A method for producing ultra-high purity pig iron for casting by using blast furnace produced ordinary pig iron
By combining the KR mechanical stirring method and the strong oxidation method, using ordinary pig iron produced in blast furnaces as raw material, and employing high oxygen flow oxygen blowing technology, the problems of high production cost and difficulty in composition control of ultra-high purity pig iron in existing technologies have been solved, realizing efficient and low-cost production of ultra-high purity pig iron.
Patent Information
- Application Number
- CN202210667909.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-06-14
AI Technical Summary
Existing technologies struggle to effectively remove impurity elements when producing ultra-high purity pig iron for casting, resulting in high production costs and difficulties in controlling composition.
Using ordinary pig iron produced in a blast furnace as raw material, it is combined with a single CaO desulfurization powder through KR mechanical stirring. Then, oxygen is blown in from above the molten iron surface in an oxidation converter at a high oxygen flow rate to remove impurity elements through strong oxidation. The slag alkalinity and temperature are controlled to meet the composition requirements of ultra-high purity pig iron.
It has achieved efficient production of ultra-high purity pig iron, reduced production costs, decreased refractory material consumption and processing time, improved oxidation removal capabilities, and can remove harmful and trace elements to extremely low levels, meeting the requirements of high-end casting fields.
Smart Images

Figure CN117265201B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to ultra-high purity pig iron production technology, specifically a method for producing ultra-high purity pig iron for casting using ordinary pig iron produced in a blast furnace. The method involves adding molten ordinary pig iron from the blast furnace as raw material to a ladle, desulfurizing it using a single CaO desulfurization powder via KR mechanical stirring, and then adding the molten iron to an oxidation converter. An oxygen flow rate of 20,000–30,000 Nm³ is used. 3 An oxygen lance operating at / h blows oxygen from above the molten iron surface into the molten iron to strongly oxidize and remove impurities. The elemental wt% content of the ultra-high purity pig iron is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.010, Mn ≤ 0.040, P ≤ 0.012, S ≤ 0.015, Cr ≤ 0.012, V ≤ 0.008, Mo ≤ 0.006, Sn ≤ 0.0010, Sb ≤ 0.0005, Pb ≤ 0.0003, Bi ≤ 0.00005, Te ≤ 0.0003, As ≤ 0.0015, B ≤ 0.0005, Al ≤ 0.010. Background Technology
[0002] Ultra-high purity pig iron for casting is an essential raw material for the production of high-end ductile iron castings. It is primarily used in low-temperature ferritic ductile iron, thick-section and ultra-thick-section ductile iron, silicon solution strengthened ferritic ductile iron, high-strength and high-ductility ductile iron, isothermal hardened ductile iron (ADI), vermicular graphite cast iron, and other high-end cast iron parts. Ultra-high purity pig iron for casting is widely used in major national projects, including nuclear power, wind power, high-speed rail, automobiles, military industry, marine engineering, and aerospace, providing high-quality raw materials for high-performance, high-quality cast iron parts.
[0003] Currently, the production of ultra-high purity pig iron for casting involves a "three-refinement method" (refining raw materials, refining, and fine treatment) to produce high-purity pig iron, followed by a weak oxidation process to control the composition of the ultra-high purity pig iron, thus completing the production of ultra-high purity pig iron for casting. The weak oxidation method involves blowing oxygen into the molten iron in a ladle (oxygen flow rate of 2000-3000 Nm³ / h). 3 / h, N represents standard conditions: 0 degrees Celsius and 1 standard atmosphere) and a method of stirring the molten iron by inserting a spray gun into the molten iron, wherein the spray gun uses nitrogen as a carrier to spray lime powder into the molten iron.
