Titanium-aluminum alloy electrode block containing adhesive raw material, preparation method and application thereof

By using partial mixing and titanium foil coating, the problems of aluminum granules sticking together and uneven distribution during electrode block pressing were solved, achieving uniform composition and high yield of TiAl ingots.

CN117253674BActive Publication Date: 2026-11-24XIAN SUPERCRYSYAL SCI TECH DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311124259.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2026-11-24
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

In the traditional process of preparing TiAl alloy electrode blocks, aluminum beads tend to stick to the mold and are unevenly distributed, which leads to cracking and compositional segregation of TiAl ingots, reducing the yield.

Method used

A method of partial mixing and titanium foil coating is adopted. Before pressing the electrode block, titanium foil is covered on the inner wall of the mold and mixed raw materials are laid to reduce the contact between the aluminum coin and the mold. Pressing is carried out in combination with appropriate pressure and time.

Benefits of technology

This effectively prevents aluminum beads from sticking to the mold, improves the uniformity of aluminum distribution, reduces the risk of cracking and component segregation in TiAl ingots, and increases the yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117253674B_ABST
    Figure CN117253674B_ABST
Patent Text Reader

Abstract

This invention discloses a titanium-aluminum alloy electrode block containing viscous raw materials, its preparation method, and its application. The titanium-aluminum alloy electrode block is prepared by the following steps: 1) Divide sponge titanium into three equal parts and aluminum granules into two equal parts. Then, mix one part of sponge titanium and one part of aluminum granules with all intermediate alloys to obtain a mixed raw material; 2) Pour the other part of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then, cut and fold titanium foil into the same shape as the mold cavity and attach it to the inner wall of the mold cavity. Pour the remaining raw material into the titanium foil; 3) Cover the upper mold of the electrode block pressing mold and press it under a set pressure. After pressing for a certain period of time, demold to obtain the target titanium-aluminum alloy electrode block. This invention solves the problems of difficult demolding of traditional titanium-aluminum alloy electrode blocks and uneven Al content distribution caused by aluminum granule agglomeration by using a combination of partial mixing, partial fabrication, and titanium foil coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy preparation technology, specifically relating to a titanium-aluminum alloy electrode block containing viscous raw materials, its preparation method, and its application. Background Technology

[0002] TiAl intermetallic compound alloys possess low density, high elastic modulus, and excellent high-temperature strength, creep resistance, and oxidation resistance. In other words, TiAl alloys combine the plasticity of metals with the high-temperature strength of ceramics, while also exhibiting unique lightweight and high-strength properties. Therefore, they have attracted widespread attention from research institutions worldwide in recent years and are considered one of the most promising new alternative high-temperature structural materials for future aerospace, automotive engine, and generator industries.

[0003] As is well known, the TiAl alloy ingot synthesized from raw materials and intermediate alloys through vacuum arc melting is the foundation for all subsequent processing and forming. It directly affects the microstructure, texture, and distribution of alloying elements in the as-cast alloy, and has a significant impact on hot working processes such as casting, forging, and hot extrusion, as well as powder metallurgy processes. The general preparation process of vacuum arc melting is as follows: raw material selection and preparation → mixing → electrode block pressing → electrode welding → melting → finished ingot processing. The main constituent elements in TiAl alloy are Ti, Al, Nb, Cr, etc., among which the Al element content is between 45 and 48 at.%, which is relatively high. Al element is generally added by adding pure aluminum briquettes or aluminum briquettes combined with aluminum-niobium alloys. Due to the large amount of aluminum briquettes added, and the high viscosity of pure aluminum briquettes, they tend to stick to the mold during electrode block pressing, leading to difficulties in demolding. At the same time, aluminum briquettes are prone to agglomeration during the mixing process, often resulting in uneven distribution of Al element. This easily leads to problems such as cracking and component segregation in the final TiAl ingot, thereby reducing the yield of TiAl ingots.

