High-strength high-temperature-resistant phosphate adhesive and preparation method thereof

By introducing magnesia, aluminum-magnesia spinel, and reinforcing fibers into phosphate adhesives, the crystal structure is controlled, solving the problems of easy expansion and insufficient strength of phosphate high-temperature adhesives at ultra-high temperatures, and achieving long-lasting application with high strength and temperature resistance.

CN117264541BActive Publication Date: 2026-11-20AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311393005.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2026-11-20
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

Existing phosphate high-temperature adhesives are prone to expansion and insufficient strength at high temperatures, leading to material failure under ultra-high temperature conditions and limiting their long-term heat resistance applications.

Method used

Magnesia and aluminum-magnesia spinel are used as ultra-high temperature components. Micro-blending modification is achieved through ball milling. The crystal structure is controlled by a mixed matrix of phosphate and chromium oxide. Aluminum nitride fibers and zirconium carbide or silicon carbide whiskers are introduced to form a pre-crosslinked system, which toughens and densifies the adhesive.

Benefits of technology

It significantly improves the high-temperature strength and temperature resistance of phosphate adhesives, enabling long-term application under ultra-high temperature conditions and avoiding cracking problems caused by thermal expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004513043880000111
    Figure BDA0004513043880000111
Patent Text Reader

Abstract

The application relates to a high-strength high-temperature-resistant phosphate binder and a preparation method thereof. The method comprises the following steps: mixing solid phosphate, magnesia, chromium oxide and alumina-magnesia spinel and performing ball milling to obtain a filler; mixing a phosphate solution with the filler and performing stirring to obtain a pre-crosslinking system; adding whiskers and aluminum nitride fibers into the pre-crosslinking system and uniformly dispersing, then adding magnesium oxide powder and uniformly dispersing, and then performing solidification to prepare the high-strength high-temperature-resistant phosphate binder; the whiskers are zirconium carbide whiskers and / or silicon carbide whiskers. The application prepares a high-performance high-temperature-resistant binder which is a multi-component compound with phosphate as a main component, has the characteristics of good high-temperature resistance and high strength, and can realize the persistent application of the phosphate binder under superhigh-temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of phosphate adhesive technology, and particularly relates to a high-strength, high-temperature resistant phosphate adhesive and its preparation method. Background Technology

[0002] Phosphate adhesives are characterized by high temperature resistance, low curing temperature, and high structural strength. They can be used for bonding and structural reinforcement of various organic and inorganic functional materials, and are especially widely used in the aerospace and nuclear industries.

[0003] However, current high-temperature phosphate adhesives mainly include aluminum phosphate, zirconium phosphate, aluminum dihydrogen phosphate, and phosphate-based composite adhesives containing other functional components. These high-temperature adhesives are prone to expansion when heated, leading to insufficient strength and cracking of the high-temperature adhesive material. Especially in the ultra-high temperature range, above 1200℃ or even 1500℃, due to changes in the crystal structure of the phosphate adhesive, the material experiences strength failure during long-term high-temperature application. These problems severely limit the long-term temperature resistance of phosphate high-temperature adhesives, posing significant application risks to various equipment. Therefore, it is essential to design the composition and structure of phosphate high-temperature adhesives to mitigate the insufficient temperature resistance caused by crystal structure transformation.

[0004] In summary, it is essential to provide a high-strength, high-temperature resistant phosphate adhesive and its preparation method. Summary of the Invention

[0005] To address one or more technical problems existing in the prior art, this invention provides a high-strength, high-temperature resistant phosphate adhesive and its preparation method. The invention prepares a high-performance, high-temperature resistant adhesive with phosphate as the main component, consisting of multiple components. It exhibits excellent high-temperature resistance and high strength, enabling the phosphate adhesive to be used sustainably under ultra-high temperature conditions.

[0006] The present invention provides a method for preparing a high-strength, high-temperature resistant phosphate adhesive in a first aspect, the method comprising the following steps:

[0007] (1) Solid phosphate, magnesium sand, chromium oxide and aluminum magnesium spinel are mixed and ball-milled to obtain filler;

[0008] (2) The phosphate solution is mixed with the filler and stirred to obtain a pre-crosslinked system;

[0009] (3) Add whiskers and aluminum nitride fibers to the pre-crosslinked system and disperse them evenly, then add magnesium oxide powder and disperse it evenly to obtain a high-strength, high-temperature resistant phosphate adhesive; the whiskers are zirconium carbide whiskers and / or silicon carbide whiskers.

