InGaN-based light emitting diode epitaxial wafer and preparation method thereof, LED
By introducing a porous InGaN/GaN superlattice structure into an InGaN-based LED epitaxial wafer, the problems of lattice mismatch and dislocation defects were solved, the internal quantum efficiency and external quantum efficiency were improved, and the light extraction efficiency was enhanced.
Patent Information
- Application Number
- CN202311458314.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-03
AI Technical Summary
Existing InGaN-based LED devices suffer from poor epitaxial quality due to lattice mismatch and dislocation defects, which affects both internal and external quantum efficiency, especially the low light extraction efficiency.
A porous InGaN/GaN superlattice structure is adopted, including a porous InGaN/GaN superlattice electron reserve layer and a porous InGaN/GaN superlattice hole reserve layer. The porous structure is formed by etching, which releases stress and improves the quality of the epitaxial layer, while improving the electron-hole matching degree and photon emission efficiency.
It significantly improves the internal and external quantum efficiency of InGaN-based LEDs, enhances the quality of epitaxial wafer materials, and improves the radiative recombination efficiency and photon emission efficiency in the active region.
Smart Images

Figure CN117276428B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of optoelectronic technology, and in particular to an InGaN-based light-emitting diode epitaxial wafer and its fabrication method, and LEDs. Background Technology
[0002] To obtain high-brightness LEDs, it is crucial to improve both the internal and external quantum efficiency of the device. Currently, GaN-based LED devices with InGaN quantum wells as the active layer are widely used in various fields. However, due to the lack of suitable homogeneous epitaxial substrates, GaN is usually grown on sapphire, silicon carbide, or silicon substrates with significant lattice mismatch. This lattice mismatch between GaN and the substrate undoubtedly creates numerous dislocation defects, thus affecting its epitaxial quality. Furthermore, because there is also a significant lattice mismatch between the InGaN quantum well active layer and GaN, the InGaN quantum well is subjected to compressive stress from GaN. Both dislocation defects and compressive stress negatively impact the performance of LED devices. While the internal quantum efficiency of blue GaN-based LEDs can reach over 80%, the external quantum efficiency of high-power LED chips is typically only around 40%. The main factor limiting the improvement of external quantum efficiency is the low light extraction efficiency of the chip. This is because the refractive index of GaN material differs significantly from that of air and the sapphire substrate, resulting in critical angles for total internal reflection at the air-GaN interface and the sapphire-GaN interface being only 23.6° and 44.4°, respectively. Only a small portion of the light generated in the active region can escape the bulk material. To improve the light extraction efficiency of the chip, the main technical solutions currently used domestically and internationally include growing distributed Bragg reflector (DBR) structures, patterned substrate (PSS) technology, surface roughening technology, and photonic crystal technology. PSS requires a high degree of pattern regularity, and given the hardness of the sapphire substrate, achieving uniformity and consistency across the entire pattern is challenging using both dry and wet etching processes. Furthermore, the fabrication process demands sophisticated equipment and processes, leading to high costs. DBR and photonic crystal fabrication processes are relatively complex and costly, while surface roughening technology, using either dry or wet etching processes, also presents significant challenges. Therefore, in order to improve the luminous efficiency of InGaN-based LEDs, that is, to improve the internal quantum efficiency and external quantum efficiency of LED devices, it is essential to improve the quality of epitaxial materials and increase the proportion of photon efferent materials in the active region by optimizing the epitaxial structure and process of InGaN-based LEDs. Summary of the Invention
[0003] The technical problem to be solved by this invention is to provide an InGaN-based light-emitting diode epitaxial wafer that can reduce the generation of defects in the epitaxial material during growth, reduce the dislocation density of the material, significantly improve the quality of the epitaxial wafer material, improve the insufficient hole concentration in the active region, and improve the electron-hole matching degree in the multi-quantum-well light-emitting layer, thereby improving the radiative recombination efficiency in the active region of the light-emitting diode, i.e., the internal quantum efficiency. At the same time, it can significantly increase the proportion of photon emanating material in the active region, i.e., improve the light extraction efficiency of the chip.