[0004] In view of this, this invention is hereby proposed. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a titanium-aluminum alloy electrode block containing viscous raw materials, its preparation method and its application. This invention mainly solves the problems of easy agglomeration of traditional aluminum briquettes and easy adhesion to the mold during electrode block pressing by mixing materials and covering the intermediate alloy cloth with titanium foil. This reduces the risk of cracking and component segregation of titanium-aluminum alloy ingots and improves the yield of TiAl ingots.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] On one hand, the present invention provides a method for preparing a titanium-aluminum alloy electrode block containing a viscous raw material, comprising the following steps:

[0008] Step 1: Mixing

[0009] Based on the composition of the target titanium-aluminum alloy, the sponge titanium is first divided into three equal parts and the aluminum granules are divided into two equal parts. Then, one part of sponge titanium and one part of aluminum granules are mixed evenly with all the intermediate alloys that make up the target titanium-aluminum alloy to obtain the mixed raw material.

[0010] Step 2: Titanium foil coating and fabric application

[0011] Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then cut and fold the titanium foil of the set thickness into the same shape as the lower mold cavity of the electrode block pressing mold, and make the folded titanium foil adhere to the inner wall of the lower mold cavity of the electrode block pressing mold. Pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium.

[0012] Step 3: Electrode Block Pressing

[0013] Cover the upper mold of the electrode block pressing mold, press the electrode block under the set pressure, and after the set pressing time is reached, demold to obtain the target titanium-aluminum alloy electrode block.

[0014] Furthermore, the intermediate alloy in the titanium-aluminum alloy of step one is one or more of aluminum-niobium alloy, niobium-titanium alloy, metallic chromium, or aluminum-vanadium alloy.

[0015] Furthermore, in step one, the mixing of raw materials is carried out in a V-shaped mixer, and the mixing time is set to 3 to 10 minutes.

[0016] Furthermore, in step two, the cross-section of the lower mold cavity of the electrode block pressing mold is U-shaped, and the titanium foil is folded into a U-shaped titanium foil, with flanges on both sides of the U-shaped titanium foil.

[0017] Furthermore, the thickness of the titanium foil is 0.1 mm to 0.3 mm.

[0018] Furthermore, in step three, when pressing the electrode block, the pressure is set to 20MPa to 30MPa, and the holding time is 20s to 30s.

[0019] On the other hand, the present invention provides a titanium-aluminum alloy electrode block containing viscous raw materials, wherein the titanium-aluminum alloy electrode block is prepared based on the above-described preparation method.

[0020] Thirdly, the present invention provides an application of a titanium-aluminum alloy electrode block containing viscous raw materials, wherein the titanium-aluminum alloy electrode block is used to prepare titanium-aluminum ingots.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] This invention employs a partial mixing and partial spreading method, which significantly reduces the agglomeration of aluminum granules during mixing and improves the uniformity of aluminum granule distribution in the electrode block. This is beneficial for the uniform distribution of Al elements after ingot smelting and reduces the risk of cracking and compositional segregation in titanium-aluminum alloy ingots. At the same time, when spreading the material in the electrode block pressing mold, the method of wrapping the raw material with titanium foil before pressing reduces the contact area between the sticky aluminum granules and the mold surface, thereby preventing the aluminum granules from sticking to the mold. Therefore, the electrode block can be easily demolded. Attached Figure Description

[0023] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.

[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 This is a flowchart of the method for preparing the titanium-aluminum alloy electrode block of the present invention;

[0026] Figure 2 This is a schematic diagram of the matching structure between the U-shaped titanium foil and the lower mold of the present invention.

[0027] Wherein: 1 is the lower mold of the electrode block pressing mold; 2 is the U-shaped titanium foil. Detailed Implementation

[0028] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of apparatuses consistent with some aspects of the invention as detailed in the appended claims.

[0029] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0030] Please see Figures 1-2 This invention provides a method for preparing a titanium-aluminum alloy electrode block containing a viscous raw material, specifically including the following steps:

[0031] Step 1: Mixing

[0032] Based on the composition of the target titanium-aluminum alloy, the sponge titanium is first divided into three equal parts, and the aluminum briquettes are divided into two equal parts. Then, one part of the sponge titanium and one part of the aluminum briquettes are mixed evenly with all the intermediate alloys that make up the target titanium-aluminum alloy (including but not limited to one or more of aluminum-niobium alloy, niobium-titanium alloy, metallic chromium or aluminum-vanadium alloy) in a V-shaped mixer. The mixing time is generally set to 3 min to 10 min to obtain the mixed raw materials.