[0010] Preferably, the mass ratio of the solid phosphate, the magnesia, the chromium oxide and the aluminum magnesium spinel is (6-13):(2-7):(1-3):(1-5).

[0011] Preferably, the particle size of the magnesia is 10-200 μm, and / or the particle size of the aluminum-magnesium spinel is 20-500 μm; and / or the ball milling time is 6-12 h.

[0012] Preferably, the solid content of the phosphate solution is 20-60 wt%; and / or the mass ratio of the phosphate solution to the filler is (2-9):1.

[0013] Preferably, the stirring is performed at room temperature for 3 to 6 hours.

[0014] Preferably, the aspect ratio of the whiskers is (5-100):1; and / or the length of the aluminum nitride fibers is 3-8 μm.

[0015] Preferably, the mass ratio of the whiskers to the pre-crosslinked system is 1:(20-30); the mass ratio of the aluminum nitride fiber to the pre-crosslinked system is 1:(30-60); and / or the mass ratio of the magnesium oxide powder to the pre-crosslinked system is 1:(15-30).

[0016] Preferably, the curing conditions for the high-strength, high-temperature resistant phosphate adhesive are: first, curing at 80–100℃ for 4–8 hours, and then curing at 120–180℃ for 10–15 hours.

[0017] Preferably, the solid phosphate is solid aluminum phosphate and / or solid zirconium phosphate; the phosphate solution is one or more of aluminum dihydrogen phosphate solution, aluminum phosphate solution, and zirconium phosphate solution.

[0018] In a second aspect, the present invention provides a high-strength, high-temperature resistant phosphate adhesive prepared by the preparation method described in the first aspect of the present invention.

[0019] Compared with the prior art, the present invention has at least the following beneficial effects:

[0020] The high-strength, high-temperature resistant phosphate adhesive prepared in this invention uses magnesia and aluminum-magnesia spinel as ultra-high temperature components. The mixed matrix of phosphate and chromium oxide achieves microscale blending modification of magnesia and / or aluminum-magnesia spinel through ball milling, thereby controlling the high-temperature crystal form of phosphate and avoiding phosphate failure at high temperatures and even ultra-high temperatures (above 1500℃). At the same time, high-temperature resistant reinforcing fibers (aluminum nitride fibers) and nanofibers (zirconia whiskers and / or silicon carbide whiskers) are introduced to toughen the high-temperature adhesive system (pre-crosslinked system). The reinforcement is densified with liquid phosphate adhesive (phosphate solution), which allows the reinforcement to bond more tightly with the main components, significantly improving the high-temperature strength of the phosphate adhesive and achieving the goal of durable application at ultra-high temperatures. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0022] The present invention provides a method for preparing a high-strength, high-temperature resistant phosphate adhesive in a first aspect, the method comprising the following steps:

[0023] (1) Solid phosphate, magnesium sand, chromium oxide (chromium trioxide) and aluminum magnesium spinel are mixed and ball-milled to obtain filler (also known as high temperature filler);

[0024] (2) The phosphate solution is mixed with the filler and stirred to obtain a pre-crosslinked system; the present invention does not specify the stirring speed, for example, it can be 200 to 800 r / min;

[0025] (3) Add whiskers and aluminum nitride fibers to the pre-crosslinked system and disperse them evenly, then add magnesium oxide powder and disperse it evenly to obtain a high-strength, high-temperature resistant phosphate adhesive; the whiskers are zirconium carbide whiskers and / or silicon carbide whiskers; in this invention, the dispersion can be uniform by stirring, for example, the stirring speed is not specifically limited, for example, it can be 200-800 r / min; in this invention, the source of each raw material is not specifically limited, and products that can be purchased directly from the market or synthesized by existing methods can be used; the high-strength, high-temperature resistant phosphate adhesive obtained by this invention can achieve the long-term application of phosphate adhesive under ultra-high temperature conditions, so it is also called high-strength, ultra-high temperature resistant phosphate adhesive (abbreviated as phosphate adhesive); in this invention, the ultra-high temperature conditions refer to high temperature conditions above 1500℃.

