layer rubber sheet of the tread is the rubber sheet adjacent to the belt layer composite.

[0012] The technical solution is further configured such that the two belt layers adjacent to the tread are a first belt layer and a second belt layer, the first belt layer is in contact with the tread, the width of the first belt layer is smaller than the width of the second belt layer, and the two sides of the second belt layer are covered with edge-sealing films, and the differential films are connected to the edge-sealing films.

[0013] The technical solution is further configured such that the width of the differential film is L2 and its thickness is H2, and satisfies: L2 / H2=(L3-10)∽(L3-4) / H1±0.1, where L3 is the distance between the edge film of the second belt layer and the first belt layer in the width direction, H1 is the thickness of the edge film, the width direction is consistent with the width direction of the tire cross section, and the thickness direction is perpendicular to the width direction.

[0014] Secondly, the present invention also provides a tire, which includes a tread and a belt layer composite, wherein the belt layer composite adopts a multi-layer structure and differential rubber sheets are bonded at the thickness difference positions of the two belt layers adjacent to the tread.

[0015] The beneficial effects of this invention are:

[0016] By improving the structure of the rear pressure roller, the shape of the rear pressure roller is made to match the shape of the tread and shoulder. Combined with the thickness difference position of the two belt layers adjacent to the tread, the thickness difference is reduced, air pockets are avoided, and the problem of air bubbles in the tread is fundamentally solved. This avoids the impact on production efficiency caused by operators repeatedly adjusting the pressing process, effectively reduces the scrap rate, and improves the stability of tire quality. Attached Figure Description

[0017] Figure 1 This is a diagram showing the relationship between the material distribution and the position of the air bubbles in the tire crown in an embodiment of the present invention;

[0018] Figure 2 This is a schematic diagram of the structure of the rear pressure roller in the prior art;

[0019] Figure 3 This is a schematic diagram of the structure of the rear pressure roller used in an embodiment of the present invention;

[0020] Figure 4 This is a schematic diagram of the four-layer belt layer composite and differential film in an embodiment of the present invention;

[0021] Figure 5 This is a schematic diagram of the three-layer belt layer composite and differential film in an embodiment of the present invention;

[0022] Figure 6 This is a schematic diagram of the two-layer belt layer composite and differential film in an embodiment of the present invention.

[0023] In the attached diagram: 1-roller body, 2-main pressing surface, 3-auxiliary pressing surface, 4-side surface, 5-differential film. Detailed Implementation

[0024] To enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. Based on the embodiments in this application, other similar embodiments obtained by those skilled in the art without creative effort should all fall within the scope of protection of this application. Furthermore, directional terms mentioned in the following embodiments, such as "up," "down," "left," and "right," are only for reference to the directions in the accompanying drawings; therefore, the directional terms used are for illustrative purposes and not for limiting the invention.

[0025] Tire tread bubbles have been observed in various tire manufacturers across China. Observation and cross-sectional analysis of these bubbles revealed the following commonalities: 1. The bubbles are located in roughly the same position, directly above the belt layer composite (including at the belt-to-layer transition). 2. Bubbles are present on both the upper and lower molds, or on one side, and they appear in strings or dots. 3. The bubble surface exhibits a honeycomb-like structure and irregular shape. Analysis of these commonalities suggests that: 1. The bubbles primarily occur above the belt layer composite, possibly due to air pockets caused by the bonding between the belt layer composite and the tread. Because the gas cannot be completely expelled after bonding, the gas between the tread and the belt layer composite requires the assistance of a rear pressure roller in the auxiliary machine for expulsion. However, the existing rear pressure roller design has flaws and cannot effectively and evenly expel the gas. 2. The air bubbles are located at the belt layer difference stage, possibly due to air pockets within that stage. Causes of air pockets at the belt layer difference stage include: insufficient tread pressing pressure preventing air expulsion; poor tread rubber adhesion, hindering effective bonding during pressing; excessively high rear roller pressing speed; or a mismatch between the tread pressing speed and pressure. The above inspection and cross-sectional analysis of the tire crown air bubbles only provide a simple indication that the air pockets are likely caused by pressing issues in the molding process. Therefore, those skilled in the art typically take measures such as adjusting molding pressing parameters and pressing position. These measures only temporarily resolve the air bubble problem above the belt layer composite and do not address the root cause of the air bubble formation mechanism.