[0033] Step 2: Titanium foil coating and fabric application

[0034] Another portion of sponge titanium is poured into the cavity of the lower mold 1 of the electrode block pressing mold and flattened. Then, titanium foil with a thickness of 0.1mm to 0.3mm is cut and folded into the same shape as the cavity of the lower mold 1 of the electrode block pressing mold. For example, in order to obtain an electrode block with a U-shaped cross section, the titanium foil is folded into a U-shaped titanium foil 2, and flanges are provided on both sides of the U-shaped titanium foil 2. The folded titanium foil is then attached to the inner wall of the cavity of the lower mold 1 of the electrode block pressing mold. The remaining portion of aluminum granules is poured into the titanium foil, followed by the mixed raw materials obtained in step one, and finally the remaining portion of sponge titanium is poured in.

[0035] Step 3: Electrode Block Pressing

[0036] Cover the upper mold of the electrode block pressing mold and press the electrode block under a pressure of 20MPa to 30MPa. After pressing for 20s to 30s, demold to obtain the target titanium-aluminum alloy electrode block.

[0037] To further verify the effectiveness of the preparation method of the present invention, the inventors conducted the following specific experiments:

[0038] Example 1 (Pressing of Ti45Al8Nb titanium-aluminum alloy electrode blocks)

[0039] The objective was to prepare a Ti45Al8Nb titanium-aluminum alloy electrode block, with a single electrode block weighing 20 kg. The aluminum content was 4.9 kg, accounting for 24.5%. The die for pressing the electrode block had dimensions of Φ110×400 mm. The specific preparation process is as follows:

[0040] 1) Mixing

[0041] First, divide 9.4 kg of sponge titanium into three equal parts and 4.9 kg of aluminum briquettes into two equal parts; then pour one part of sponge titanium, one part of aluminum briquettes, and all of the aluminum-niobium alloy and niobium-titanium alloy into a V-shaped mixer, set the mixing time to 8 minutes, and obtain the mixed raw materials.

[0042] 2) Titanium foil coating, fabric

[0043] Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then, cut and fold a 0.2mm thick titanium foil into a U-shape of the same size as the lower mold cavity of the electrode block pressing mold, and adhere the folded titanium foil to the inner wall of the lower mold cavity of the electrode block pressing mold (e.g., Figure 2 As shown), pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium.

[0044] 3) Electrode block pressing

[0045] Cover the upper mold of the electrode block pressing mold and press the electrode block. The pressing pressure of the electrode block is 25MPa and the holding time is 20s. After the holding time is up, demolding is performed and the electrode block is successfully demolded.

[0046] The electrode block obtained in Example 1 was used to prepare titanium-aluminum ingots according to the conventional method. No cracking occurred in the final titanium-aluminum ingot. At the same time, the longitudinal Al content of the titanium-aluminum ingot was analyzed. The results are shown in Table 1 below. The Al content was between 29.00 and 29.10, which means that the distribution was uniform and there was no segregation problem.

[0047] Table 1. Vertical Al element distribution of Ti45Al8Nb ingot

[0048]

[0049]

[0050] Example 2 (Pressing of Ti45Al8Nb titanium-aluminum alloy electrode blocks)

[0051] The objective was to prepare a Ti45Al8Nb titanium-aluminum alloy electrode block, weighing 10 kg, with an aluminum content of 2.4 kg (24%). The die for pressing the electrode block had dimensions of Φ110×400 mm. The specific preparation process is as follows:

[0052] 1) Mixing

[0053] First, divide 4.7 kg of sponge titanium into three equal parts and 2.4 kg of aluminum briquettes into two equal parts; then pour one part of sponge titanium, one part of aluminum briquettes, and all of the aluminum-niobium alloy and niobium-titanium alloy into a V-shaped mixer, set the mixing time to 3 minutes, and obtain the mixed raw materials.