[0026] This invention first designs the ultra-high temperature resistant components, using magnesia and aluminum-magnesia spinel as the ultra-high temperature components. Magnesia, in particular, is an ideal component for ultra-high temperature phosphate adhesives, enhancing their high-temperature dimensionality. Simultaneously, a mixed matrix of phosphate and chromium oxide is used to ball-mill and microscale modify magnesia and / or aluminum-magnesia spinel, controlling the high-temperature crystal structure of the phosphate and thus preventing high-temperature failure of the high-temperature adhesive (phosphate adhesive). Secondly, this invention mixes and stirs the phosphate solution (liquid phosphate) with the filler to form a pre-crosslinked system. In this invention, the filler contains solid phosphate, which increases the phosphate content of the high-temperature resistant crystal structure, improves the dispersibility between the phosphate solution and other filler components, and promotes pre-crosslinking, thereby improving the performance of the phosphate adhesive and optimizing its composition. Finally, this invention adds whiskers to the pre-crosslinked system. (e.g., zirconium carbide whiskers) and aluminum nitride fibers are stirred and dispersed evenly. Then, magnesium oxide powder is added and stirred and dispersed evenly to obtain the high-strength, high-temperature resistant phosphate adhesive. This invention first forms a pre-crosslinked system to build a basic network structure in the adhesive, and then adds whiskers (e.g., zirconium carbide whiskers), aluminum nitride fibers, and magnesium oxide powder. This makes it easier to achieve uniform dispersion of these compound components, helps to ensure that each component can be fully distributed throughout the phosphate adhesive, and can better ensure the interaction between the components. It maximizes the toughening and high-temperature stability of whiskers (e.g., zirconium carbide whiskers), aluminum nitride fibers, and magnesium oxide powder, thereby significantly enhancing the overall performance of the phosphate adhesive. This invention prepares a high-performance, high-temperature resistant adhesive with phosphate as the main component, which is resistant to high temperatures without expansion and has high strength, enabling the phosphate adhesive to be used for long-term applications under ultra-high temperature conditions.

[0027] The high-strength, high-temperature resistant phosphate adhesive prepared in this invention uses magnesia and aluminum-magnesia spinel as ultra-high temperature components. A mixed matrix of phosphate and chromium oxide is used to ball-mill the magnesia and / or aluminum-magnesia spinel to achieve microscale blending modification, thereby controlling the high-temperature crystal structure of the phosphate and preventing its failure at high temperatures, even above 1500°C. Simultaneously, high-temperature resistant reinforcing fibers (aluminum nitride fibers) and nanofibers (zirconia whiskers and / or silicon carbide whiskers) are introduced to toughen the high-temperature adhesive system (pre-crosslinked system). The liquid phosphate adhesive (phosphate solution) densifies the reinforcement, allowing it to bond more tightly to the main components, significantly improving the high-temperature strength of the phosphate adhesive and achieving durable application at ultra-high temperatures. Furthermore, this invention adds magnesium oxide powder to the pre-crosslinked system, which improves the high-temperature stability of the phosphate adhesive and better controls its thermal expansion properties, effectively preventing breakage or damage caused by thermal expansion mismatch.

[0028] According to some preferred embodiments, the mass ratio of the solid phosphate, the magnesia, the chromium oxide, and the aluminum-magnesium spinel is (6-13):(2-7):(1-3):(1-5). This invention obtained this preferred ratio through a large number of creative experiments. This invention found that this ratio can achieve effective control of the crystal form and realize the high-temperature resistance modification design of the phosphate adhesive system, thereby ensuring that a phosphate adhesive with ultra-high temperature resistance and high strength is obtained. In this invention, if the proportions of each component are not within this preferred range, it may lead to failure of crystal form control, and an inappropriate mass ratio may also lead to uneven material composition and unstable crystal structure, thereby reducing the overall performance of the phosphate adhesive under high temperature conditions.

[0029] According to some preferred embodiments, the particle size (average particle size) of the magnesia is 10–200 μm (e.g., 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, or 200 μm), and / or the particle size (average particle size) of the aluminum-magnesium spinel is 20–500 μm (e.g., 20, 50, 80, 100, 150, 200, 250, 300, 350, 400, 450 μm). (or 500 μm); In this invention, preferably, the particle size of the magnesia is 10-200 μm, and the particle size of the aluminum magnesium spinel is 20-500 μm. If the particle size of these two components is too small, they are prone to agglomeration, which will lead to poor high-temperature stability of the prepared adhesive. If the particle size of these two components is too large, it is difficult to form a modified eutectic system with phosphate and chromium oxide during the ball milling process, which is also not conducive to improving the high-temperature stability of the adhesive; and / or the ball milling time is 6-12 h (e.g., 6, 7, 8, 9, 10, 11 or 12 h).

