Metal oxide semiconductor thin film transistor array substrate and method of manufacturing the same
By using a bridging layer to protect the vias in the fabrication process of metal oxide semiconductor thin film transistor array substrates, the problem of etching solution entering the metal oxide semiconductor layer is solved, improving product yield and reducing manufacturing costs.
Patent Information
- Application Number
- CN202311272751.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-09-28
AI Technical Summary
In the fabrication process of thin-film transistor array substrates using metal oxide semiconductors, when problems occur with the source/drain electrodes and the data lines and peripheral conductors formed on the same layer, the etching solution enters the metal oxide semiconductor layer through vias, causing functional abnormalities, resulting in reduced product yield and increased manufacturing costs.
A bridging layer and an initial metal layer are formed using the same photomask pattern on the etch barrier layer. The bridging layer is connected to the metal oxide semiconductor layer through vias. When rework is required, the initial metal layer is removed and a reset metal layer is formed on the bridging layer. The bridging layer protects the vias and prevents etchant from entering, thus solving the problem using existing photomask processes.
It improves product yield, avoids the risk of wire breakage at the through-hole position when resetting the metal layer, reduces manufacturing costs, and causes no damage during the film removal and rework process, simplifying the process flow.
Smart Images

Figure CN117276195B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of display technology, and in particular to a metal oxide semiconductor thin film transistor array substrate and its fabrication method. Background Technology
[0002] Liquid crystal display panels have advantages such as good image quality, small size, light weight, low driving voltage, low power consumption, no radiation, and relatively low manufacturing cost, and they dominate the flat panel display field.
[0003] A liquid crystal display panel consists of an opposing thin-film transistor array substrate and a color filter substrate, with liquid crystal molecules filling the space between them. Fabricating the thin-film transistor array substrate requires multiple deposition, photolithography, and etching processes to create the gate, gate insulating layer, semiconductor layer, source / drain electrodes, pixel electrodes, and protective layers of the thin-film transistors.
[0004] In thin-film transistor array substrates with metal oxide semiconductor layers, the source / drain electrodes need to contact and connect with the metal oxide semiconductor layer through vias on the etch barrier layer. When problems occur with the source / drain electrodes and the data lines and surrounding conductors formed on the same layer, requiring film stripping and rework, the entire metal layer forming the source / drain electrodes needs to be etched away using etching solution during the stripping and rework process. The etching solution will flow into the metal oxide semiconductor layer through the vias on the etch barrier layer and etch away the metal oxide at the via locations, ultimately causing the metal oxide semiconductor layer to malfunction.
[0005] Therefore, in the process of fabricating thin-film transistor array substrates using metal oxide semiconductors, if a batch-specific anomaly occurs in the metal layer forming the source / drain during the process, the entire semi-finished product can only be stripped multiple times to restore it to a smooth glass state or be scrapped. Moreover, multiple stripping will also damage the glass body, increasing the probability of subsequent breakage, ultimately resulting in a decrease in yield and an increase in manufacturing costs. Summary of the Invention
[0006] The purpose of this invention is to provide a metal oxide semiconductor thin film transistor array substrate and its fabrication method, which can improve product yield and reduce manufacturing costs.
[0007] This invention provides a method for fabricating a metal-oxide-semiconductor (MOS) thin-film transistor (TFT) array substrate, comprising: providing a MOS thin-film transistor (TFT) array substrate, wherein the MOS thin-film transistor (TFT) array substrate includes a substrate, a MOS layer and an etch barrier layer stacked on the substrate; and...
[0008] A bridging layer and an initial metal layer are formed using the same photomask pattern on the etch stop layer; wherein, the formed bridging layer includes a first bridging pattern and a second bridging pattern spaced apart, the etch stop layer has a first via and a second via, the first bridging pattern is contacted and connected to the metal oxide semiconductor layer through the first via, and the second bridging pattern is contacted and connected to the metal oxide semiconductor layer through the second via; the formed initial metal layer includes an initial source and an initial drain, the initial source is stacked on the first bridging pattern, and the initial drain is stacked on the second bridging pattern;
[0009] Furthermore, when the initial metal layer requires rework, the initial metal layer is removed; and
[0010] A reset metal layer is patterned on the bridging layer. The reset metal layer includes a reset source and a reset drain that are spaced apart. The reset source is stacked on the first bridging pattern, and the reset drain is stacked on the second bridging pattern.