[0004] The elemental wt% content of ordinary pig iron produced by blast furnace is as follows: C ≥ 4.5, Si ≤ 0.80, Ti ≤ 0.031, Mn ≤ 0.11, P ≤ 0.12, S ≤ 0.052, Cr ≤ 0.028, V ≤ 0.025, Mo ≤ 0.004, Sn ≤ 0.0003, Sb ≤ 0.0008, Pb ≤ 0.0023, Bi ≤ 0.0001, Te ≤ 0.0004, As ≤ 0.0005, B ≤ 0.002, Al ≤ 0.02. This invention uses molten pig iron produced by blast furnace as raw material, and performs stepwise KR desulfurization and oxidation to remove harmful and trace elements, achieving the required composition for ultra-high purity pig iron, thus obtaining ultra-high purity pig iron. Summary of the Invention
[0005] This invention addresses the deficiencies or shortcomings of existing technologies by providing a method for producing ultra-high purity pig iron for casting using ordinary pig iron produced in a blast furnace. The method involves adding molten ordinary pig iron from the blast furnace as raw material to a ladle, desulfurizing it using a single CaO desulfurization powder via KR mechanical stirring, and then adding the molten iron to an oxidation converter. An oxygen flow rate of 20,000–30,000 Nm³ is used. 3 An oxygen lance operating at / h blows oxygen from above the molten iron surface into the molten iron to strongly oxidize and remove impurities. The elemental wt% content of the ultra-high purity pig iron is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.010, Mn ≤ 0.040, P ≤ 0.012, S ≤ 0.015, Cr ≤ 0.012, V ≤ 0.008, Mo ≤ 0.006, Sn ≤ 0.0010, Sb ≤ 0.0005, Pb ≤ 0.0003, Bi ≤ 0.00005, Te ≤ 0.0003, As ≤ 0.0015, B ≤ 0.0005, Al ≤ 0.010.
[0006] The technical solution of the present invention is as follows:
[0007] A method for producing ultra-high purity pig iron for casting from ordinary pig iron produced in a blast furnace is characterized by the following steps: molten ordinary pig iron produced in the blast furnace is added to a ladle as raw material; after desulfurization using a single CaO desulfurization powder via KR mechanical stirring, the molten iron is added to an oxidation converter, and oxygen is introduced at a flow rate of 20,000–30,000 Nm³. 3 An oxygen lance operating at / h blows oxygen from above the molten iron into the surface layer of the molten iron to remove impurities through strong oxidation.
[0008] The elemental wt% content of ultra-high purity pig iron for casting is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.010, Mn ≤ 0.040, P ≤ 0.012, S ≤ 0.015, Cr ≤ 0.012, V ≤ 0.008, Mo ≤ 0.006, Sn ≤ 0.0010, Sb ≤ 0.0005, Pb ≤ 0.0003, Bi ≤ 0.00005, Te ≤ 0.0003, As ≤ 0.0015, B ≤ 0.0005, Al ≤ 0.010.
[0009] The elemental wt% content of ultra-high purity pig iron for casting is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.008, Mn ≤ 0.030, P ≤ 0.010, S ≤ 0.012, Cr ≤ 0.010, V ≤ 0.005, Mo ≤ 0.005, Sn ≤ 0.0005, Sb ≤ 0.0004, Pb ≤ 0.0002, Bi ≤ 0.00003, Te ≤ 0.0001, As ≤ 0.0012, B ≤ 0.0003, Al ≤ 0.010.
[0010] The elemental wt% content of ultra-high purity pig iron for casting is as follows: C≥3.30, Si≤0.50, Ti≤0.005, Mn≤0.020, P≤0.008, S≤0.010, Cr≤0.008, V≤0.003, Mo≤0.003, Sn≤0.0003, Sb≤0.0003, Pb≤0.0001, Bi≤0.00001, Te≤0.00005, As≤0.0008, B≤0.0001, Al≤0.005.
[0011] The elemental wt% content of molten iron produced by blast furnace is as follows: C ≥ 4.5, Si ≤ 0.80, Ti ≤ 0.031, Mn ≤ 0.11, P ≤ 0.12, S ≤ 0.052, Cr ≤ 0.028, V ≤ 0.025, Mo ≤ 0.004, Sn ≤ 0.0003, Sb ≤ 0.0008, Pb ≤ 0.0023, Bi ≤ 0.0001, Te ≤ 0.0004, As ≤ 0.0005, B ≤ 0.002, Al ≤ 0.02.
[0012] The top inlet of the molten iron ladle is connected to a hopper via a chute. The hopper has a CaO powder outlet. A rotary agitator is installed on the top of the molten iron ladle. The cross-shaped stirring head of the rotary agitator extends into the surface of the molten iron and rotates under the drive of a motor. CaO powder is added while stirring to achieve the following desulfurization reaction:
[0013] CaO + FeS = CaS + FeO
[0014] 2FeO + Si = 2Fe + SiO2
[0015] Through the above reactions, the S content in the molten iron is reduced to ≤0.005.