[0030] According to some preferred embodiments, the solid content of the phosphate solution is 20-60 wt% (e.g., 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, or 60 wt%), that is, the phosphate solution contains a phosphate mass fraction of 20-60 wt%; and / or the mass ratio of the phosphate solution to the filler is (2-9):1 (e.g., 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, or 9:1); in this invention, the preferred mass ratio of the phosphate solution to the filler is (2-9):1. 9):1, which is beneficial to ensure that a phosphate adhesive with high strength and resistance to ultra-high temperature is obtained. Within this preferred ratio range, it can be adjusted according to different viscosity requirements of the high-strength, high-temperature resistant phosphate adhesive system to obtain high-temperature resistant adhesives with different viscosities, so as to better adapt to actual application conditions. In this invention, it is preferred that the solid content of the phosphate solution is controlled between 20wt% and 60wt%. If the solid content in the phosphate solution is too high, it will result in less high-temperature resistant component in the phosphate adhesive of this invention, and the temperature resistance of the adhesive will be difficult to improve effectively. If there is too much high-temperature resistant component, the improvement of the high-temperature strength of the material will be limited.

[0031] According to some preferred embodiments, the stirring is performed at room temperature for 3 to 6 hours (e.g., 3, 4, 5 or 6 hours); in this invention, the room temperature can be, for example, 20 to 30°C.

[0032] According to some preferred embodiments, the aspect ratio of the whiskers is (5-100):1; in some specific embodiments of the present invention, the whiskers are, for example, zirconium carbide whiskers, and the particle size of the zirconium carbide whiskers is, for example, 10-100 nm; and / or the length (average length) of the aluminum nitride fibers is 3-8 μm; in the present invention, the diameter of the aluminum nitride fibers can be, for example, 100-1000 nm; in the present invention, preferably, the whiskers are zirconium carbide whiskers, the aspect ratio of the zirconium carbide whiskers is (5-100):1, and the length of the aluminum nitride fibers is 3-8 μm. If the aspect ratio of the zirconium carbide whiskers is too small and the length of the aluminum nitride fibers is too small, it cannot play an effective toughening role; if the aspect ratio of the zirconium carbide whiskers is too large and the length of the aluminum nitride fibers is too large, adhesion and agglomeration are likely to occur, which is also not conducive to improving the overall bonding performance of the material.

[0033] The present invention does not have any special requirements on the particle size of chromium oxide and magnesium oxide powders. Micron-sized or nano-sized powders can be selected. In some specific embodiments, the particle size of the magnesium oxide powder is, for example, 0.1 to 1 μm, and the particle size of the chromium oxide (chromium oxide powder) is, for example, 15 to 75 μm.

[0034] According to some preferred embodiments, the mass ratio of the whiskers to the pre-crosslinked system is 1:(20-30); the mass ratio of the aluminum nitride fiber to the pre-crosslinked system is 1:(30-60); and / or the mass ratio of the magnesium oxide powder to the pre-crosslinked system is 1:(15-30). In this invention, in order to ensure effective dispersion of the toughening components and magnesium oxide powder components and to effectively ensure the high temperature resistance and high strength properties of the phosphate binder, this invention has obtained the most preferred amounts of whiskers, aluminum nitride fiber and magnesium oxide powder through a large number of creative experiments. In this invention, preferably, the mass ratio of the whiskers to the pre-crosslinked system is 1:(20-30), the mass ratio of the aluminum nitride fiber to the pre-crosslinked system is 1:(30-60), and the mass ratio of the magnesium oxide powder to the pre-crosslinked system is 1:(15-30).

[0035] According to some preferred embodiments, the curing conditions of the high-strength, high-temperature resistant phosphate adhesive are as follows: first, curing at 80–100°C (e.g., 80°C, 90°C, or 100°C) for 4–8 hours (e.g., 4, 5, 6, 7, or 8 hours), and then curing at 120–180°C (e.g., 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, or 180°C) for 10–15 hours (e.g., 10, 11, 12, 13, 14, or 15 hours). In this invention, when the high-strength, high-temperature resistant phosphate adhesive is used as an adhesive, it is preferable to perform this gradient temperature curing. This can effectively prevent bubbling and other issues from occurring during application of the phosphate adhesive, thereby helping to ensure the overall performance of the phosphate adhesive.

[0036] According to some preferred embodiments, the solid phosphate is solid aluminum phosphate and / or solid zirconium phosphate; the phosphate solution is one or more of aluminum dihydrogen phosphate solution, aluminum phosphate solution, and zirconium phosphate solution; in this invention, the phosphate is aluminum-based phosphate and / or zirconium-based phosphate; in this invention, the phosphate solution refers to an aqueous phosphate solution.