[0011] Further, the metal-oxide-semiconductor thin-film transistor array substrate has a display area and a non-display area; the metal-oxide-semiconductor layer is located in the display area; the metal-oxide-semiconductor thin-film transistor array substrate further includes a gate metal layer, the gate metal layer including a gate located in the display area and a first peripheral conductor located in the non-display area, the gate being located above or below the metal-oxide-semiconductor layer; the bridging layer further includes a third bridging pattern located in the non-display area, the etch stop layer is further disposed in the non-display area and has a third via, the third bridging pattern being contacted and connected to the first peripheral conductor through the third via; the initial metal layer further includes an initial second peripheral conductor overlapping the third bridging pattern, and the fabrication method further includes:
[0012] Removing the initial metal layer also includes removing the initial second peripheral conductor; and
[0013] When the reset metal layer is patterned, the reset metal layer also includes a reset second peripheral conductor, which is overlapped on the third bridging pattern.
[0014] Furthermore, the metal oxide semiconductor thin film transistor array substrate further includes a gate insulating layer, the gate metal layer is formed on the substrate, the gate insulating layer is formed on the substrate and covers the gate metal layer, the metal oxide semiconductor layer is formed on the gate insulating layer, the etch barrier layer is formed on the gate insulating layer and covers the metal oxide semiconductor layer, and the bridging layer is formed on the etch barrier layer.
[0015] Furthermore, the reset metal layer and the bridging layer are patterned using the same photomask.
[0016] Further, the method for patterning the bridging layer and the initial metal layer includes: depositing a bridging material layer and a first photoresist layer on the substrate after the etch stop layer is formed; patterning the bridging material layer using the photomask to form the bridging layer; depositing an initial metal material layer and a second photoresist layer on the substrate after the bridging layer is formed; and patterning the initial metal material layer using the photomask used to form the bridging layer to form the initial metal layer. Alternatively, a bridging material layer, an initial metal material layer, and a third photoresist layer are sequentially deposited on the substrate after the etch stop layer is formed; and the initial metal material layer and the bridging material layer are sequentially patterned using the photomask to form the initial metal layer and the bridging layer.
[0017] Furthermore, the material of the reset metal layer is the same as that of the initial metal layer; the bridging layer is formed of a transparent conductive material.
[0018] Furthermore, when the initial metal layer does not require rework, the fabrication method further includes:
[0019] A first passivation layer is formed on the etch barrier layer, the first passivation layer covering the reset metal layer;
[0020] A planarization layer is formed on the first passivation layer;
[0021] A first electrode layer is formed on the planarization layer;
[0022] A second passivation layer is formed on the planarization layer, and the second passivation layer covers the first electrode layer;
[0023] A fourth via is formed at the location of the reset drain corresponding to the second passivation layer, the planarization layer, and the first passivation layer to expose the reset drain; and
[0024] A second electrode layer is patterned on the second passivation layer and then filled into the fourth via to make contact with the reset drain electrode.
[0025] Furthermore, the metal oxide semiconductor thin film transistor array substrate further includes a gate insulating layer, the gate metal layer is formed on the substrate, the gate insulating layer is formed on the substrate and covers the gate metal layer, the metal oxide semiconductor layer is formed on the gate insulating layer, the etch barrier layer is formed on the gate insulating layer and covers the metal oxide semiconductor layer, and the bridging layer is formed on the etch barrier layer.
[0026] Furthermore, the manufacturing method also includes:
[0027] A first passivation layer is formed on the etch barrier layer, the first passivation layer covering the initial metal layer;
[0028] A planarization layer is formed on the first passivation layer;
[0029] A first electrode layer is formed on the planarization layer;
[0030] A second passivation layer is formed on the planarization layer, and the second passivation layer covers the first electrode layer;
[0031] A fourth via is formed at the location of the second passivation layer, the planarization layer, and the first passivation layer corresponding to the initial drain to expose the initial drain; and
[0032] A second electrode layer is patterned on the second passivation layer and then filled into the fourth via to contact and connect with the initial drain electrode.