[0004] The technical problem to be solved by the present invention is to provide a method for preparing InGaN-based light-emitting diode epitaxial wafers, which has a simple process and can stably produce InGaN-based light-emitting diode epitaxial wafers with good luminous efficiency.
[0005] To address the aforementioned technical problems, this invention provides an InGaN-based light-emitting diode epitaxial wafer, comprising a substrate on which an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum-well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed.
[0006] In one embodiment, the porous InGaN / GaN superlattice electron reserve layer comprises alternating layers of undoped porous InGaN and a first undoped GaN layer, with the number of alternating growth cycles being 5 to 30.
[0007] The thickness of the undoped porous InGaN layer is 0.5 nm to 2 nm;
[0008] The thickness of the first undoped GaN layer is 1 nm to 5 nm;
[0009] The thickness ratio of the undoped porous InGaN layer to the first undoped GaN layer is 1:(2-3).
[0010] In one embodiment, the undoped porous InGaN layer is obtained by etching an InGaN layer. The etching process is as follows: under the conditions of a gas treatment temperature of 800℃~950℃ and a pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the InGaN layer is etched for 5s~50s to obtain an undoped porous InGaN layer.
[0011] In one embodiment, the InGaN / GaN superlattice well preparation layer includes alternating layers of undoped InGaN layers and Si-doped GaN layers, with the number of alternating growth cycles being 2 to 10.
[0012] The thickness of the undoped InGaN layer is 2.5 nm to 5 nm;
[0013] The thickness of the Si-doped GaN layer is 7 nm to 16 nm.
[0014] The thickness ratio of the undoped InGaN layer to the Si-doped GaN layer is 1:(3-5);
[0015] The Si doping concentration of the Si-doped GaN layer is 5 × 10⁻⁶. 17 atoms / cm 3 ~8×10 18 atoms / cm 3 .
[0016] In one embodiment, the porous InGaN / GaN superlattice hole reservoir layer comprises alternating layers of Mg-doped porous InGaN layers and a second undoped GaN layer, with the number of alternating growth cycles being 5 to 30.
[0017] The thickness of the Mg-doped porous InGaN layer is 0.5 nm to 2 nm;
[0018] The thickness of the second undoped GaN layer is 1 nm to 5 nm;
[0019] The thickness ratio of the Mg-doped porous InGaN layer to the second undoped GaN layer is 1:(2-3);
[0020] The Mg doping concentration of the Mg-doped porous InGaN layer is 2 × 10⁻⁶. 18 atoms / cm 3 ~5×10 19 atoms / cm 3 .
[0021] In one embodiment, the Mg-doped porous InGaN layer is obtained by etching a Mg-doped InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 5s~50s to obtain the Mg-doped porous InGaN layer.
[0022] To address the above problems, this invention also provides a method for fabricating an InGaN-based light-emitting diode epitaxial wafer, comprising the following steps:
[0023] S1. Prepare the substrate;
[0024] S2. Sequentially deposit an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer on the substrate.
[0025] In one embodiment, the porous InGaN / GaN superlattice electron reserve layer is prepared by the following method:
[0026] The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and In source were introduced to grow InGaN layer;
[0027] Then, the InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of InGaN layer is etched for 5s~50s to obtain an undoped porous InGaN layer.
[0028] The temperature of the reaction chamber is controlled at 800℃~900℃, the pressure is controlled at 20torr~300torr, and an N source and a Ga source are introduced. A first undoped GaN layer is deposited on the undoped porous InGaN layer, and the first undoped GaN layer fills the pores of the undoped porous InGaN layer.
[0029] The undoped porous InGaN layer and the first undoped GaN layer are alternately stacked to obtain the porous InGaN / GaN superlattice electron reserve layer.
[0030] In one embodiment, the porous InGaN / GaN superlattice hole reservoir layer is prepared by the following method:
[0031] The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow Mg-doped InGaN layer;
[0032] Then, the Mg-doped InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 5s~50s to obtain a Mg-doped porous InGaN layer.