[0037] In a second aspect, the present invention provides a high-strength, high-temperature resistant phosphate adhesive prepared by the preparation method described in the first aspect of the present invention.

[0038] The present invention will be further described below by way of examples, but the scope of protection of the present invention is not limited to these embodiments.

[0039] It should be noted that in this invention, "parts" refers to "parts by weight". In specific embodiments and comparative examples, the unit of weight parts can be uniformly expressed as "g" or "kg".

[0040] Example 1

[0041] ① Mix 60 parts of solid aluminum phosphate, 20 parts of magnesia (particle size 200μm), 10 parts of chromium oxide and 10 parts of aluminum magnesium spinel (particle size 20μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0042] ② Mix 200 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0043] ③ Add 15 parts of zirconium carbide whiskers (aspect ratio of 100) and 10 parts of aluminum nitride fibers with a length of 8 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 10 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, high-temperature resistant phosphate adhesive.

[0044] Example 2

[0045] ① Mix 60 parts of solid aluminum phosphate, 20 parts of magnesia (particle size 20μm), 10 parts of chromium oxide and 10 parts of aluminum magnesium spinel (particle size 30μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0046] ② Mix 200 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0047] ③ Add 10 parts of zirconium carbide whiskers (aspect ratio of 100) and 5 parts of aluminum nitride fibers with a length of 3 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 10 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, high-temperature resistant phosphate adhesive.

[0048] Example 3

[0049] ① Mix 60 parts of solid aluminum phosphate, 20 parts of magnesia (particle size 20μm), 10 parts of chromium oxide and 10 parts of aluminum magnesium spinel (particle size 30μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0050] ② Mix 200 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0051] ③ Add 12 parts of zirconium carbide whiskers (aspect ratio of 20) and 7 parts of aluminum nitride fibers with a length of 4 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 20 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, high-temperature resistant phosphate adhesive.

[0052] Example 4

[0053] ① Mix 13 parts of solid aluminum phosphate, 7 parts of magnesia (particle size 10 μm), 3 parts of chromium oxide and 2 parts of aluminum magnesium spinel (particle size 500 μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0054] ② Mix 225 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 h to obtain a pre-crosslinked system.

[0055] ③ Add 2 parts of zirconium carbide whiskers (aspect ratio of 20) and 2 parts of aluminum nitride fibers with a length of 4 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 10 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, high-temperature resistant phosphate adhesive.

[0056] Example 5

[0057] ① Mix 8 parts solid zirconium phosphate, 3 parts magnesia (particle size 20 μm), 2 parts chromium oxide and 5 parts aluminum magnesium spinel (particle size 50 μm) and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0058] ② Mix 90 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0059] ③ Add 4 parts of zirconium carbide whiskers (aspect ratio of 20) and 2 parts of aluminum nitride fibers with a length of 3 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 5 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, high-temperature resistant phosphate adhesive.

[0060] Example 6

[0061] ① Mix 13 parts of solid aluminum phosphate, 8 parts of magnesia (particle size 200μm), 4 parts of chromium oxide and 6 parts of aluminum magnesium spinel (particle size 20μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0062] ② Mix 279 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 h to obtain a pre-crosslinked system.

[0063] ③ Add 15 parts of zirconium carbide whiskers (aspect ratio of 100) and 10 parts of aluminum nitride fibers with a length of 8 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 10 parts of magnesium oxide powder, stir and disperse evenly to obtain a high-strength, ultra-high temperature resistant phosphate adhesive.

[0064] Comparative Example 1

[0065] 90 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% were mixed with 4 parts of zirconium carbide whiskers (aspect ratio of 20) and 2 parts of aluminum nitride fibers with a length of 3 μm. The mixture was stirred and dispersed evenly. Then, 5 parts of magnesium oxide powder were added and stirred and dispersed evenly to obtain a phosphate adhesive.

[0066] Comparative Example 2

[0067] ① Mix 8 parts of solid zirconium phosphate and 5 parts of aluminum magnesium spinel (particle size 50 μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0068] ② Mix 90 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0069] ③ Add 4 parts of zirconium carbide whiskers (aspect ratio of 20) and 2 parts of aluminum nitride fibers with a length of 3 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 5 parts of magnesium oxide powder, stir and disperse evenly to obtain phosphate adhesive.

