Method for fabricating optical waveguide by femtosecond laser wet etching and liquid filling and optical waveguide
By employing femtosecond laser wet etching and liquid infusion methods, the problems of high precision and high loss in three-dimensional waveguide fabrication have been solved, enabling the fabrication of high-precision, low-loss optical waveguides.
Patent Information
- Application Number
- CN202210681326.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-06-15
AI Technical Summary
Existing three-dimensional waveguide fabrication processes result in poor accuracy, high loss, large processing roughness, low flexibility, and poor modifiability of three-dimensional waveguides.
The method employs femtosecond laser wet etching and liquid infusion to form a modified region by focusing a femtosecond laser on a transparent substrate, and then etching an etching channel in an etching solution. Subsequently, composite resin or organic polymer is infused to form an optical waveguide structure.
It improves the flexibility and modifiability of optical waveguide fabrication, reduces optical transmission loss, and enhances processing accuracy and repeatability.
Smart Images

Figure CN117270105B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to optical waveguides and methods for fabricating optical waveguides, specifically to a method for fabricating optical waveguides based on femtosecond laser wet etching and liquid infusion, and the optical waveguide fabricated therefrom. Background Technology
[0002] An optical waveguide is a structure that utilizes the principle of total internal reflection at an optically denser or less dense interface to transmit light waves with low loss. Optical waveguides play a crucial role in photonic integrated circuits. Increasing the fabrication dimensions of the waveguide, optimizing its quality, and reducing its loss are key to improving the performance of photonic integrated circuits. The principle is that when light is incident from an optically denser (high-refractive-index core layer) to an optically less dense (low-refractive-index cladding layer) interface at a certain angle, total internal reflection occurs, confining the light wave within a waveguide structure of a certain size and propagating along the predetermined direction of the waveguide.
[0003] Optical waveguides are the most fundamental building blocks in photonic integrated circuits, possessing functions such as active gain, signal transmission, and nonlinear transformation. They have significant applications in photonic integrated circuits, and have already been used to create photonic integrated devices such as beam splitters, electro-optic modulators, waveguide gratings, waveguide lasers, frequency converters, and directional couplers. Currently, waveguide fabrication is mainly divided into two categories: planar waveguide fabrication and three-dimensional waveguide fabrication. Planar waveguide fabrication methods include proton / ion exchange, ion implantation, photolithography, high-frequency sputtering, plasma polymerization, and thermal diffusion particle exchange, but these processes are complex, the equipment is expensive, and most importantly, the applications of planar waveguides are limited. Three-dimensional waveguide fabrication mainly involves 3D printing and femtosecond laser direct-writing waveguide technology. 3D printed three-dimensional waveguides have large dimensions, poor precision, and high losses. Femtosecond laser direct-writing technology is currently a hot research topic, but it has relatively high surface roughness, insufficient flexibility, and poor modifiability. Once the material is selected, the degree of material modification by the laser is limited, which in turn limits the optimization of waveguide losses. Summary of the Invention
[0004] The purpose of this invention is to solve the technical problems of poor accuracy, high loss, large processing roughness, low flexibility and poor modifiability of existing three-dimensional waveguide fabrication processes. The invention proposes a femtosecond laser wet etching and liquid infusion method for fabricating optical waveguides and an optical waveguide thereof.
[0005] The technical solution of this invention is as follows:
[0006] A method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, characterized by the following steps:
[0007] A1. Place the transparent substrate on the processing table, focus the femtosecond laser inside the transparent substrate, and modify the transparent substrate according to the predetermined path to form a modified area;
[0008] A2. Immerse the modified transparent substrate in the etching solution for etching to form etching channels in the modified area. Place the etched transparent substrate in an alcohol solution with a volume concentration of 90-95% for ultrasonic cleaning for 3-15 minutes, and then take it out and dry it.
[0009] A3. Elevate the first end of the etching channel to tilt the transparent substrate. Drop composite resin into the first end of the etching channel. The refractive index of the composite resin is higher than that of the transparent substrate. After the composite resin flows from the first end of the etching channel to the second end, place the transparent substrate horizontally for 20 to 500 seconds. Then place the transparent substrate in a vacuum chamber to remove residual gas caused by the composite resin flowing into the etching channel and gas dissolved in the composite resin.