[0033] The present invention also provides a metal oxide semiconductor thin film transistor array substrate, which is manufactured by the above-described method for manufacturing a metal oxide semiconductor thin film transistor array substrate.
[0034] In the method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate provided by this invention, when a problem occurs in the initial metal layer requiring rework, a bridging layer located above the first, second, and third vias protects them. During etching of the initial metal layer, this prevents the etching solution from entering the metal-oxide-semiconductor layer through the first and second vias and etching it, thus preventing functional abnormalities. It also prevents the etching solution from entering the first peripheral conductor through the third via and etching it, thus preventing abnormal connections to subsequently formed conductors. This improves product yield. Furthermore, the bridging layer fills the first, second, and third vias, and the subsequent reset metal layer forms a conductive connection with the bridging layer, avoiding the risk of breakage at the via location. Moreover, the problem can be solved using existing photomask processes, causing no damage to the array substrate during rework and eliminating the need for multiple rework processes to achieve a smooth glass surface, thus reducing manufacturing costs.
[0035] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and to make other objects, features and advantages of the above-mentioned metal oxide semiconductor thin film transistor array substrate and its fabrication method of the present invention more apparent and understandable, preferred embodiments are described below in detail with reference to the accompanying drawings. Attached Figure Description
[0036] Figures 1a to 1g This is a schematic diagram of the cross-sectional structure of the metal oxide semiconductor thin film transistor array substrate in each step of the fabrication method of the metal oxide semiconductor thin film transistor array substrate according to the first embodiment of the present invention.
[0037] Figures 2a to 2h This is a schematic diagram of the cross-sectional structure of the metal oxide semiconductor thin film transistor array substrate in each step of patterning to form the bridging layer and the initial metal layer in the fabrication method of the metal oxide semiconductor thin film transistor array substrate according to the first embodiment of the present invention.
[0038] Figures 3a to 3d This is a schematic diagram of the cross-sectional structure of the metal oxide semiconductor thin film transistor array substrate in each step of patterning to form the bridging layer and the initial metal layer in the fabrication method of the metal oxide semiconductor thin film transistor array substrate according to the second embodiment of the present invention. Detailed Implementation
[0039] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description, in conjunction with the accompanying drawings and preferred embodiments, details the specific implementation methods, structures, features, and effects of the metal oxide semiconductor thin-film transistor array substrate and its fabrication method according to the present invention:
[0040] The foregoing and other technical contents, features, and effects of the present invention will be clearly presented in the following detailed description of preferred embodiments with reference to the accompanying drawings. Through the description of the specific embodiments, a more in-depth and specific understanding can be gained of the technical means and effects adopted by the present invention to achieve its intended purpose. However, the accompanying drawings are for reference and illustration only and are not intended to limit the present invention.
[0041] [First Embodiment]
[0042] The preferred embodiment of the present invention provides a metal-oxide-semiconductor thin-film transistor array substrate having a display area 101 and a non-display area 102. The display area 101 is used to display images, and the non-display area 102 is used to house peripheral components such as driving circuits. The specific steps of the method for fabricating the metal-oxide-semiconductor thin-film transistor array substrate are as follows:
[0043] Please see Figure 1a A substrate 110 is provided, and a gate metal layer 120 is patterned on the substrate 110. The gate metal layer 120 includes a gate 121 located in the display area 101 and a first peripheral conductor 122 located in the non-display area 102.
[0044] Please see Figure 1bA gate insulating layer 130 is deposited on the substrate 110, and the gate insulating layer 130 covers the gate metal layer 120. A metal oxide semiconductor layer 140 is patterned on the gate insulating layer 130.
[0045] In this embodiment, the metal-oxide-semiconductor layer 140 is located in the display area 101. The gate 121 is formed before the metal-oxide-semiconductor layer 140, and therefore is located below the metal-oxide-semiconductor layer 140. In other embodiments, the gate 121 may also be located above the metal-oxide-semiconductor layer 140, that is, the gate 121 is formed after the metal-oxide-semiconductor layer 140.