[0033] The temperature of the reaction chamber is controlled at 800℃~900℃ and the pressure is controlled at 20 torr~300 torr. An N source and a Ga source are introduced to deposit a second undoped GaN layer on the Mg-doped porous InGaN layer. The second undoped GaN layer fills the pores of the Mg-doped porous InGaN layer.
[0034] The porous InGaN / GaN superlattice hole reserve layer is obtained by alternately stacking the Mg-doped porous InGaN layer and the second undoped GaN layer.
[0035] Accordingly, the present invention also provides an LED comprising the above-described InGaN-based light-emitting diode epitaxial wafer.
[0036] Implementing this invention has the following beneficial effects:
[0037] The InGaN-based light-emitting diode epitaxial wafer provided by the present invention comprises, sequentially on a substrate, an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer.
[0038] This invention designs a porous InGaN / GaN superlattice electron reservoir layer before the multi-quantum-well emitting layer and a porous InGaN / GaN superlattice hole reservoir layer after the multi-quantum-well emitting layer.
[0039] The porous InGaN / GaN superlattice electron storage layer includes alternating layers of undoped porous InGaN and a first undoped GaN layer. The porous InGaN layer is a porous structure formed by etching with H2 gas. After H2 gas treatment, materials with poor surface crystal quality are decomposed, which can effectively improve the quality of the epitaxial layer material. At the same time, the formation of an uneven porous structure can release the stress of the epitaxial layer, which is beneficial to the subsequent growth of a high-quality multi-quantum-well light-emitting layer.
[0040] Furthermore, the porous InGaN / GaN superlattice electron storage layer can store some electrons, thereby blocking electrons and reducing their mobility. This effectively improves the problem of electron-hole concentration mismatch in the active region and enhances the electron-hole matching degree in the multi-quantum-well light-emitting layer, thereby improving the luminous efficiency of InGaN-based blue LEDs or InGaN-based green LEDs.
[0041] The porous InGaN / GaN superlattice hole reserve layer comprises alternating layers of Mg-doped porous InGaN layer and a second undoped GaN layer. The Mg-doped porous InGaN layer is a porous structure formed by etching with H2 gas. After H2 gas treatment, materials with poor surface crystal quality are decomposed, which can effectively improve the quality of epitaxial layer materials. At the same time, it forms an uneven porous rough surface, which can effectively reduce in-plane total internal reflection of semiconductor materials and significantly increase the proportion of photon emanating material in the active region, that is, improve the light extraction efficiency of the chip.
[0042] Furthermore, the porous InGaN / GaN superlattice hole reservoir layer can store some holes to improve the hole injection efficiency of the P-type semiconductor layer. At the same time, the Mg-doped porous InGaN layer is doped with Mg, which can also provide some hole concentration to the multi-quantum well light-emitting layer to compensate for the problem of insufficient hole concentration in the active region. In addition, it can also block electrons and reduce electron mobility to prevent electrons from being injected into the P-type semiconductor layer and causing electron leakage.
[0043] In summary, the LED epitaxial wafer prepared using this invention can reduce the generation of defects in the epitaxial material during growth, lower the dislocation density of the material, significantly improve the quality of the epitaxial wafer material, improve the insufficient hole concentration in the active region, and increase the electron-hole matching degree in the multi-quantum-well light-emitting layer, thereby improving the radiative recombination efficiency in the active region of the light-emitting diode, i.e., the internal quantum efficiency. At the same time, it can significantly increase the proportion of photon emanating material in the active region, i.e., improve the light extraction efficiency of the chip. Attached Figure Description
[0044] Figure 1 This is a schematic diagram of the structure of the InGaN-based light-emitting diode epitaxial wafer provided by the present invention;
[0045] Figure 2 This is a flowchart illustrating the method for fabricating an InGaN-based light-emitting diode epitaxial wafer provided by the present invention. Detailed Implementation
[0046] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0047] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:
[0048] In this invention, "preferred" is merely a description of a more effective implementation method or embodiment, and should be understood as not constituting a limitation on the scope of protection of this invention.
[0049] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.
[0050] In this invention, numerical ranges are involved, and unless otherwise specified, they include the two endpoints of the numerical range.