[0010] A4. Remove the transparent substrate from the vacuum chamber, cure the composite resin and combine it with the transparent substrate to form a complete optical waveguide structure.
[0011] Furthermore, in step A1, the laser power of the femtosecond laser is 1mW-30mW; the scanning speed of the femtosecond laser is 5μm / s-500μm / s;
[0012] The transparent substrate is a quartz glass substrate;
[0013] The etching solution is an HF acid solution with a volume concentration of 3%-30%, and the etching time is 2-7 hours.
[0014] The femtosecond laser is generated by a Ti:sapphire laser, a light conversion laser, or a fiber laser.
[0015] In step A3, the composite resin is a photocurable composite resin or a thermocurable composite resin.
[0016] Furthermore, in step A1, the laser power of the femtosecond laser is 5mW-15mW; the scanning speed of the femtosecond laser is 5μm / s-200μm / s.
[0017] This invention also provides an optical waveguide fabricated using the above-described femtosecond laser wet etching and liquid infusion method, characterized in that:
[0018] Including the core layer and the cladding layer;
[0019] The core layer is a composite resin layer, and the cladding layer is a transparent base layer;
[0020] The optical refractive index of the composite resin layer is greater than that of the transparent substrate layer.
[0021] Meanwhile, this invention also provides another method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, which is characterized by including the following steps:
[0022] B1. Place the transparent substrate on the processing table, focus the femtosecond laser inside the transparent substrate, and modify the transparent substrate according to the predetermined path to form a modified area;
[0023] B2. Immerse the modified transparent substrate in the etching solution for etching to form etching channels in the modified area. Place the etched transparent substrate in an alcohol solution with a volume concentration of 90-95% for ultrasonic cleaning for 3-15 minutes, and then take it out and dry it.
[0024] B3. Preparation of organic polymer coating:
[0025] B3.1 The transparent substrate treated in step B2 is immersed in a mixed solution of organic polymer and volatile solvent for 1 min to 5 days; the organic polymer can adhere to and precipitate on the inner wall of the etched channel;
[0026] B3.2 Remove the transparent substrate and allow it to stand until the volatile solvent has completely evaporated, forming an organic polymer film on the inner wall surface of the etched channel;
[0027] B3.3 Determine whether the thickness of the organic polymer film formed on the inner wall of the etching channel meets the design requirements;
[0028] If so, the organic polymer coating preparation is complete, proceed to step B4;
[0029] If not, proceed to step B3.4;
[0030] B3.4 Immerse the transparent substrate again in a mixed solution of organic polymer and volatile solvent for 1 minute to 5 days;
[0031] B3.5 The transparent substrate was removed again and allowed to stand until the volatile solvent had completely evaporated, forming an organic polymer film on the inner wall of the etched channel once more.
[0032] B3.6 Determine whether the thickness of the organic polymer film formed on the inner wall of the etching channel meets the design requirements;
[0033] If so, the organic polymer coating preparation is complete, proceed to step B4;
[0034] If not, return to step B3.4;
[0035] B4. Elevate the first end of the etching channel with the organic polymer coating to tilt the transparent substrate. Drop composite resin into the first end of the etching channel. The refractive index of the composite resin is higher than that of the organic polymer coating. After the composite resin flows from the first end of the etching channel to the second end, place the transparent substrate horizontally for 20 to 500 seconds. Then place the transparent substrate in a vacuum chamber and evacuate to remove residual gas caused by the composite resin flowing into the etching channel and gas dissolved in the composite resin.
[0036] B5. Remove the transparent substrate from the vacuum chamber, cure the composite resin and combine it with the organic polymer cladding to form a complete optical waveguide structure.
[0037] Furthermore, in step B1, the laser power of the femtosecond laser is 1mW-30mW; the scanning speed of the femtosecond laser is 5μm / s-500μm / s;
[0038] The transparent substrate is a quartz glass substrate;
[0039] The etching solution is an HF acid solution with a volume concentration of 3%-30%, and the etching time is 2-7 hours.
[0040] The femtosecond laser is generated by a Ti:sapphire laser, a light conversion laser, or a fiber laser.
[0041] Furthermore, in step B1, the laser power of the femtosecond laser is 5mW-15mW; the scanning speed of the femtosecond laser is 5μm / s-200μm / s.