[0026] Based on this, the inventors first analyzed the location of air bubbles in the tire crown from the perspective of the generation mechanism: Taking a four-layer belt layer composite as an example, the belt layer composite consists of belt layer #1, belt layer #2, belt layer #3, and belt layer #4 from bottom to top. Among them, belt layer #4 is attached to the tread. Based on the finished cross-section, the air bubble is located directly above belt layer #4. The air bubble is relatively large, and after cutting it open, the surface and interior are rough, and gas is found. The air bubble is about 50-60mm away from the center of the tread. The air bubble is located between belt layers #4 and #3 (i.e., the air bubble is located at the difference in belt layer position). At the same time, the inventors analyzed the positional relationship of the air bubbles in the tire crown based on the material distribution diagram. Please refer to [link / reference]. Figure 1 Furthermore, a bubble machine was used to obtain a bubble location map to further confirm the location of the bubbles.

[0027] Secondly, the inventors analyzed the equipment's suitability for tire products: the width and shape of existing rear pressure rollers remain fixed; please refer to [link to relevant documentation]. Figure 2 The following problems exist during the tread pressing process: Because the width of the rear pressure roller is fixed, when producing narrow-shoulder tires, the edges of the tread are pre-compacted, preventing air from escaping from the center and causing air pockets. When producing wide-shoulder tires, some areas of the tread are not properly rolled, resulting in insufficient compaction and air pockets. Additionally, the shape of the rear pressure roller does not match the tread shape, leading to uneven force on the tread during pressing and causing air pockets.

[0028] Finally, the inventors analyzed the product structure design from the perspective of fulfillment: based on Figure 1 The product structure design requirements have inherent differences, resulting in the following issues: There is a thickness difference between the #3 and #4 belt layers, posing a risk of material loss and air pockets during tread application. Unevenness on the surface of the belt layer composite prevents proper gas escape during tread pressing, leading to air pockets. If the thickness difference between the #3 and #4 belt layers is too small, the tire is prone to crown detachment and blowouts during market use. If the thickness difference between the #3 and #4 belt layers is too large, the risk of crown air bubbles during production is high, and the tire will lack rigidity during later use.

[0029] In summary, the inventors analyzed the bubble generation mechanism above the belt layer composite and made targeted improvements to the structure of the rear pressure roller and the thickness difference between the two belt layers adjacent to the tread to avoid air pockets that could lead to bubble formation.

[0030] According to an embodiment of the present invention, a method for resolving air bubbles in the tire tread is provided. Please refer to [link / reference]. Figures 3 to 6 During the molding process, a rear pressure roller with a protrusion in the middle of roller body 1 is used to press and mold the tread and belt layer composite. The belt layer composite adopts a multi-layer structure, and a differential film 5 is attached at the thickness difference position of the two belt layers adjacent to the tread.

[0031] It should be noted that currently, belt-layer composite components generally adopt a 2-layer, 3-layer, or 4-layer structure.

[0032] Preferably, the roller body 1 is made of nylon, which has extremely high wear resistance, heat resistance, self-smoothing properties and low wear resistance.

[0033] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 3 The protrusion includes a main pressing surface 2 and auxiliary pressing surfaces 3 located on both sides of the main pressing surface 2. The main pressing surface 2 is parallel to the central axis of the roller body, and the auxiliary pressing surfaces 3 are inclined. The distance between the main pressing surface 2 and the central axis of the roller body is greater than the distance between the auxiliary pressing surfaces 3 and the central axis of the roller body.

[0034] Specifically, during the compression molding process, the main compression surface 2 contacts the tire tread and plays a major role in compression and air release on the tire tread, while the auxiliary compression surface 3 contacts the tire shoulder, and the main compression surface 2 and the auxiliary compression surface 3 form an angle of 15°-75°.

[0035] It should be noted that the auxiliary pressing surface 3 is inclined, which allows for better contact with the tire shoulder and prevents air from being trapped at the edges. Preferably, the main pressing surface 2 and the auxiliary pressing surface 3 form an angle of 28°.

[0036] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 3 The width of the protrusion is L, and satisfies: L = L1 ± 10 mm, where L1 is the width of the belt layer adjacent to the tread, that is, the width of the uppermost belt layer, and the width direction is consistent with the width direction of the tire cross section.

[0037] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 3 The protrusion also includes a side surface 4 that is in contact with the auxiliary pressing surface 3, and the side surface 4 is perpendicular to the central axis of the roller body.

[0038] Specifically, the height of the side 4 is less than half the radius of the protrusion, which is beneficial for the pressing force generated by the rear pressure roller to act directly on the tire surface.

[0039] Experiment 1: Design rear pressure rollers of different widths, with the tread size remaining unchanged, and conduct experiments under the same machine and process conditions. The data obtained are shown in Table 1.