[0051] To address the above problems, the present invention provides a light-emitting diode epitaxial wafer, such as... Figure 1 As shown, the substrate includes a substrate 100, on which are sequentially disposed an N-type semiconductor layer 200, a stress relief layer 300, a porous InGaN / GaN superlattice electron storage layer 400, an InGaN / GaN superlattice well preparation layer 500, a multi-quantum well light-emitting layer 600, a porous InGaN / GaN superlattice hole storage layer 700, an electron blocking layer 800, and a P-type semiconductor layer 900.
[0052] The present invention designs a porous InGaN / GaN superlattice electron storage layer 400 before the multi-quantum well light-emitting layer 600, and a porous InGaN / GaN superlattice hole storage layer 700 after the multi-quantum well light-emitting layer 600.
[0053] The specific structure of the porous InGaN / GaN superlattice electron reserve layer 400 is as follows:
[0054] In one embodiment, the porous InGaN / GaN superlattice electron reserve layer 400 includes alternating layers of undoped porous InGaN layers and a first undoped GaN layer, with the number of alternating growth cycles being 5 to 30; preferably, the number of alternating growth cycles of the undoped porous InGaN layers and the first undoped GaN layer is 10 to 25.
[0055] In one embodiment, the thickness of the undoped porous InGaN layer is 0.5 nm to 2 nm; exemplary thicknesses of the undoped porous InGaN layer are 0.7 nm, 0.9 nm, 1.1 nm, 1.3 nm, 1.5 nm, 1.7 nm, and 1.9 nm, but are not limited thereto.
[0056] In one embodiment, the thickness of the first undoped GaN layer is 1 nm to 5 nm; exemplary thicknesses of the first undoped GaN layer are 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited thereto.
[0057] In one embodiment, the thickness ratio of the undoped porous InGaN layer to the first undoped GaN layer is 1:(2-3); preferably, the thickness ratio of the undoped porous InGaN layer to the first undoped GaN layer is 1:2.5.
[0058] In one embodiment, the undoped porous InGaN layer is obtained by etching an InGaN layer. The etching process involves introducing H2 and NH3 gases at a gas treatment temperature of 800℃~950℃ and a pressure of 100 torr~500 torr, and etching the surface of the InGaN layer for 5s~50s to obtain the undoped porous InGaN layer. The porous InGaN layer is a porous structure formed by etching with H2 gas. After H2 gas treatment, materials with poor surface crystal quality are decomposed, which can effectively improve the quality of the epitaxial layer material. Simultaneously, the formation of an uneven porous structure can release the stress in the epitaxial layer, which is beneficial for the subsequent growth of a high-quality multi-quantum-well light-emitting layer.
[0059] The porous InGaN / GaN superlattice electron reserve layer can store some electrons, thereby blocking electrons and reducing their migration rate. This effectively improves the problem of electron-hole concentration mismatch in the active region and increases the electron-hole matching degree in the multi-quantum-well light-emitting layer, thus improving the luminous efficiency of InGaN-based blue LEDs or InGaN-based green LEDs.
[0060] The specific structure of the InGaN / GaN superlattice well pre-preparation layer 500 is as follows:
[0061] In one embodiment, the InGaN / GaN superlattice well preparation layer 500 includes alternating layers of undoped InGaN layers and Si-doped GaN layers, with the number of alternating growth cycles being 2 to 10; preferably, the number of alternating growth cycles of the undoped InGaN layers and Si-doped GaN layers is 3 to 9.
[0062] In one embodiment, the thickness of the undoped InGaN layer is 2.5 nm to 5 nm; exemplary thicknesses of the undoped InGaN layer are 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited thereto.
[0063] In one embodiment, the thickness of the Si-doped GaN layer is 7 nm to 16 nm; the exemplary thickness of the undoped InGaN layer is 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, or 15 nm, but is not limited thereto.
[0064] In one embodiment, the thickness ratio of the undoped InGaN layer to the Si-doped GaN layer is 1:(3-5); preferably, the thickness ratio of the undoped InGaN layer to the Si-doped GaN layer is 1:(3.5-4.5).