[0042] Further, in step B3, the organic polymer is polymethyl methacrylate, and the volatile solvent is acetone;
[0043] The concentration of the polymethyl methacrylate acetone solution is 0.01 g / ml to 0.3 g / ml.
[0044] The organic polymer can also be polystyrene (PS) or polycarbonate (PC), and the volatile organic solvent can also be ethanol. It can be formulated into polymethyl methacrylate ethanol solution, polystyrene acetone solution, polycarbonate acetone solution, polystyrene ethanol solution, or polycarbonate ethanol solution.
[0045] Furthermore, in step B4, the composite resin is a photocurable composite resin or a thermocurable composite resin.
[0046] This invention also provides an optical waveguide fabricated using yet another femtosecond laser wet etching and liquid infusion method, characterized in that:
[0047] Includes waveguide core, waveguide cladding, and outer shell;
[0048] The waveguide core layer is a composite resin layer, and the waveguide cladding is an organic polymer cladding;
[0049] The outer shell is a transparent substrate layer used to protect the waveguide cladding and waveguide core layer;
[0050] The optical refractive index of the composite resin layer is higher than that of the organic polymer coating.
[0051] The beneficial effects of this invention are:
[0052] 1. This invention fabricates optical waveguides by combining femtosecond laser wet etching and liquid infusion. On the one hand, femtosecond laser wet etching can fabricate three-dimensional etching channels of arbitrary shapes as needed; on the other hand, liquid infusion can select the infusion material to fabricate the waveguide as needed, greatly improving the flexibility and modifiability of the fabrication.
[0053] 2. In this invention, the optical waveguide is fabricated inside a transparent material, which reduces the cleanliness requirements of the external environment.
[0054] 3. By directly injecting composite resin into the etching channel to prepare the waveguide core layer, the high uniformity of the inner wall surface of the etching channel formed by wet etching makes the contact surface between the waveguide core layer and the etching channel uniform and flat, which improves the precision of waveguide processing; the diameter and uniformity of the etching channel are controllable, and the repeatability of optical waveguide preparation is high.
[0055] 4. By injecting a mixture of an organic polymer that can adhere to the wall and a volatile organic solvent into the etched channel, an organic polymer cladding is prepared as the waveguide cladding. Then, a composite resin is injected to prepare the waveguide core layer. Since the surface flatness of the prepared organic polymer cladding is higher, the precision of waveguide processing and the accuracy of light propagation are further improved, and the loss in the light transmission process is reduced.
[0056] 5. Using an organic polymer cladding as the waveguide cladding and a composite resin as the waveguide core layer allows the materials of both the waveguide cladding and the waveguide core layer to be adjusted according to the actual needs of the light waves, resulting in greater processing flexibility and easier process improvement. Attached Figure Description
[0057] Figure 1 This is a flowchart of Example 1 of the method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion according to the present invention;
[0058] Figure 2 This is a flowchart of Example 2 of the method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion according to the present invention;
[0059] Figure 3 This is a schematic diagram of femtosecond laser modification of a quartz glass substrate in an embodiment of the present invention;
[0060] Figure 4 This is a schematic diagram of the etching of the modified quartz glass substrate in HF acid solution in an embodiment of the present invention;
[0061] Figure 5 This is a schematic diagram of the etching channel in an embodiment of the present invention;
[0062] Figure 6 This is a schematic diagram of an acetone solution used for injecting polymethyl methacrylate in an embodiment of the present invention;
[0063] Figure 7 This is an axial cross-sectional view of the etched channel forming the polymethyl methacrylate coating in an embodiment of the present invention;
[0064] Figure 8 This is a radial cross-sectional view of the etched channel forming the polymethyl methacrylate coating in an embodiment of the present invention;
[0065] Figure 9 This is a schematic diagram of the infusion of photocurable composite resin in an embodiment of the present invention;
[0066] Figure 10 This is a schematic diagram of the curing process of the photocurable composite resin in an embodiment of the present invention;
[0067] Figure 11 This is a radial cross-sectional view of the optical waveguide formed by the photocurable composite resin and the polymethyl methacrylate cladding in an embodiment of the present invention.