[0016] The molten iron temperature in the oxidation converter is ≤1380℃ in order to control carbon loss in the molten iron during the strong oxidation process. Lime, iron ore, and dolomite are added to the furnace during the strong oxidation oxygen blowing smelting process to control slag basicity and molten iron temperature. Iron ore and dolomite act as cooling agents, and scrap steel is not used as a cooling agent.
[0017] In the strong oxidation oxygen blowing smelting process, the slag basicity control adopts the principle of low at the beginning and high at the end. In the early stage of blowing, a low basicity control of R=1.5~1.8 is adopted to facilitate the oxidation and removal of manganese. In the middle and late stages of blowing, a high basicity control of R=2.5~3.5 is adopted to facilitate the oxidation and removal of phosphorus. Sb and Pb in the molten iron are evaporated and removed at the smelting temperature. Ti, Mn, P, Cr, V, B and Al in the molten iron are all oxidized and removed during blowing. When it is detected that all elements meet the target requirements for ultra-high purity pig iron for casting, the strong oxidation endpoint of the converter is reached. Then, the temperature of the molten iron is adjusted to 1410~1450℃ for a short time to compensate for the temperature drop during the tapping process. The molten iron is tapped from the converter into the ladle and then cast into ultra-high purity pig iron blocks using a casting machine.
[0018] During the process of tapping molten iron from the converter into the ladle, a carburizing agent or ferrosilicon is added along with the iron flow to meet the preset limits on the C or Si content of the molten iron.
[0019] During the process of tapping molten iron from the converter into the ladle, slag is blocked during tapping, and the slag remains in the converter and is poured into the slag pot from the large furnace opening.
[0020] The technical effects of this invention are as follows: This invention provides a method for producing ultra-high purity pig iron for casting using ordinary pig iron produced in a blast furnace. The method uses molten pig iron produced in a blast furnace as raw material and performs KR desulfurization (KR, Kambara Reactor, also known as KR mechanical stirring method) and oxidation to remove harmful and trace elements in steps to achieve the composition requirements of ultra-high purity pig iron.
[0021] This invention has the following characteristics: 1. The method of this invention uses ordinary pig iron produced in a blast furnace as raw material and adopts a strong oxidation production process to produce ultra-high purity pig iron. This differs from the original weak oxidation method for producing ultra-high purity pig iron using high-purity pig iron. 2. The strong oxidation method for producing ultra-high purity pig iron uses ordinary pig iron as raw material, significantly reducing the production cost of pig iron. 3. Comparison between the strong oxidation method and the weak oxidation method for producing ultra-high purity pig iron: The oxygen flow rate of the oxygen lance in the strong oxidation method is 8 to 10 times that of the weak oxidation method. The oxygen flow has a greater stirring force on the molten pool, eliminating the need for a stirring lance and saving on refractory material consumption for the stirring lance; the oxygen blowing time is shorter, reducing process temperature drop and saving production costs; the processing time is shorter, reducing refractory material consumption in the reaction vessel and saving production costs; and the strong oxidation capacity can remove harmful and trace elements to even lower levels. Attached Figure Description
[0022] Figure 1 This is a schematic diagram illustrating the pretreatment and desulfurization deployment of ordinary pig iron produced in the blast furnace in the ladle, which is part of the method for producing ultra-high purity pig iron for casting using ordinary pig iron produced in a blast furnace according to the present invention. Figure 1 The process includes a ladle of molten iron and the molten iron (ordinary pig iron produced by a blast furnace). The surface of the molten iron is covered with iron slag. An agitator is inserted into the surface of the molten iron and rotated to stir it. CaO powder is added while stirring.
[0023] Figure 2 This is a schematic diagram of the strong oxidation smelting deployment in an oxygen converter involved in implementing the method of producing ultra-high purity pig iron for casting using ordinary pig iron produced by a blast furnace according to the present invention. Figure 2 The process includes a converter and the molten iron inside. The surface of the molten iron is covered with iron slag. The oxygen lance blows oxygen (O2 gas, supplied by an oxygen tank) into the surface of the molten iron through its oxygen nozzle. Detailed Implementation
[0024] The following describes the embodiments and accompanying drawings ( Figures 1-2 The present invention will be described below.