[0065] In one embodiment, the Si doping concentration of the Si-doped GaN layer is 5 × 10⁻⁶.17 atoms / cm 3 ~8×10 18 atoms / cm 3 Preferably, the Si doping concentration of the Si-doped GaN layer is 6 × 10⁻⁶. 17 atoms / cm 3 ~7×10 18 atoms / cm 3 .
[0066] The InGaN / GaN superlattice well preparation layer 500 can alleviate stress and block the propagation of dislocations caused by partial mismatch between the substrate and the epitaxial growth layer.
[0067] The specific structure of the porous InGaN / GaN superlattice hole reserve layer 700 is as follows:
[0068] In one embodiment, the porous InGaN / GaN superlattice hole reserve layer 700 includes alternating layers of Mg-doped porous InGaN layer and a second undoped GaN layer, with the number of alternating growth cycles being 5 to 30; preferably, the number of alternating growth cycles of the Mg-doped porous InGaN layer and the second undoped GaN layer is 10 to 25.
[0069] In one embodiment, the thickness of the Mg-doped porous InGaN layer is 0.5 nm to 2 nm; exemplary thicknesses of the Mg-doped porous InGaN layer are 0.7 nm, 0.9 nm, 1.1 nm, 1.3 nm, 1.5 nm, 1.7 nm, and 1.9 nm, but are not limited thereto.
[0070] In one embodiment, the thickness of the second undoped GaN layer is 1 nm to 5 nm; exemplary thicknesses of the second undoped GaN layer are 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited thereto.
[0071] In one embodiment, the thickness ratio of the Mg-doped porous InGaN layer to the second undoped GaN layer is 1:(2-3); preferably, the thickness ratio of the Mg-doped porous InGaN layer to the second undoped GaN layer is 1:2.5.
[0072] In one embodiment, the Mg doping concentration of the Mg-doped porous InGaN layer is 2 × 10⁻⁶. 18 atoms / cm 3 ~5×10 19 atoms / cm 3 Preferably, the Mg doping concentration of the Mg-doped porous InGaN layer is 3 × 10⁻⁶. 18atoms / cm 3 ~4×10 19 atoms / cm 3 .
[0073] In one embodiment, the Mg-doped porous InGaN layer is obtained by etching a Mg-doped InGaN layer. The etching process involves introducing H2 and NH3 gases at a gas treatment temperature of 800℃~950℃ and a pressure of 100 torr~500 torr, and etching the surface of the Mg-doped InGaN layer for 5s~50s to obtain the Mg-doped porous InGaN layer. The Mg-doped porous InGaN layer is a porous structure formed by etching with H2 gas. After H2 gas treatment, materials with poor surface crystal quality are decomposed, effectively improving the quality of the epitaxial layer material. Simultaneously, it forms an uneven, porous, rough surface, effectively reducing in-plane total internal reflection of the semiconductor material and significantly increasing the proportion of photon efferent material in the active region, thus improving the light extraction efficiency of the chip.
[0074] The porous InGaN / GaN superlattice hole reservoir layer can store some holes to improve the hole injection efficiency of the P-type semiconductor layer. At the same time, the Mg-doped porous InGaN layer is doped with Mg, which can also provide some hole concentration to the multi-quantum well light-emitting layer to compensate for the problem of insufficient hole concentration in the active region. In addition, it can also block electrons and reduce electron mobility to prevent electrons from being injected into the P-type semiconductor layer and causing electron leakage.