[0046] Please see Figure 1c An etch barrier layer 150 is patterned on the gate insulating layer 130 and covers the metal oxide semiconductor layer 140. A first via 150a and a second via 150b are provided on the etch barrier layer 150 in the display area 101 to expose the metal oxide semiconductor layer 140. A third via 150c is provided through the etch barrier layer 150 and the gate insulating layer 130 in the non-display area 102 to expose the first peripheral conductor 122.
[0047] Please see Figure 1d A bridging layer 160 and an initial metal layer 170A are patterned on the etch stop layer 150. The bridging layer 160 includes a first bridging pattern 161 and a second bridging pattern 162 spaced apart. The first bridging pattern 161 is connected to the metal-oxide-semiconductor layer 140 through a first via 150a, and the second bridging pattern 162 is connected to the metal-oxide-semiconductor layer 140 through a second via 150b. The initial metal layer 170A includes an initial source 171A and an initial drain 172A. The initial source 171A is stacked on the first bridging pattern 161, and the initial drain 172A is stacked on the second bridging pattern 162.
[0048] Furthermore, the bridging layer 160 also includes a third bridging pattern 163 located in the non-display area 102, the third bridging pattern 163 being contacted and connected to the first peripheral conductor 122 through a third through-hole 150c. The initial metal layer 170A also includes an initial second peripheral conductor 173A overlapping the third bridging pattern 163.
[0049] The metal-oxide-semiconductor thin-film transistor array substrate formed by the above-described fabrication steps includes a substrate 110, a gate metal layer 120, a gate insulating layer 130, a metal-oxide-semiconductor layer 140, an etch stop layer 150, a bridging layer 160, and an initial metal layer 170A. The gate metal layer 120 is formed on the substrate 110, the gate insulating layer 130 is formed on the substrate 110 and covers the gate metal layer 120, the metal-oxide-semiconductor layer 140 is formed on the gate insulating layer 130, the etch stop layer 150 is formed on the gate insulating layer 130 and covers the metal-oxide-semiconductor layer 140, the bridging layer 160 is formed on the etch stop layer 150, and the initial metal layer 170A is formed on the bridging layer 160.
[0050] When problems arise in the initial metal layer 170A (initial source 171A and initial drain 172A) of the metal oxide semiconductor thin-film transistor array substrate after its formation, requiring rework, the fabrication method of the metal oxide semiconductor thin-film transistor array substrate further includes:
[0051] like Figure 1e As shown, the initial metal layer 170A is removed.
[0052] like Figure 1f As shown, a reset metal layer 170 is patterned on the bridging layer 160. The reset metal layer 170 includes a reset source 171 and a reset drain 172 spaced apart. The reset source 171 is stacked on the first bridging pattern 161, and the reset drain 172 is stacked on the second bridging pattern 162.
[0053] Furthermore, when removing the initial metal layer 170A, the initial second peripheral conductor 173A is also removed; and when patterning to form the reset metal layer 170, the reset metal layer 170 also includes a reset second peripheral conductor 173, which is overlapped on the third bridging pattern 163.
[0054] In this embodiment, the same photomask 300 is used when forming the bridging layer 160, the initial metal layer 170A, and the reset metal layer 170 (e.g., ...). Figure 2b Patterning is performed as shown. The patterning process includes cleaning, applying photoresist, exposure, development, and photoresist removal.
[0055] When the initial metal layer 170A (initial source 171A and initial drain 172A) does not require rework, the next fabrication process can proceed directly after the initial metal layer 170A is formed.
[0056] Furthermore, such as Figure 1g As shown, the method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate further includes:
[0057] A first passivation layer 181 is formed on the etch barrier layer 150, and the first passivation layer 181 covers the initial metal layer 170A / reset metal layer 170; that is, when no film stripping and rework is required, the first passivation layer 181 directly covers the initial metal layer 170A, and when film stripping and rework are required, the first passivation layer 181 covers the reset metal layer 170.
[0058] A planarization layer 182 is formed on the first passivation layer 181;
[0059] A first electrode layer 183 is formed on the planarization layer 182;
[0060] A second passivation layer 184 is formed on the planarization layer 182, and the second passivation layer 184 covers the first electrode layer 183;
[0061] A fourth via 184a is formed at the positions of the second passivation layer 184, planarization layer 182, and first passivation layer 181 corresponding to the initial drain 172A / reset drain 172 to expose the initial drain 172A / reset drain 172; and
[0062] A second electrode layer 185 is patterned on the second passivation layer 184 and the second electrode layer 185 is filled into the fourth via 184a and makes contact with the initial drain 172A / reset drain 172.