[0068] The attached figures are labeled as follows:
[0069] 1-Femtosecond laser, 2-Modified region, 3-Quartz glass substrate, 4-HF acid solution, 5-Etching channel, 6-Polymethyl methacrylate acetone solution, 7-Polymethyl methacrylate cladding, 8-Photocurable composite resin, 9-Ultraviolet light source. Detailed Implementation
[0070] Example 1
[0071] See Figure 1 This embodiment provides a method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, the method comprising the following steps:
[0072] A1, see also Figure 3A quartz glass substrate 3 is placed on a three-dimensional processing stage. A Gaussian femtosecond laser generated by a Ti:sapphire laser is sequentially focused through an aperture, an attenuator, a quarter-wave plate, an aperture, a beam lifter, and an objective lens system. The femtosecond laser 1 is then focused inside the quartz glass substrate 3. The movement trajectory of the three-dimensional processing stage is controlled by a program to modify the sample along a predetermined path, forming a modified region 2. The beam lifter is a reflector that elevates the laser beam. The laser power is controlled between 1mW and 30mW by adjusting the attenuator, preferably between 5mW and 15mW. The scanning speed is controlled between 5μm / s and 500μm / s, preferably between 5μm / s and 200μm / s. Laser power and scanning speed can control the modified region and thus the uniformity of the channels subsequently etched. If the laser power is too high or the scanning speed is too low, the surface of the quartz glass substrate will be deformed, and defects are likely to occur. If the laser power is too low or the scanning speed is too high, the uniformity of the etched channels will be poor. In this embodiment, a scanning speed of 25 μm / s is selected. Within the range of laser power of 5 mW-15 mW, a modified region 2 with excellent performance can be obtained.
[0073] Understandably, the laser can also be a light conversion laser, a fiber laser, or another laser capable of focusing femtosecond laser light into a quartz glass substrate for modification.
[0074] A2, see also Figure 4 The modified quartz glass substrate 3 is immersed in HF acid solution 4 for etching for 2-7 hours to form etching channels 5. The volume concentration of HF acid solution 4 is 3%-30%. If the concentration of HF acid solution 4 is too high, surface defects in the etching channel 5 increase; if the concentration is too low, the etching rate is too slow. In this embodiment, a 10% concentration of HF acid solution is selected. After etching with HF acid solution 4, etching channels 5 with a certain diameter (30μm-100μm) are formed. If the diameter is small, the channel uniformity is insufficient, which will affect the waveguide transmission loss. To obtain a larger diameter channel, the etching time will be very long. Therefore, in this embodiment, a channel with a diameter of 45μm is selected. See [link to relevant documentation]. Figure 5 After etching, the quartz glass substrate 3 is immersed in an alcohol solution with a volume concentration of 90-95% and ultrasonically cleaned for 15 minutes, then removed and dried.
[0075] A3, see also Figure 9The first end of the etching channel 5 is raised to tilt the quartz glass substrate 3. A photocurable composite resin 8 is then dripped into the first end of the etching channel 5. The photocurable composite resin has a higher refractive index than the transparent substrate. The quartz glass substrate 3 forms an angle greater than 0° and less than 30° with the horizontal plane. This tilting is primarily to allow the liquid photocurable composite resin 8 to flow from one end to the other. The appropriate angle is selected based on the viscosity of the chosen composite resin; a smaller tilt angle (0°-15°) is used when the resin viscosity is low, and a larger angle (10°-30°) is used when the resin viscosity is high. After the photocurable composite resin 8 flows from the first end of the etching channel 5 to the second end, the quartz glass substrate 3 is horizontally stabilized for 20-500 seconds. Then, the quartz glass substrate 3 is placed in a vacuum chamber to remove residual gas caused by the inflow of the photocurable composite resin into the etching channel, as well as dissolved gas in the photocurable composite resin. This prevents the formation of an air layer in the optical waveguide structure, which would increase transmission loss.
[0076] A4, see also Figure 10 and Figure 11 The quartz glass substrate 3 is removed from the vacuum chamber and cured by the ultraviolet light source 9. The photocurable composite resin 8 is cured and forms a complete optical waveguide structure with the quartz glass substrate 3. It can be understood that the filling in step A3 can also be a thermocurable composite resin. The selected photocurable composite resin 8 or thermocurable composite resin should meet the following requirements: low viscosity, easy to pour; low shrinkage rate, small shrinkage range after curing, and close fit with the etched channel 5 on the quartz glass substrate 3; and high optical refractive index, forming a certain optical refractive index difference with the quartz glass substrate 3.