[0040] Table 1:

[0041]

[0042]

[0043] Preliminary analysis of the results shown in Table 1 indicates that, under the condition of the same tread width, different widths of the rear pressure rollers affect the air bubbles above the tread. When the width of the rear pressure rollers is 115mm and 95mm, the defect rate of air bubbles in the tread is zero.

[0044] Experiment 2: Using a rear pressure roller with a width of 90mm-120mm, the experiment was conducted on the same machine under the same process conditions. The number of tire inspections was increased to verify the pressing stability. The data obtained are shown in Table 2.

[0045] Table 2:

[0046]

[0047] Preliminary analysis of the results shown in Table 2 indicates that, under the condition that the width of the belt layers adjacent to the tread is the same (105mm), the design width of the rear pressure roller is most in line with the standard when it is between 95mm and 115mm. Therefore, it can be inferred that the crown bubble above the belt layer composite is directly related to the width of the belt layer adjacent to the tread and the width of the rear pressure roller, and satisfies that the width of the protrusion is L, L = L1 ± 10mm, where L1 is the width of the belt layer adjacent to the tread, that is, the width of the uppermost belt layer, and the width direction is consistent with the width direction of the tire cross section.

[0048] In practical applications, a database of the width of the belt layer adjacent to the tread of each tire specification is established. The rear pressure rollers are then processed according to the width of the belt layer adjacent to the tread and stored in categories. The rear pressure rollers of the appropriate width are then replaced according to the tire specification.

[0049] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figures 4-6 The tread is composed of multiple layers of rubber sheets. The material of the differential rubber sheet 5 is the same as that of the bottom layer rubber sheet of the tread. The bottom layer rubber sheet of the tread is the rubber sheet adjacent to the belt layer composite.

[0050] It should be noted that adding differential rubber sheet 5 reduces the differential between belt layers, preventing air pockets at this location. At the same time, adding differential rubber sheet 5 allows for more sufficient flow of rubber material between belt layer differentials, preventing tire delamination problems later on.

[0051] In the method for resolving air bubbles in the tire crown of this embodiment, the two belt layers adjacent to the tread are a first belt layer and a second belt layer. The first belt layer is attached to the tread, and the width of the first belt layer is smaller than the width of the second belt layer. Edge-binding films are attached to both sides of the second belt layer, and the differential film 5 is connected to the edge-binding film.

[0052] Specifically, the width of the differential film 5 is L2, and its thickness is H2, and it satisfies: L2 / H2=(L3-10)∽(L3-4) / H1±0.1, where L3 is the distance between the edge film of the second belt layer and the first belt layer in the width direction, H1 is the thickness of the edge film, the width direction is consistent with the width direction of the tire cross section, and the thickness direction is perpendicular to the width direction.

[0053] Experiment 3: Selecting the 10R22.5 specification, and ensuring that the process conditions remain unchanged, different widths and thicknesses of the differential rubber sheet 5 were selected for the experiment. The selection principle of differential rubber sheet 5 is to minimize cost input, ensure that tire performance is not affected, and ensure that production efficiency is not affected. The data obtained are shown in Table 3.

[0054] Table 3:

[0055]

[0056]

[0057] Experiment 4: To verify the stability of the results shown in Table 3 during continuous production, the number of experiments was increased according to the above scheme and the verification was continued. The data obtained are shown in Table 4.

[0058] Table 4:

[0059]

[0060] Preliminary analysis of the results shown in Table 4 indicates that no crown bubbles appeared when the width of the differential rubber sheet 5 was 17mm-23mm and the thickness was 0.7mm-0.8mm. This suggests a direct relationship between the crown bubbles above the belt layer composite and the width and thickness of the differential rubber sheet 5. Specifically, the differential rubber sheet 5 has a width of L2 and a thickness of H2, where L2 / H2 = (L3-10)∽(L3-4) / H1±0.1. Here, L3 is the distance between the second belt layer's edge rubber sheet and the first belt layer in the width direction, and H1 is the thickness of the edge rubber sheet. The width direction is consistent with the width direction of the tire cross-section, and the thickness direction is perpendicular to the width direction. Preferably, the differential rubber sheet 5 is rectangular.

[0061] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 4 The belt layer composite adopts a 4-layer structure, which consists of belt layer 1, belt layer 2, belt layer 3 and belt layer 4 from bottom to top. Among them, belt layer 4 is bonded to the tread. At this time, belt layer 4 serves as the first belt layer and belt layer 3 serves as the second belt layer. The differential film 5 is located at the thickness difference level between belt layer 4 and belt layer 3.