[0025] Figure 1 This is a schematic diagram illustrating the pretreatment and desulfurization deployment of ordinary pig iron produced in the blast furnace in the ladle, which is part of the method for producing ultra-high purity pig iron for casting using ordinary pig iron produced in a blast furnace according to the present invention. Figure 2 This is a schematic diagram illustrating the strong oxidation smelting deployment in an oxygen converter involved in implementing a method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace, according to the present invention. (Reference) Figures 1 to 2As shown, a method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace includes adding molten ordinary pig iron from the blast furnace as raw material to a ladle, desulfurizing it using a single CaO desulfurization powder via KR mechanical stirring, then adding the molten iron to an oxidation converter, and using an oxygen flow rate of 20,000–30,000 Nm³. 3 An oxygen lance operating at / h blows oxygen from above the molten iron surface into the inner layer of the iron to remove impurities through strong oxidation. The elemental wt% content of ultra-high purity pig iron for casting is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.010, Mn ≤ 0.040, P ≤ 0.012, S ≤ 0.015, Cr ≤ 0.012, V ≤ 0.008, Mo ≤ 0.006, Sn ≤ 0.0010, Sb ≤ 0.0005, Pb ≤ 0.0003, Bi ≤ 0.00005, Te ≤ 0.0003, As ≤ 0.0015, B ≤ 0.0005, Al ≤ 0.010.
[0026] The elemental wt% content of ultra-high purity pig iron for casting is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.008, Mn ≤ 0.030, P ≤ 0.010, S ≤ 0.012, Cr ≤ 0.010, V ≤ 0.005, Mo ≤ 0.005, Sn ≤ 0.0005, Sb ≤ 0.0004, Pb ≤ 0.0002, Bi ≤ 0.00003, Te ≤ 0.0001, As ≤ 0.0012, B ≤ 0.0003, Al ≤ 0.010. The elemental wt% content of ultra-high purity pig iron for casting is as follows: C≥3.30, Si≤0.50, Ti≤0.005, Mn≤0.020, P≤0.008, S≤0.010, Cr≤0.008, V≤0.003, Mo≤0.003, Sn≤0.0003, Sb≤0.0003, Pb≤0.0001, Bi≤0.00001, Te≤0.00005, As≤0.0008, B≤0.0001, Al≤0.005. The elemental wt% content of molten iron produced by blast furnace is as follows: C ≥ 4.5, Si ≤ 0.80, Ti ≤ 0.031, Mn ≤ 0.11, P ≤ 0.12, S ≤ 0.052, Cr ≤ 0.028, V ≤ 0.025, Mo ≤ 0.004, Sn ≤ 0.0003, Sb ≤ 0.0008, Pb ≤ 0.0023, Bi ≤ 0.0001, Te ≤ 0.0004, As ≤ 0.0005, B ≤ 0.002, Al ≤ 0.02.
[0027] The top inlet of the molten iron ladle is connected to a hopper via a chute. The hopper has a CaO powder outlet. A rotary agitator is installed on the top of the molten iron ladle. The cross-shaped stirring head of the rotary agitator extends into the surface of the molten iron and rotates under the drive of a motor. CaO powder is added while stirring to achieve the following desulfurization reaction:
[0028] CaO + FeS = CaS + FeO
[0029] 2FeO + Si = 2Fe + SiO2
[0030] Through the above reactions, the S content in the molten iron is reduced to ≤0.005.
[0031] The molten iron temperature in the oxidation converter is ≤1380℃ in order to control carbon loss in the molten iron during the strong oxidation process. Lime, iron ore, and dolomite are added to the furnace during the strong oxidation oxygen blowing smelting process to control slag basicity and molten iron temperature. Iron ore and dolomite act as cooling agents, and scrap steel is not used as a cooling agent. In the strong oxidation oxygen blowing smelting process, the slag basicity control adopts the principle of low at the beginning and high at the end. In the early stage of blowing, a low basicity control of R=1.5~1.8 is adopted to facilitate the oxidation and removal of manganese. In the middle and late stages of blowing, a high basicity control of R=2.5~3.5 is adopted to facilitate the oxidation and removal of phosphorus. Sb and Pb in the molten iron are evaporated and removed at the smelting temperature. Ti, Mn, P, Cr, V, B and Al in the molten iron are all oxidized and removed during blowing. When it is detected that all elements meet the target requirements for ultra-high purity pig iron for casting, the strong oxidation endpoint of the converter is reached. Then, the temperature of the molten iron is adjusted to 1410~1450℃ for a short time to compensate for the temperature drop during the tapping process. The molten iron is tapped from the converter into the ladle and then cast into ultra-high purity pig iron blocks using a casting machine.