[0063] Please refer to Figures 2a to 2h In this embodiment, the method for patterning the bridging layer 160 and the initial metal layer 170A includes:
[0064] A bridging material layer 16 is deposited on the substrate 110 after the etch barrier layer 150 is formed, and the bridging material layer 16 is patterned using a photomask 300 to form a bridging layer 160. An initial metal material layer 17 is deposited on the substrate 110 after the bridging layer 160 is formed, and the initial metal material layer 17 is patterned using the photomask 300 used to form the bridging layer 160 to form an initial metal layer 170A.
[0065] Specifically, such as Figure 2a As shown, a bridging material layer 16 and a first photoresist layer 310 are sequentially deposited on the substrate 110 after the etch barrier layer 150 is formed.
[0066] like Figure 2b As shown, the first photoresist 310 is ashing processed using a photomask 300 to form a first photoresist pattern 311.
[0067] like Figure 2c As shown, the bridging material layer 16 is etched under the cover of the first photoresist pattern 311, and the bridging material layer 16 is patterned to form the bridging layer 160.
[0068] like Figure 2d As shown, the first photoresist pattern 311 is removed.
[0069] like Figure 2e As shown, an initial metal material layer 17 and a second photoresist layer 320 are sequentially deposited on the substrate 110 after the bridging layer 160 is formed.
[0070] like Figure 2f As shown, the second photoresist 320 is ashing processed again using the photomask 300 to form the second photoresist pattern 321.
[0071] like Figure 2g As shown, the initial metal material layer 17 is etched under the cover of the second photoresist pattern 321, and the initial metal material layer 17 is patterned to form the initial metal layer 170A.
[0072] like Figure 2h As shown, the second photoresist pattern 321 is removed.
[0073] Since the patterned bridging layer 160 and the initial metal layer 170A both use the same photomask 300, the formed bridging layer 160 and the initial metal layer 170A are arranged in overlapping contact and have the same pattern.
[0074] Furthermore, the initial metal layer 170A is made of the same material as the reset metal layer 170, for example, both using a three-layer structure of molybdenum (Mo) / aluminum (Al) / molybdenum (Mo), or copper (Cu). The bridging layer 160 is formed of a transparent conductive material, such as tin-doped indium trioxide (ITO) or aluminum-doped zinc oxide (AZO). When copper is used to fabricate the initial metal layer 170A or the reset metal layer 170, the bridging layer 160 also prevents copper ions from diffusing into the metal oxide semiconductor layer 140 and affecting its semiconductor performance.
[0075] Furthermore, the metal oxide semiconductor layer 140 is made of an oxide containing at least one or more elements selected from zinc, indium, gallium, tin, aluminum, silicon, scandium, titanium, vanadium, yttrium, zirconium, niobium, molybdenum, hafnium, tantalum, tungsten, and lanthanides. Examples include indium gallium zinc oxide (IGZO), indium zinc oxide (IZO), lanthanide rare earth doped indium zinc oxide (Ln-IZO), indium tin zinc oxide (ITZO), or indium gallium zinc tin oxide (IGZTO).
[0076] The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate provided in this embodiment of the invention protects the first via 150a, the second via 150b, and the third via 150c from being exposed to a problem and requiring rework when the initial metal layer 170A has a problem. This prevents the etching solution from entering the metal-oxide-semiconductor layer 14 through the first via 150a and the second via 150b during the etching of the initial metal layer 170A. The etching process prevents the metal oxide semiconductor layer 140 from malfunctioning due to etching, and also prevents the etching solution from entering the first peripheral conductor 122 through the third via 150c and etching it, thus preventing subsequent conductors from having abnormal connections. This improves product yield. Furthermore, the bridging layer 160 fills the first via 150a, the second via 150b, and the third via 150c, and the subsequently formed reset metal layer 170 makes contact with the bridging layer 160 for conductive connection, avoiding the risk of the reset metal layer 170 breaking at the via location. Moreover, the existing photomask process can solve the problem, causing no damage to the array substrate during the rework process, and eliminating the need for multiple rework processes to achieve a smooth glass surface, thus reducing manufacturing costs.