[0054] 2) Titanium foil coating, fabric

[0055] Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then, cut and fold a 0.1mm thick titanium foil into a U-shape of the same size as the lower mold cavity of the electrode block pressing mold, and adhere the folded titanium foil to the inner wall of the lower mold cavity of the electrode block pressing mold (e.g., Figure 2As shown), pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium.

[0056] 3) Electrode block pressing

[0057] Cover the upper mold of the electrode block pressing mold and press the electrode block. The pressing pressure of the electrode block is 20MPa and the holding time is 25s. After the holding time is up, demolding is performed and the electrode block is successfully demolded.

[0058] The electrode block obtained in Example 2 was used to prepare titanium-aluminum ingots according to the conventional method. No cracking occurred in the final titanium-aluminum ingot. At the same time, the longitudinal Al content of the titanium-aluminum ingot was analyzed. The results are shown in Table 2 below. The Al content was between 29.30 and 29.40, which means that the distribution was uniform and there was no segregation problem.

[0059] Table 2. Vertical Al element distribution of Ti45Al8Nb ingots

[0060] Sampling location Al(wt.%) Ingot head 29.31 Ingot middle 29.40 Ingot tail 29.39

[0061] Example 3 (Pressing of Ti48Al2Nb2Cr titanium-aluminum alloy electrode blocks)

[0062] The objective was to prepare a Ti48Al2Nb2Cr titanium-aluminum alloy electrode block, weighing 10 kg, with an aluminum content of 3.5 kg (35%). The die for pressing the electrode block had dimensions of Φ110×400 mm. The specific preparation process is as follows:

[0063] 1) Mixing

[0064] First, divide 5.2 kg of sponge titanium into three equal parts and 3.5 kg of aluminum briquettes into two equal parts; then pour one part of sponge titanium, one part of aluminum briquettes, and all the metallic chromium and niobium titanium alloy into a V-shaped mixer, set the mixing time to 5 minutes, and obtain the mixed raw materials.

[0065] 2) Titanium foil coating, fabric

[0066] Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then, cut and fold a 0.2mm thick titanium foil into a U-shape of the same size as the lower mold cavity of the electrode block pressing mold, and adhere the folded titanium foil to the inner wall of the lower mold cavity of the electrode block pressing mold (e.g., Figure 2 As shown), pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium.

[0067] 3) Electrode block pressing

[0068] Cover the upper mold of the electrode block pressing mold and press the electrode block. The pressing pressure of the electrode block is 25MPa and the holding time is 25s. After the holding time is up, demolding is performed and the electrode block is successfully demolded.

[0069] The electrode block obtained in Example 3 was used to prepare titanium-aluminum ingots according to the conventional method. No cracking occurred in the final titanium-aluminum ingot. At the same time, the longitudinal Al content of the titanium-aluminum ingot was analyzed. The results are shown in Table 3 below. The Al content was between 34.45 and 34.50, which means that the distribution was uniform and there was no segregation problem.

[0070] Table 3. Vertical Al element distribution of Ti48Al2Nb2Cr ingots

[0071] Sampling location Al(wt.%) Ingot head 34.49 Ingot middle 34.50 Ingot tail 34.47

[0072] Example 4 (Pressing of Ti48Al7Nb2.5V1Cr titanium-aluminum alloy electrode blocks)

[0073] The objective was to prepare a Ti48Al7Nb2.5V1Cr titanium-aluminum alloy electrode block, with a single electrode block weighing 20 kg. The aluminum content was 6.4 kg, accounting for 32%. The die for pressing the electrode block had dimensions of Φ110×400 mm. The specific preparation process is as follows:

[0074] 1) Mixing

[0075] First, divide 7.7 kg of sponge titanium into three equal parts and 6.4 kg of aluminum briquettes into two equal parts; then pour one part of sponge titanium, one part of aluminum briquettes, and all the metallic chromium, niobium-titanium alloy, aluminum-niobium alloy, and aluminum-vanadium alloy into a V-shaped mixer, and set the mixing time to 10 minutes to obtain mixed raw materials.