[0075] In one embodiment, the N-type semiconductor layer 200 is an N-type GaN layer with a thickness of 1 μm to 10 μm and a Si doping concentration of 5 × 10⁻⁶. 18 atoms / cm 3 ~2×10 20 atoms / cm 3 The growth temperature is 1050℃~1200℃, and the pressure is 50 torr~500 torr;
[0076] The stress relief layer 300 is a low-temperature GaN material with low Si doping, a thickness of 20 nm to 500 nm, and a Si doping concentration of 5 × 10⁻⁶. 17 atoms / cm 3 ~2×10 19 atoms / cm 3 The growth temperature is 800℃~950℃, and the pressure is 10 torr~300 torr;
[0077] The multi-quantum-well layer 600 comprises alternating stacked InGaN quantum well layers and GaN quantum barrier layers. The InGaN quantum well layers are made of InGaN material with an In composition of 0–0.4%, a thickness of 2.5 nm–5 nm, and are not intentionally doped. The growth temperature is 700 °C–850 °C, and the pressure is 20 torr–300 torr. The GaN quantum barrier layers are made of GaN material with a thickness of 7 nm–16 nm and a Si doping concentration of 5 × 10⁻⁶. 16 atoms / cm 3 ~2×10 18 atoms / cm 3 The growth temperature is 780℃~880℃, and the pressure is 20 torr~300 torr;
[0078] The electron blocking layer 800 is an AlGaN monolayer or multilayer structure doped with Mg, wherein the Al composition is 0.2-1, the thickness is 10 nm-200 nm, and the Mg concentration is 2 × 10⁻⁶. 18 atoms / cm 3 ~5×10 19 atoms / cm 3 The growth temperature is 820℃~1050℃, and the pressure is 10 torr~200 torr;
[0079] The P-type semiconductor layer 900 is an Al doped with Mg. x In y GaN single-layer or multi-layer structure; wherein the Al component is 0≤x≤0.2, the In component is 0≤y≤0.2, the thickness is 20nm~200nm, and the Mg concentration is 5×10 19 atoms / cm 3 ~2×10 21 atoms / cm 3 The growth temperature is 850℃~1050℃, and the pressure is 20 torr~300 torr.
[0080] Based on the above material design and fabrication process, the epitaxial wafer prepared using this invention can reduce the stress and defect density of the epitaxial layer material, improve the quality of the multi-quantum-well light-emitting layer material, and while effectively enhancing the injection of holes in the active region and improving the electron-hole matching degree in the quantum well, increase the light-emitting area of the platform quantum well required by the light-emitting diode, thereby improving the radiative recombination efficiency in the multi-quantum-well light-emitting layer and thus improving the luminous efficiency of the light-emitting diode.
[0081] Accordingly, the present invention provides a method for fabricating a light-emitting diode epitaxial wafer, such as... Figure 2 As shown, it includes the following steps:
[0082] S1. Prepare substrate 100;
[0083] S2. On the substrate 100, an N-type semiconductor layer 200, a stress relief layer 300, a porous InGaN / GaN superlattice electron storage layer 400, an InGaN / GaN superlattice well preparation layer 500, a multi-quantum well light-emitting layer 600, a porous InGaN / GaN superlattice hole storage layer 700, an electron blocking layer 800, and a P-type semiconductor layer 900 are deposited sequentially.
[0084] In one embodiment, the porous InGaN / GaN superlattice electron reserve layer 400 is prepared by the following method:
[0085] The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and In source were introduced to grow InGaN layer;
[0086] Then, the InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of InGaN layer is etched for 5s~50s to obtain an undoped porous InGaN layer.
[0087] The temperature of the reaction chamber is controlled at 800℃~900℃, the pressure is controlled at 20torr~300torr, and an N source and a Ga source are introduced. A first undoped GaN layer is deposited on the undoped porous InGaN layer, and the first undoped GaN layer fills the pores of the undoped porous InGaN layer.
[0088] The undoped porous InGaN layer and the first undoped GaN layer are alternately stacked to obtain the porous InGaN / GaN superlattice electron reserve layer.
[0089] In one embodiment, the InGaN / GaN superlattice well pre-preparation layer 500 is prepared by the following method:
[0090] The temperature of the reaction chamber was controlled at 760℃~850℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and In source were introduced to grow undoped InGaN layer.
[0091] The temperature of the reaction chamber is controlled at 780℃~880℃, the pressure is controlled at 20torr~300torr, and N source, Ga source and Si source are introduced to deposit a Si-doped GaN layer on the undoped InGaN layer.
[0092] The undoped InGaN layer and the Si-doped GaN layer are alternately stacked to obtain the pre-preparation layer for the InGaN / GaN superlattice well.