[0077] The three-dimensional optical waveguide fabricated using the above-mentioned femtosecond laser wet etching and liquid infusion method includes a photocurable composite resin layer and a quartz glass substrate 3. The refractive index of the photocurable composite resin layer is higher than that of the quartz glass substrate 3. This optical waveguide has a replaceable core material, and different core layers can be selected to be fabricated according to different infusion materials to optimize the waveguide performance.
[0078] Example 2
[0079] See Figure 2 This embodiment provides a method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, the method comprising the following steps:
[0080] B1, the same as A1 in Example 1;
[0081] B2, the same as A2 in Example 1;
[0082] B3. Preparation of organic polymer coating:
[0083] See B3.1 Figure 6The quartz glass substrate 3 after step B2 is immersed in a mixed solution of polymethyl methacrylate (PMMA) and acetone for 1 min to 5 days. The concentration of the polymethyl methacrylate-acetone solution 6 is 0.01 g / ml to 0.3 g / ml, preferably 0.02 g / ml to 0.12 g / ml. The concentration of the polymethyl methacrylate-acetone solution 6 affects the continuity of the cladding. When the concentration is too low, it is difficult to form a complete and continuous cladding in the channel. When the concentration is too high, PMMA will block the channel. The immersion time affects the quality of the cladding. When the time is too short, the cladding surface is not smooth, which will affect the transmission loss of the waveguide. The time should not be too long either, as the fixed concentration of polymethyl methacrylate-acetone solution 6 will evaporate completely after a certain time, and the immersion time is too long, which does not optimize the cladding surface morphology. Generally, 10 min to 3 days is selected. In this embodiment, it is selected to be immersed in polymethyl methacrylate-acetone solution 6 for 18 hours. Understandably, the organic polymer can also be polystyrene (PS) or polycarbonate (PC), and the volatile organic solvent can also be ethanol, etc.
[0084] B3.2 Remove the quartz glass substrate 3 and let it stand until the acetone has completely evaporated, forming a polymethyl methacrylate film on the inner wall of the etching channel 5;
[0085] B3.3 Determine whether the thickness of the polymethyl methacrylate film formed on the inner wall of the etched channel 5 meets the design requirements; if yes, the polymethyl methacrylate coating preparation is complete, proceed to step B4; if no, proceed to step B3.4.
[0086] B3.4 Immerse the quartz glass substrate 3 again in a mixed solution of polymethyl methacrylate and acetone for 18 hours;
[0087] B3.5 Remove the quartz glass substrate 3 again and let it stand until the volatile solvent has completely evaporated, so that a polymethyl methacrylate film is formed again on the inner wall surface of the etching channel 5.
[0088] B3.6 Determine whether the thickness of the polymethyl methacrylate (PMMA) film formed on the inner wall of etched channel 5 meets the design requirements; if so, the PMMA coating preparation is complete. See [link to relevant documentation]. Figures 7-8 If not, proceed to step B4; otherwise, return to step B3.4. The number of soaking times will affect the thickness of the coating. The more times you soak, the thicker the coating will be. However, the number of soaking times should not be too many, as it will block the channels. In this embodiment, 1-5 soaking times are selected.
[0089] B4, see also Figure 9The first end of the etching channel 5 with the polymethyl methacrylate (PMMA) coating 7 is raised to tilt the quartz glass substrate 3. A photocurable composite resin 8 is then dropped into the first end of the etching channel 5. The refractive index of the photocurable composite resin 8 is higher than that of the PMMA coating. The quartz glass substrate 3 forms an angle greater than 0° and less than 30° with the horizontal plane. This tilting is primarily to allow the liquid to flow from one end to the other. The appropriate angle is selected based on the viscosity of the chosen composite resin. When the composite resin viscosity is low, the tilt angle will be smaller (0°-15°), and when the composite resin viscosity is high, it can be larger (10°-30°). After the photocurable composite resin 8 flows from the first end of the etching channel 5 to the second end, the quartz glass substrate 3 is left horizontally still for 20-500 seconds. Then, the quartz glass substrate 3 is placed in a vacuum chamber to remove residual gas caused by the inflow of the photocurable composite resin into the etching channel, as well as dissolved gas in the photocurable composite resin. This prevents the formation of an air layer in the optical waveguide structure, which would increase the transmission loss of the optical waveguide.