[0062] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 5The belt layer composite adopts a 3-layer structure, consisting of belt layer 1, belt layer 2, and belt layer 3 from bottom to top. Belt layer 3 is bonded to the tread. At this time, belt layer 3 serves as the first belt layer, belt layer 2 serves as the second belt layer, and the differential film 5 is located at the thickness difference level between belt layer 3 and belt layer 2.

[0063] For the method of resolving air bubbles in the tire tread in this embodiment, please refer to [link / reference]. Figure 6 The belt layer composite adopts a two-layer structure, consisting of belt layer #1 and belt layer #2 from bottom to top. Belt layer #2 is bonded to the tread. At this time, belt layer #2 serves as the first belt layer and belt layer #1 serves as the second belt layer. The differential film 5 is located at the thickness difference level between belt layer #2 and belt layer #1.

[0064] According to an embodiment of the present invention, a tire is provided, which includes a tread and a belt layer composite, wherein the belt layer composite adopts a multi-layer structure and differential rubber sheets are bonded at the thickness difference positions of the two belt layers adjacent to the tread.

[0065] The present invention has been described in detail above. The above description is only a preferred embodiment of the present invention and should not be construed as limiting the scope of the present invention. All equivalent changes and modifications made in accordance with the scope of this application should still fall within the scope of the present invention.

Claims

1. A method for solving tire crown blisters, characterized in that, During the molding process, a rear pressure roller with a protrusion in the middle of the roller body is used to press and mold the tread and the belt layer composite. The belt layer composite adopts a multi-layer structure. The two belt layers adjacent to the tread are the first belt layer and the second belt layer. The first belt layer is attached to the tread. The two sides of the second belt layer are covered with edge wrapping film. At the thickness difference position of the two belt layers adjacent to the tread, a differential film is attached. The differential film is connected to the edge wrapping film, increasing the differential film and reducing the thickness difference between the belt layers. The width of the protrusion is L, and satisfies: L=L1±10mm, where L1 is the width of the belt layer adjacent to the tread, and the width direction is consistent with the width direction of the tire cross section. The width of the differential film is L2, and its thickness is H2, and it satisfies: L2 / H2=(L3-10)∽(L3-4) / H1±0.1, where L3 is the distance between the edge film of the second belt layer and the first belt layer in the width direction, H1 is the thickness of the edge film, the width direction is consistent with the width direction of the tire cross section, and the thickness direction is perpendicular to the width direction.

2. A method for resolving tire crown blisters according to claim 1, characterized in that, The protrusion includes a main pressing surface and auxiliary pressing surfaces located on both sides of the main pressing surface. The main pressing surface is parallel to the central axis of the roller body, and the auxiliary pressing surfaces are inclined. The distance between the main pressing surface and the central axis of the roller body is greater than the distance between the auxiliary pressing surface and the central axis of the roller body.

3. A method for resolving tire crown blisters according to claim 2, characterized in that, During the compression molding process, the main compression surface contacts the tire tread, the auxiliary compression surface contacts the tire shoulder, and an angle of 15°-75° is formed between the main compression surface and the auxiliary compression surface.

4. A method for resolving tire crown blisters according to claim 2, characterized in that, The protrusion also includes a side surface that is in contact with the auxiliary pressing surface, and the side surface is perpendicular to the central axis of the roller body.

5. A method for resolving air bubbles in tire crowns according to claim 4, characterized in that, The height of the side is less than 1 / 2 of the radius of the protrusion.

6. The method for resolving air bubbles in tire crowns according to claim 1, characterized in that, The tread is composed of multiple layers of rubber sheets. The material of the differential rubber sheets is the same as that of the bottom layer rubber sheet of the tread. The bottom layer rubber sheet of the tread is the rubber sheet adjacent to the belt layer composite.

7. A method for resolving air bubbles in tire crowns according to claim 6, characterized in that, The width of the first belt layer is smaller than the width of the second belt layer.

8. A tire prepared using the method for resolving air bubbles in the tire crown as described in any one of claims 1-7, characterized in that, It includes a tread and a belt layer composite, wherein the belt layer composite adopts a multi-layer structure, and differential films are bonded at the thickness difference positions of the two belt layers adjacent to the tread.

Citation Information

Patent Citations

  • Manufacturing method of pneumatic tire

    CN101454146A

  • Rear compression roller of tread auxiliary machine

    CN214872857U

  • Belt type auxiliary drum equipment for solving air clog between belt layer and tire crown

    CN217891950U