[0032] During the process of tapping molten iron from the converter into the ladle, a carburizing agent or ferrosilicon is added along with the iron flow to meet the preset limits on the C or Si content of the molten iron. Slag-blocking is used during the tapping process, with the slag remaining in the converter and poured into a slag ladle from the large furnace opening.
[0033] This invention is a method for obtaining ultra-high purity pig iron by using ordinary pig iron produced in a blast furnace as raw material and performing KR desulfurization and oxidation in steps to remove harmful and trace elements, thereby achieving the required composition of ultra-high purity pig iron.
[0034] 1. Ultra-high purity pig iron for casting is pig iron with extremely low levels of conventional harmful elements and trace impurities. It is an indispensable high-quality raw material in the high-end casting field, and its chemical composition requirements are as follows:
[0035] Table 1. Common Elements in Ultra-High Purity Pig Iron for Casting
[0036]
[0037] Table 2 Trace Elements in Ultra-High Purity Pig Iron for Casting
[0038]
[0039]
[0040] The composition of molten iron produced by blast furnaces is as follows:
[0041] Table 3. Composition of ordinary pig iron produced by blast furnace (w, %)
[0042] C Si Ti Mn P S Cr V Mo 4.5 0.8 0.031 0.11 0.12 0.052 0.028 0.025 0.004 Sn Sb Pb Bi Te As B Al 0.0003 0.0008 0.0023 0.0001 0.0004 0.0005 0.002 0.02
[0043] Note: Mo, Sn, Bi, Te, and As elements in ordinary molten iron have higher oxygen potential than carbon and are difficult to remove by oxidation. However, due to their extremely low content, the requirements can be met by paying a little attention when selecting raw materials.
[0044] 2. The main steps for producing ultra-high purity pig iron for casting, using molten pig iron from blast furnaces as raw material, and carrying out KR desulfurization and oxidation to remove harmful elements and trace impurities, are as follows:
[0045] 1) Process flow. Blast furnace molten iron → KR molten iron pretreatment and desulfurization → slag removal → oxygen converter strong oxidation smelting → ultra-high purity pig iron.
[0046] 2) Desulfurize molten iron produced by blast furnace using the KR method.
[0047] The KR method is used to stir and desulfurize the molten iron in the ladle. The motor drives the cross-shaped stirrer, which descends to a certain depth from the surface of the molten iron. At the same time, a certain amount of lime powder is added to the surface of the molten iron while the stirrer is rotating, which will remove the sulfur in the molten iron to an extremely low level.
[0048] Since this desulfurization method uses only lime as the desulfurizing agent and the slag contains no oxidizing materials, other elements remain largely unchanged during the desulfurization process, although the silicon content in the molten iron decreases slightly. The main desulfurization reactions are: CaO + FeS = CaS + FeO, 2FeO + Si = 2Fe + SiO2. When the sulfur content in the molten iron is reduced to ≤0.005%, this desulfurization process is complete. The desulfurization slag on the surface of the molten iron is then removed using a slag remover, and a certain amount of heat-insulating agent is added to the surface before proceeding to the next process.
[0049] 3) Strong oxidation is used to remove harmful conventional elements and trace elements after desulfurization.
[0050] The desulfurized molten iron is added to the converter and subjected to strong oxidizing smelting by blowing oxygen. During the oxygen blowing smelting process, lime and cooling agents (iron ore, dolomite, etc.) are added to the furnace to control the slag alkalinity and molten iron temperature. Scrap steel is not used as a cooling agent because it contains high levels of impurities that are difficult to remove.
[0051] The total oxygen blowing time is 5-11 minutes, completing the strong oxidation smelting of the molten iron in the converter. The composition of the molten iron after the strong oxidation smelting is as follows:
[0052] Table 4. Composition of molten iron (w%) after strong oxidation smelting
[0053] C Si Ti Mn P S Cr V Mo 3.7 0.005 0.0003 0.015 0.001 0.008 0.002 0.002 0.003 Sn Sb Pb Bi Te As B Al 0.0003 0.0003 0.0001 0.0001 0.0005 0.0005 0.0001 0.003
[0054] To achieve optimal oxidation and removal of harmful and impurity elements, the temperature and basicity of molten iron must be strictly controlled during oxygen blowing smelting. During the strong oxidation process, to prevent carbon loss in the molten iron, the smelting temperature must be controlled at ≤1380℃. If the molten iron temperature is improperly controlled (>1410℃), the carbon in the molten iron will react violently with oxygen, releasing a large amount of heat instantaneously, which will weaken the oxidation of other elements by oxygen, thus reducing the effectiveness of removing harmful conventional elements and trace impurities. Therefore, during the early oxidation stage of oxygen blowing, cooling agents such as lime, ore, and dolomite (scrap steel is strictly prohibited) should be continuously added to control the molten iron temperature at ≤1380℃.