[0093] In one embodiment, the porous InGaN / GaN superlattice hole reservoir 700 is prepared by the following method:
[0094] The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow Mg-doped InGaN layer;
[0095] Then, the Mg-doped InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 5s~50s to obtain a Mg-doped porous InGaN layer.
[0096] The temperature of the reaction chamber is controlled at 800℃~900℃ and the pressure is controlled at 20 torr~300 torr. An N source and a Ga source are introduced to deposit a second undoped GaN layer on the Mg-doped porous InGaN layer. The second undoped GaN layer fills the pores of the Mg-doped porous InGaN layer.
[0097] The porous InGaN / GaN superlattice hole reserve layer is obtained by alternately stacking the Mg-doped porous InGaN layer and the second undoped GaN layer.
[0098] Accordingly, the present invention also provides an LED comprising the aforementioned InGaN-based light-emitting diode epitaxial wafer. The photoelectric efficiency of the LED is effectively improved, and other electrical properties are also excellent.
[0099] The present invention is further illustrated below with specific embodiments:
[0100] Example 1
[0101] This embodiment provides an InGaN-based light-emitting diode epitaxial wafer, including a substrate, on which are sequentially disposed an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum-well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer.
[0102] The porous InGaN / GaN superlattice electron reserve layer comprises alternating layers of undoped porous InGaN and a first undoped GaN layer, with 15 alternating growth cycles. The thickness of the undoped porous InGaN layer is 1 nm, and the thickness of the first undoped GaN layer is 2.5 nm. The undoped porous InGaN layer is obtained by etching the InGaN layer. The etching process is as follows: under a gas treatment temperature of 900℃ and a pressure of 300 torr, H2 gas and NH3 gas are introduced, and the surface of the InGaN layer is etched for 30 seconds to obtain the undoped porous InGaN layer.
[0103] The pre-well preparation layer for the InGaN / GaN superlattice comprises alternating layers of undoped InGaN and Si-doped GaN layers, with 6 alternating growth cycles. The thickness of the undoped InGaN layer is 3 nm, the thickness of the Si-doped GaN layer is 12 nm, and the Si doping concentration of the Si-doped GaN layer is 1 × 10⁻⁶. 18 atoms / cm 3 .
[0104] The porous InGaN / GaN superlattice hole reservoir comprises alternating layers of Mg-doped porous InGaN and a second undoped GaN layer, with 15 alternating growth cycles. The thickness of the Mg-doped porous InGaN layer is 1 nm, and the thickness of the second undoped GaN layer is 2.5 nm. The Mg doping concentration of the Mg-doped porous InGaN layer is 1 × 10⁻⁶. 19 atoms / cm 3 The Mg-doped porous InGaN layer is obtained by etching the Mg-doped InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 900℃ and pressure of 300 torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 30s to obtain the Mg-doped porous InGaN layer.
[0105] Example 2
[0106] This embodiment provides an InGaN-based light-emitting diode epitaxial wafer, including a substrate, on which are sequentially disposed an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum-well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer.
[0107] The porous InGaN / GaN superlattice electron reserve layer comprises alternating layers of undoped porous InGaN and a first undoped GaN layer, with 5 alternating growth cycles. The thickness of the undoped porous InGaN layer is 2 nm, and the thickness of the first undoped GaN layer is 4 nm. The undoped porous InGaN layer is obtained by etching the InGaN layer. The etching process is as follows: under a gas treatment temperature of 800℃ and a pressure of 100 torr, H2 gas and NH3 gas are introduced, and the surface of the InGaN layer is etched for 30 seconds to obtain the undoped porous InGaN layer.
[0108] The pre-well preparation layer for the InGaN / GaN superlattice comprises alternating layers of undoped InGaN and Si-doped GaN, with two alternating growth cycles. The thickness of the undoped InGaN layer is 5 nm, and the thickness of the Si-doped GaN layer is 15 nm. The Si doping concentration of the Si-doped GaN layer is 5 × 10⁻⁶. 17 atoms / cm 3 .