[0077] [Second Embodiment]
[0078] The fabrication method of the metal-oxide-semiconductor thin-film transistor array substrate in the second embodiment differs from that in the first embodiment in that the method for patterning the bridging layer 160 and the initial metal layer 170A is different. In this embodiment, the method for patterning the bridging layer 160 and the initial metal layer 170A includes:
[0079] A bridging material layer 16, an initial metal material layer 17, and a third photoresist 330 are sequentially deposited on the substrate 110 after the etch barrier layer 150 is formed. The initial metal material layer 17 and the bridging material layer 16 are sequentially patterned using a photomask 300 to form an initial metal layer 170A and a bridging layer 160.
[0080] Specifically, such as Figure 3a As shown, a bridging material layer 16, an initial metal material layer 17, and a third photoresist 330 are sequentially deposited on the substrate 110 after the etch barrier layer 150 is formed.
[0081] like Figure 3b As shown, the third photoresist 330 is ashing processed using a photomask 300 to form the third photoresist pattern 331.
[0082] like Figure 3c As shown, under the cover of the third photoresist pattern 331, the initial metal material layer 17 is first etched to form the initial metal layer 170A. After changing the etching solution, the bridging material layer 16 is etched to form the bridging layer 160.
[0083] like Figure 3d As shown, the third photoresist pattern 331 is removed.
[0084] The fabrication methods for the other films in this embodiment are the same as those in the first embodiment, and will not be repeated here.
[0085] The present invention also relates to a metal oxide semiconductor thin film transistor array substrate, which is manufactured by the above-described method for manufacturing a metal oxide semiconductor thin film transistor array substrate.
[0086] The metal oxide semiconductor thin film transistor array substrate and its fabrication method provided by the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate, characterized in that, The manufacturing method includes: A metal-oxide-semiconductor (MOS) thin-film transistor (TFT) array substrate is provided, the MOS thin-film transistor array substrate comprising a substrate (110), a MOS layer (140) stacked on the substrate (110), and an etch barrier layer (150); and A bridging layer (160) and an initial metal layer (170A) are patterned on the etch barrier layer (150) using the same photomask (300); wherein the formed bridging layer (160) includes a first bridging pattern (161) and a second bridging pattern (162) spaced apart, and the etch barrier layer (150) is provided with a first via (150a) and a second via (150b), and the first bridging pattern (161) is connected to the metal oxide through the first via (150a). The metal oxide semiconductor layer (140) is contacted and connected, and the second bridging pattern (162) is contacted and connected to the metal oxide semiconductor layer (140) through the second via (150b); the formed initial metal layer (170A) includes an initial source (171A) and an initial drain (172A), the initial source (171A) is stacked on the first bridging pattern (161), and the initial drain (172A) is stacked on the second bridging pattern (162).
2. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 1, characterized in that, When the initial metal layer (170A) requires rework, the manufacturing method further includes: Remove the initial metal layer (170A); and A reset metal layer (170) is patterned on the bridging layer (160). The reset metal layer (170) includes a reset source (171) and a reset drain (172) spaced apart. The reset source (171) is stacked on the first bridging pattern (161), and the reset drain (172) is stacked on the second bridging pattern (162).
3. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 2, characterized in that, The metal-oxide-semiconductor thin-film transistor array substrate has a display area (101) and a non-display area (102); the metal-oxide-semiconductor layer (140) is located in the display area (101); the metal-oxide-semiconductor thin-film transistor array substrate further includes a gate metal layer (120), the gate metal layer (120) includes a gate (121) located in the display area (101) and a first peripheral conductor (122) located in the non-display area (102), the gate (121) being located in the metal-oxide-semiconductor layer (140). Above or below; the bridging layer (160) further includes a third bridging pattern (163) located in the non-display area (102), the etch barrier layer (150) is also disposed in the non-display area (102) and has a third via (150c), the third bridging pattern (163) is contacted and connected to the first peripheral conductor (122) through the third via (150c); the initial metal layer (170A) further includes an initial second peripheral conductor (173A) overlapping the third bridging pattern (163), the fabrication method further includes: Removing the initial metal layer (170A) also includes removing the initial second peripheral conductor (173A); and When the reset metal layer (170) is patterned, the reset metal layer (170) also includes a reset second peripheral conductor (173) which is overlapped on the third bridging pattern (163).
4. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 3, characterized in that, The metal-oxide-semiconductor thin-film transistor array substrate further includes a gate insulating layer (130), a gate metal layer (120) formed on the substrate (110), the gate insulating layer (130) formed on the substrate (110) and covering the gate metal layer (120), a metal-oxide-semiconductor layer (140) formed on the gate insulating layer (130), an etch stop layer (150) formed on the gate insulating layer (130) and covering the metal-oxide-semiconductor layer (140), and a bridging layer (160) formed on the etch stop layer (150).
5. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 3, characterized in that, The reset metal layer (170) and the bridging layer (160) are patterned using the same photomask (300).
6. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 5, characterized in that, The method for patterning the bridging layer (160) and the initial metal layer (170A) includes: A bridging material layer (16) and a first photoresist (310) are deposited on the substrate (110) after the etch barrier layer (150) is formed. The bridging material layer (16) is patterned using the photomask (300) to form the bridging layer (160). An initial metal material layer (17) and a second photoresist (320) are deposited on the substrate (110) after the bridging layer (160) is formed. The initial metal material layer (17) is patterned using the photomask (300) that forms the bridging layer (160) to form the initial metal layer (170A). Alternatively, a bridging material layer (16), an initial metal material layer (17), and a third photoresist layer (330) may be sequentially deposited on the substrate (110) after the etch barrier layer (150) is formed, and the initial metal material layer (17) and the bridging material layer (16) may be sequentially patterned using the photomask (300) to form the initial metal layer (170A) and the bridging layer (160).
7. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 2, characterized in that, The reset metal layer (170) is made of the same material as the initial metal layer (170A); the bridging layer (160) is formed of a transparent conductive material.
8. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in any one of claims 2 to 7, characterized in that, The manufacturing method further includes: A first passivation layer (181) is formed on the etch barrier layer (150), and the first passivation layer (181) covers the reset metal layer (170); A planarization layer (182) is formed on the first passivation layer (181); A first electrode layer (183) is formed on the planar layer (182); A second passivation layer (184) is formed on the planarization layer (182), and the second passivation layer (184) covers the first electrode layer (183); A fourth via (184a) is formed in the second passivation layer (184), the planarization layer (182), and the first passivation layer (181) at the position corresponding to the reset drain (172) to expose the reset drain (172); and A second electrode layer (185) is patterned on the second passivation layer (184) and the second electrode layer (185) is filled into the fourth via (184a) and makes contact with the reset drain (172).
9. The method for fabricating a metal-oxide-semiconductor thin-film transistor array substrate as described in claim 1, characterized in that, When the initial metal layer (170A) does not require rework, the fabrication method further includes: A first passivation layer (181) is formed on the etch barrier layer (150), and the first passivation layer (181) covers the initial metal layer (170A); A planarization layer (182) is formed on the first passivation layer (181); A first electrode layer (183) is formed on the planar layer (182); A second passivation layer (184) is formed on the planarization layer (182), and the second passivation layer (184) covers the first electrode layer (183); A fourth via (184a) is formed in the second passivation layer (184), the planarization layer (182), and the first passivation layer (181) at the position corresponding to the initial drain (172A) to expose the initial drain (172A); and A second electrode layer (185) is patterned on the second passivation layer (184) and the second electrode layer (185) is filled into the fourth via (184a) and makes contact with the initial drain (172A).
10. A metal-oxide-semiconductor thin-film transistor array substrate, characterized in that, It is manufactured by the method of fabricating a metal oxide semiconductor thin film transistor array substrate according to any one of claims 1 to 9.
Citation Information
Patent Citations
Rework manufacture method of base holder in heterojunction bipolar transistor device
CN107958926A
Method for manufacturing FFS type array substrate and FFS type array substrate
CN108646487A