[0076] 2) Titanium foil coating, fabric

[0077] Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then, cut and fold a 0.3mm thick titanium foil into a U-shape of the same size as the lower mold cavity of the electrode block pressing mold, and adhere the folded titanium foil to the inner wall of the lower mold cavity of the electrode block pressing mold (e.g., Figure 2 As shown), pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium.

[0078] 3) Electrode block pressing

[0079] Cover the upper mold of the electrode block pressing mold and press the electrode block. The pressing pressure of the electrode block is 28MPa and the holding time is 30s. After the holding time is up, demolding is performed and the electrode block is successfully demolded.

[0080] The electrode block obtained in Example 4 was used to prepare titanium-aluminum ingots according to the conventional method. No cracking occurred in the final titanium-aluminum ingot. At the same time, the longitudinal Al content of the titanium-aluminum ingot was analyzed. The results are shown in Table 4 below. The Al content was between 31.45 and 31.50, which means that the distribution was uniform and there was no segregation problem.

[0081] Table 4. Vertical Al element distribution of Ti48Al7Nb2.5V1Cr ingot

[0082] Sampling location Al(wt.%) Ingot head 31.48 Ingot middle 31.45 Ingot tail 31.49

[0083] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.

[0084] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a titanium-aluminum alloy electrode block containing a viscous raw material, characterized in that, Includes the following steps: Step 1: Mixing Based on the composition of the target titanium-aluminum alloy, the sponge titanium is first divided into three equal parts and the aluminum granules are divided into two equal parts. Then, one part of sponge titanium and one part of aluminum granules are mixed evenly with all the intermediate alloys that make up the target titanium-aluminum alloy to obtain the mixed raw material. Step 2: Titanium foil coating and fabric application Pour another portion of sponge titanium into the lower mold cavity of the electrode block pressing mold and flatten it. Then cut and fold the titanium foil of the set thickness into the same shape as the lower mold cavity of the electrode block pressing mold, and make the folded titanium foil adhere to the inner wall of the lower mold cavity of the electrode block pressing mold. Pour the remaining portion of aluminum granules into the titanium foil, then pour in the mixed raw materials obtained in step one, and finally pour in the remaining portion of sponge titanium. Step 3: Electrode Block Pressing Cover the upper mold of the electrode block pressing mold, press the electrode block under the set pressure, and after the set pressing time is reached, demold to obtain the target titanium-aluminum alloy electrode block.

2. The method for preparing the titanium-aluminum alloy electrode block containing viscous raw materials according to claim 1, characterized in that, The intermediate alloy in the titanium-aluminum alloy of step one is one or more of aluminum-niobium alloy, niobium-titanium alloy, metallic chromium, or aluminum-vanadium alloy.

3. The method for preparing the titanium-aluminum alloy electrode block containing viscous raw materials according to claim 1, characterized in that, In step one, the raw materials are mixed in a V-shaped mixer, and the mixing time is set to 3 to 10 minutes.

4. The method for preparing the titanium-aluminum alloy electrode block containing viscous raw materials according to claim 1, characterized in that, In step two, the cross-section of the lower mold cavity of the electrode block pressing mold is U-shaped, and the titanium foil is folded into a U-shaped titanium foil, with flanges on both sides of the U-shaped titanium foil.

5. The method for preparing the titanium-aluminum alloy electrode block containing viscous raw materials according to claim 1, characterized in that, The thickness of the titanium foil is 0.1 mm to 0.3 mm.

6. The method for preparing the titanium-aluminum alloy electrode block containing viscous raw materials according to claim 1, characterized in that, In step three, when pressing the electrode block, the pressure is set to 20MPa to 30MPa, and the holding time is 20s to 30s.

7. A titanium-aluminum alloy electrode block containing a viscous raw material, characterized in that, The titanium-aluminum alloy electrode block is prepared based on any one of the preparation methods in claims 1 to 6.

8. The application of the titanium-aluminum alloy electrode block containing viscous raw material as described in claim 7, characterized in that, The titanium-aluminum alloy electrode block is used to prepare titanium-aluminum ingots.

Citation Information

Patent Citations

  • Smelting method for high-Nb-TiAl based alloy

    CN103773981A

  • Preparation method of homogeneous titanium-aluminum alloy ingots for casting

    CN110684908A