[0090] B5. Remove the quartz glass substrate 3 from the vacuum chamber. (See below) Figure 10 Under ultraviolet light source 9, the photocurable composite resin 8 cures and forms a complete optical waveguide structure with the polymethyl methacrylate cladding layer 7. (See [reference]). Figure 11 It is understandable that the filler in step B3 can also be a thermosetting composite resin. The selected light-curing composite resin 8 or thermosetting composite resin should meet the following requirements: low viscosity, easy to pour; low shrinkage rate, small shrinkage range after curing, and close adhesion with polymethyl methacrylate coating 7; high optical refractive index, forming a certain optical refractive index difference with polymethyl methacrylate coating 7.
[0091] The three-dimensional optical waveguide fabricated using the aforementioned femtosecond laser wet etching and liquid infusion method comprises a waveguide core, a waveguide cladding, and a shell. The waveguide core is a composite resin layer, and the waveguide cladding is an organic polymer cladding. The shell is a quartz glass substrate 3, used to protect the waveguide cladding and waveguide core. The refractive index of the composite resin layer is higher than that of the organic polymer cladding. The waveguide structure features replaceable materials; the cladding can be fabricated using different organic polymers, and the core layer can be fabricated using different composite resins, allowing for further optimization of the waveguide's performance. Furthermore, this optical waveguide integrates the advantages of polymer waveguides and silicon-based waveguides: firstly, it has a high thermo-optic coefficient; secondly, the material properties used to fabricate the waveguide can be improved and optimized through molecular engineering; and finally, this waveguide is compatible with traditional semiconductor processes and has high integration.
Claims
1. A method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, characterized in that, Includes the following steps: A1. Place the transparent substrate on the processing table, focus the femtosecond laser (1) inside the transparent substrate, and modify the transparent substrate according to the predetermined path to form a modified area (2). A2. Immerse the modified transparent substrate in the etching solution for etching to form an etching channel (5) in the modified area (2); place the etched transparent substrate in an alcohol solution with a volume concentration of 90-95% for ultrasonic cleaning for 3-15 minutes and then take it out and dry it. A3. Elevate the first end of the etching channel (5) to tilt the transparent substrate, forming an angle greater than 0° and less than 30° between the transparent substrate and the horizontal plane. Select an appropriate angle according to the viscosity of the composite resin to be dripped in, and drip the composite resin into the first end of the etching channel (5). The refractive index of the composite resin is higher than that of the transparent substrate. After the composite resin flows from the first end of the etching channel (5) to the second end of the etching channel (5), place the transparent substrate horizontally for 20 to 500 seconds, and then place the transparent substrate in a vacuum chamber to evacuate. The composite resin is a photocurable composite resin (8) or a thermocurable composite resin. A4. Remove the transparent substrate from the vacuum chamber, cure the composite resin and combine it with the transparent substrate to form a complete optical waveguide structure.
2. The method for fabricating optical waveguides by femtosecond laser wet etching and liquid infusion according to claim 1, characterized in that: In step A1, the laser power of the femtosecond laser (1) is 1mW-30mW; the scanning speed of the femtosecond laser (1) is 5μm / s-500μm / s; the femtosecond laser (1) is generated by a Ti:sapphire laser, a light conversion laser, or a fiber laser. The transparent substrate is a quartz glass substrate (3); In step A2, the etching solution is an HF acid solution (4), the volume concentration of the HF acid solution (4) is 3%-30%, and the etching time is 2-7 hours.
3. The method for fabricating optical waveguides by femtosecond laser wet etching and liquid infusion according to claim 2, characterized in that: In step A1, the laser power of the femtosecond laser (1) is 5mW-15mW; the scanning speed of the femtosecond laser (1) is 5μm / s-200μm / s.
4. An optical waveguide fabricated using the femtosecond laser wet etching and liquid infusion method according to any one of claims 1-3, characterized in that: Includes the core layer and the cladding layer; The core layer is a composite resin layer, and the cladding layer is a transparent base layer; The refractive index of the composite resin layer is higher than that of the transparent substrate layer.