[0070] Comparative Example 3

[0071] ① Mix 60 parts of solid aluminum phosphate, 20 parts of magnesia (particle size 200μm), 10 parts of chromium oxide and 10 parts of aluminum magnesium spinel (particle size 20μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0072] ② Mix 200 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir for 20 min to disperse evenly. Then add 15 parts of zirconium carbide whiskers (aspect ratio of 100) and 10 parts of aluminum nitride fibers with a length of 8 μm, stir to disperse evenly, and then add 10 parts of magnesium oxide powder, stir to disperse evenly to obtain phosphate adhesive.

[0073] Comparative Example 4

[0074] ① Mix 20 parts of magnesia (particle size 200μm), 10 parts of chromium oxide and 10 parts of aluminum magnesium spinel (particle size 20μm), and then ball mill them in a ball mill jar for 8 hours to obtain the filler.

[0075] ② Mix 200 parts of aluminum dihydrogen phosphate solution with a solid content of 40 wt% with the filler obtained in step ① and stir at room temperature (25℃) for 5 hours to obtain a pre-crosslinked system.

[0076] ③ Add 15 parts of zirconium carbide whiskers (aspect ratio of 100) and 10 parts of aluminum nitride fibers with a length of 8 μm to the pre-crosslinked system obtained in step ②, stir and disperse evenly, then add 10 parts of magnesium oxide powder, stir and disperse evenly to obtain phosphate adhesive.

[0077] The phosphate adhesives prepared in each embodiment and comparative example of this invention were first cured at 90°C for 6 hours, and then cured at 150°C for 12 hours. The results of the compressive strength (compressive strength at compression failure) at 1500°C and 1800°C are shown in Table 1. In Table 1, the compressive strength at compression failure is recorded as the failure strength of the phosphate adhesive. In this invention, the compressive strength at compression failure is used to represent the failure strength of the phosphate adhesive. The greater the compressive strength at high temperature, the higher the failure strength of the phosphate adhesive under high temperature conditions, the better the temperature resistance, and the more durable the application under ultra-high temperature (above 1500°C) conditions.

[0078] Table 1: Breaking strength results of phosphate adhesives prepared in each embodiment and comparative example

[0079]

[0080] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a high-strength, high-temperature resistant phosphate adhesive, characterized in that, The method includes the following steps: (1) Solid phosphate, magnesia, chromium oxide and aluminum-magnesia spinel are mixed and ball-milled to obtain filler; the mass ratio of the solid phosphate, the magnesia, the chromium oxide and the aluminum-magnesia spinel is (6~13):(2~7):(1~3):(1~5); the particle size of the magnesia is 10~200μm and the particle size of the aluminum-magnesia spinel is 20~500μm; (2) The phosphate solution is mixed with the filler and stirred to obtain a pre-crosslinked system; the solid content of the phosphate solution is 20~60wt%; the mass ratio of the phosphate solution to the filler is (2~9):1; the stirring is carried out at room temperature for 3~6h; (3) Add whiskers and aluminum nitride fibers to the pre-crosslinked system and disperse them evenly, then add magnesium oxide powder and disperse it evenly to obtain a high-strength, high-temperature resistant phosphate adhesive; the whiskers are zirconium carbide whiskers and / or silicon carbide whiskers; the aspect ratio of the whiskers is (5~100):1; the length of the aluminum nitride fibers is 3~8μm; the mass ratio of the whiskers to the pre-crosslinked system is 1:(20~30); the mass ratio of the aluminum nitride fibers to the pre-crosslinked system is 1:(30~60); the mass ratio of the magnesium oxide powder to the pre-crosslinked system is 1:(15~30).

2. The preparation method according to claim 1, characterized in that: The ball milling time is 6-12 hours.

3. The preparation method according to claim 1, characterized in that: The curing conditions for the high-strength, high-temperature resistant phosphate adhesive are as follows: first, cure at 80~100℃ for 4~8 hours, and then cure at 120~180℃ for 10~15 hours.

4. The preparation method according to claim 1, characterized in that: The solid phosphate is solid aluminum phosphate and / or solid zirconium phosphate; The phosphate solution is one or more of aluminum dihydrogen phosphate solution, aluminum phosphate solution, and zirconium phosphate solution.

5. A high-strength, high-temperature resistant phosphate adhesive prepared by any one of claims 1 to 4.

Citation Information

Patent Citations

  • Phosphates adhesive and preparation method thereof

    CN101358111A

  • High temperature resisting magnesium phosphate adhesive with high strength and preparation method thereof

    CN103305134A