[0055] Controlling the temperature of molten iron during strong oxygen blowing oxidation has a good inhibitory effect on carbon oxidation. However, the high carbon content in the molten iron and the frequent contact with oxygen lead to a certain degree of carbon oxidation. Due to oxidation, the final carbon content decreases, generally within the range of 2.8% to 4.1%.
[0056] During the oxygen blowing strong oxidation process, alkalinity control is also very necessary. The alkalinity control follows the principle of low at the beginning and high at the end. In the early stage of blowing, a low alkalinity of R=1.5 to 1.8 is used, which is conducive to the oxidation and removal of manganese. In the middle and late stages of blowing, the slag alkalinity is increased to R=2.5 to 3.5, which is conducive to the oxidation and removal of phosphorus.
[0057] During the final stage of strong oxidation smelting in the converter, Sb and Pb, which are volatile elements, can be evaporated and removed at this smelting temperature. The oxidation removal rate of conventional harmful elements such as Ti, Mn, and P, as well as trace impurities such as Cr, V, B, and Al, can all reach over 90%. The composition of the ultra-high purity pig iron meets the standard requirements, completing the production of ultra-high purity pig iron. It is now ready to be tapped from the converter into the ladle.
[0058] Before tapping (i.e., at the end of the strong oxidation process in the converter), the temperature and individual components of the molten iron are adjusted. The temperature of the molten iron is adjusted to 1410-1450℃ by blowing oxygen for a short time to compensate for the temperature drop during tapping, and the preparation for tapping is completed. If there are special requirements for the carbon or silicon in the molten iron, a carburizing agent or ferrosilicon can be added with the iron stream during the tapping process to complete the adjustment of the composition of the molten iron.
[0059] Iron tapping is complete. After the composition and temperature are adjusted, the converter is rotated, and the molten iron enters the ladle from the tapping spout. Iron is tapped using a slag-blocking method, and the slag remains in the converter and is poured into the slag ladle from the large furnace opening. Iron tapping is then complete.
[0060] 4) The prepared ultra-high purity molten iron is cast into iron blocks using a casting machine, thus completing the entire production and preparation process.
[0061] This invention uses ordinary molten iron produced by blast furnace to produce ultra-high purity pig iron. Compared with the production of ultra-high purity pig iron using high-purity pig iron, the cost of carefully selected raw materials is greatly reduced.
[0062] The method of this invention has a short processing time. Compared with the weak oxidation method, the strong oxidation method saves more than 50 minutes of processing time, reduces the temperature drop during the process, and reduces the consumption of refractory materials, thus significantly reducing production costs.
[0063] The strong oxidation method has a strong ability to remove harmful conventional elements and trace impurities, reducing their content to extremely low levels, resulting in a high yield of ultra-high purity pig iron. It also boasts high oxygen utilization, saving on oxygen consumption.
[0064] The strong oxidation method used in this invention to produce high-purity pig iron reduces the overall cost by half compared to the weak oxidation method.
[0065] High-purity pig iron is produced using a strong oxidation method, which can produce large quantities in a single process, meeting the requirements for ultra-high-purity pig iron for ultra-large tonnage castings.
[0066] Contents not described in detail in this specification are existing technologies known to those skilled in the art. It is hereby indicated that the above description is intended to help those skilled in the art understand the present invention, but does not limit the scope of protection of the present invention. Any equivalent substitutions, modifications, improvements, and / or simplifications of the above descriptions that do not depart from the essence of the present invention fall within the scope of protection of the present invention.