5. A method for fabricating optical waveguides using femtosecond laser wet etching and liquid infusion, characterized in that, Includes the following steps: B1. Place the transparent substrate on the processing table, focus the femtosecond laser (1) inside the transparent substrate, and modify the transparent substrate according to the predetermined path to form a modified area (2). B2. Immerse the modified transparent substrate in the etching solution for etching to form an etching channel (5) in the modified area (2); place the etched transparent substrate in an alcohol solution with a volume concentration of 90-95% for ultrasonic cleaning for 3-15 minutes and then take it out and dry it. B3. Preparation of organic polymer coating: B3.1 The transparent substrate treated in step B2 is immersed in a mixed solution of organic polymer and volatile solvent for 1 min to 5 days; the organic polymer can be deposited on the inner wall of the etching channel (5); B3.2 Remove the transparent substrate and let it stand until the volatile solvent has completely evaporated, forming an organic polymer film on the inner wall surface of the etched channel (5); B3.3 Determine whether the thickness of the organic polymer film formed on the inner wall of the etched channel (5) meets the design requirements; If so, the organic polymer coating preparation is complete, proceed to step B4; If not, proceed to step B3.4; B3.4 Immerse the transparent substrate again in a mixed solution of organic polymer and volatile solvent for 1 minute to 5 days; B3.5 The transparent substrate was removed again and left to stand until the volatile solvent completely evaporated, and an organic polymer film was formed again on the inner wall surface of the etched channel (5); B3.6 Determine whether the thickness of the organic polymer film formed on the inner wall of the etched channel (5) meets the design requirements; If so, the organic polymer coating preparation is complete, proceed to step B4; If not, return to step B3.4; B4. Elevate the first end of the etching channel (5) with the organic polymer coating to tilt the transparent substrate. Drop composite resin into the first end of the etching channel (5). The refractive index of the composite resin is higher than that of the organic polymer coating. After the composite resin flows from the first end of the etching channel (5) to the second end of the etching channel (5), place the transparent substrate horizontally for 20 to 500 seconds, and then place the transparent substrate in a vacuum chamber to evacuate. The composite resin is a photocurable composite resin (8) or a thermocurable composite resin. B5. Remove the transparent substrate from the vacuum chamber, cure the composite resin and combine it with the organic polymer cladding to form a complete optical waveguide structure.
6. The method for fabricating optical waveguides by femtosecond laser wet etching and liquid infusion according to claim 5, characterized in that: In step B1, the laser power of the femtosecond laser (1) is 1mW-30mW; the scanning speed of the femtosecond laser (1) is 5μm / s-500μm / s; the femtosecond laser (1) is generated by a Ti:sapphire laser, a light conversion laser, or a fiber laser. The transparent substrate is a quartz glass substrate (3); In step B2, the etching solution is an HF acid solution (4), the volume concentration of the HF acid solution (4) is 3%-30%, and the etching time is 2-7 hours.
7. The method for fabricating optical waveguides by femtosecond laser wet etching and liquid infusion according to claim 6, characterized in that: In step B1, the laser power of the femtosecond laser (1) is 5mW-15mW; the scanning speed of the femtosecond laser (1) is 5μm / s-200μm / s.
8. The method for fabricating optical waveguides by femtosecond laser wet etching and liquid infusion according to any one of claims 5-7, characterized in that: In step B3, the organic polymer is polymethyl methacrylate, and the volatile solvent is acetone; The concentration of the polymethyl methacrylate acetone solution (6) is 0.01 g / ml to 0.3 g / ml.
9. An optical waveguide fabricated using the femtosecond laser wet etching and liquid infusion method according to any one of claims 5-8, characterized in that: Includes waveguide core, waveguide cladding, and outer shell; The waveguide core layer is a composite resin layer, and the waveguide cladding is an organic polymer cladding; The outer shell is a transparent substrate layer used to protect the waveguide cladding and waveguide core layer; The optical refractive index of the composite resin layer is higher than that of the organic polymer coating.
Citation Information
Patent Citations
Method for preparing microfluid optical waveguide on glass substrate using femtosecond laser