Claims
1. A method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace, characterized in that, This process involves adding ordinary pig iron produced in a blast furnace as raw material to a ladle, desulfurizing it using a single CaO desulfurization powder via KR mechanical stirring, then adding the molten iron to an oxidation converter, and using an oxygen lance with an oxygen flow rate of 20,000 to 30,000 Nm³ / h to blow oxygen from above the surface of the molten iron into the surface layer for strong oxidation to remove impurity elements from the molten iron. The elemental wt% content of ultra-high purity pig iron for casting is as follows: C≥3.30, Si≤0.50, Ti≤0.010, Mn≤0.040, P≤0.012, S≤0.015, Cr≤0.012, V≤0.008, Mo≤0.006, Sn≤0.0010, Sb≤0.0005, Pb≤0.0003, Bi≤0.00005, Te≤0.0003, As≤0.0015, B≤0.0005, Al≤0.010; The top inlet of the molten iron ladle is connected to a hopper via a discharge chute. The hopper has a CaO powder outlet. A rotary agitator is installed on the top of the molten iron ladle. The cross-shaped stirring head of the rotary agitator extends into the surface of the molten iron and rotates under the drive of a motor. CaO powder is added while stirring to achieve the following desulfurization reaction: CaO + FeS = CaS + FeO 2FeO + Si = 2Fe + SiO2 Through the above reactions, the S content in the molten iron is ≤0.005; In the strong oxidation oxygen blowing smelting process, the slag basicity control adopts the principle of low at the beginning and high at the end. In the early stage of blowing, a low basicity control of R=1.5~1.8 is adopted to facilitate the oxidation and removal of manganese. In the middle and late stages of blowing, a high basicity control of R=2.5~3.5 is adopted to facilitate the oxidation and removal of phosphorus. Sb and Pb in the molten iron are evaporated and removed at the smelting temperature. Ti, Mn, P, Cr, V, B and Al in the molten iron are all oxidized and removed during blowing. When it is detected that all elements meet the target requirements for ultra-high purity pig iron for casting, the strong oxidation endpoint of the converter is reached. Then, the temperature of the molten iron is adjusted to 1410~1450℃ for a short time to compensate for the temperature drop during the tapping process. The molten iron is tapped from the converter into the ladle and then cast into ultra-high purity pig iron blocks using a casting machine.
2. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, The elemental wt% content of ultra-high purity pig iron for casting is as follows: C ≥ 3.30, Si ≤ 0.50, Ti ≤ 0.008, Mn ≤ 0.030, P ≤ 0.010, S ≤ 0.012, Cr ≤ 0.010, V ≤ 0.005, Mo ≤ 0.005, Sn ≤ 0.0005, Sb ≤ 0.0004, Pb ≤ 0.0002, Bi ≤ 0.00003, Te ≤ 0.0001, As ≤ 0.0012, B ≤ 0.0003, Al ≤ 0.
010.
3. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, The elemental wt% content of ultra-high purity pig iron for casting is as follows: C≥3.30, Si≤0.50, Ti≤0.005, Mn≤0.020, P≤0.008, S≤0.010, Cr≤0.008, V≤0.003, Mo≤0.003, Sn≤0.0003, Sb≤0.0003, Pb≤0.0001, Bi≤0.00001, Te≤0.00005, As≤0.0008, B≤0.0001, Al≤0.
005.
4. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, The elemental wt% content of molten iron produced by blast furnace is as follows: C ≥ 4.5, Si ≤ 0.80, Ti ≤ 0.031, Mn ≤ 0.11, P ≤ 0.12, S ≤ 0.052, Cr ≤ 0.028, V ≤ 0.025, Mo ≤ 0.004, Sn ≤ 0.0003, Sb ≤ 0.0008, Pb ≤ 0.0023, Bi ≤ 0.0001, Te ≤ 0.0004, As ≤ 0.0005, B ≤ 0.002, Al ≤ 0.
02.
5. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, The molten iron temperature in the oxidation converter is ≤1380℃ in order to control carbon loss in the molten iron during the strong oxidation process. Lime, iron ore, and dolomite are added to the furnace during the strong oxidation oxygen blowing smelting process to control slag basicity and molten iron temperature. Iron ore and dolomite act as cooling agents, and scrap steel is not used as a cooling agent.
6. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, During the process of tapping molten iron from the converter into the ladle, a carburizing agent or ferrosilicon is added along with the iron flow to meet the preset limits on the C or Si content of the molten iron.
7. The method for producing ultra-high purity pig iron for casting using ordinary pig iron from a blast furnace according to claim 1, characterized in that, During the process of tapping molten iron from the converter into the ladle, slag is blocked during tapping, and the slag remains in the converter and is poured into the slag pot from the large furnace opening.
Citation Information
Patent Citations
Converting process for converter low-silicon molten iron
CN101117651A
Method of preliminary treatment for molten iron in converter
JP2013136831A
Method for manufacturing foundry pig iron
KR101424643B1