[0109] The porous InGaN / GaN superlattice hole reservoir comprises alternating layers of Mg-doped porous InGaN and a second undoped GaN layer, with 5 alternating growth cycles. The thickness of the Mg-doped porous InGaN layer is 2 nm, and the thickness of the second undoped GaN layer is 4 nm. The Mg doping concentration of the Mg-doped porous InGaN layer is 2 × 10⁻⁶. 18 atoms / cm 3 The Mg-doped porous InGaN layer is obtained by etching the Mg-doped InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 800℃ and pressure of 100 torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 30s to obtain the Mg-doped porous InGaN layer.
[0110] Example 3
[0111] This embodiment provides an InGaN-based light-emitting diode epitaxial wafer, including a substrate, on which are sequentially disposed an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum-well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer.
[0112] The porous InGaN / GaN superlattice electron reserve layer comprises alternating layers of undoped porous InGaN and a first undoped GaN layer, with 30 alternating growth cycles. The thickness of the undoped porous InGaN layer is 0.5 nm, and the thickness of the first undoped GaN layer is 1.5 nm. The undoped porous InGaN layer is obtained by etching the InGaN layer. The etching process is as follows: under a gas treatment temperature of 950°C and a pressure of 500 torr, H2 gas and NH3 gas are introduced, and the surface of the InGaN layer is etched for 30 seconds to obtain the undoped porous InGaN layer.
[0113] The pre-well preparation layer for the InGaN / GaN superlattice comprises alternating layers of undoped InGaN and Si-doped GaN, with 10 alternating growth cycles. The thickness of the undoped InGaN layer is 2.5 nm, the thickness of the Si-doped GaN layer is 7.5 nm, and the Si doping concentration of the Si-doped GaN layer is 8 × 10⁻⁶. 18 atoms / cm 3 .
[0114] The porous InGaN / GaN superlattice hole reservoir comprises alternating layers of Mg-doped porous InGaN and a second undoped GaN layer, with 30 alternating growth cycles. The thickness of the Mg-doped porous InGaN layer is 0.5 nm, and the thickness of the second undoped GaN layer is 1 nm. The Mg doping concentration of the Mg-doped porous InGaN layer is 5 × 10⁻⁶. 19 atoms / cm 3 The Mg-doped porous InGaN layer is obtained by etching the Mg-doped InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 950℃ and pressure of 500 torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 30s to obtain the Mg-doped porous InGaN layer.
[0115] Comparative Example 1
[0116] This comparative example provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is sequentially provided with an N-type semiconductor layer, a stress relief layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole reserve layer, an electron blocking layer, and a P-type semiconductor layer. It does not have a porous InGaN / GaN superlattice electron reserve layer. All other aspects are the same as in Example 1.
[0117] Comparative Example 2
[0118] This comparative example provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is sequentially provided with an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer. It does not have an InGaN / GaN superlattice well preparation layer. All other aspects are the same as in Example 1.
[0119] Comparative Example 3
[0120] This comparative example provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is provided with an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer in sequence. It does not have a porous InGaN / GaN superlattice hole storage layer. All other aspects are the same as in Example 1.
[0121] The light-emitting diode epitaxial wafers prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were fabricated into 3mil×5mil chips using the same chip process conditions. 300 LED chips were randomly selected from each example and tested at a current of 3mA. The luminous efficiency improvement rate of each example and comparative example was calculated. The specific test results are shown in Table 1.
[0122] Table 1. Performance test results of LEDs prepared in Examples 1-3 and Comparative Examples 1-3
[0123]
[0124] The results above show that the substrate sequentially comprises an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron reservoir layer, an InGaN / GaN superlattice pre-well preparation layer, a multi-quantum-well light-emitting layer, a porous InGaN / GaN superlattice hole reservoir layer, an electron blocking layer, and a P-type semiconductor layer. This invention designs a porous InGaN / GaN superlattice electron reservoir layer before the multi-quantum-well light-emitting layer and a porous InGaN / GaN superlattice hole reservoir layer after the multi-quantum-well light-emitting layer. XRD (002) data can characterize screw dislocations, and XRD (102) data can characterize mixed dislocations of screw and edge dislocations. Smaller XRD (002) or XRD (102) values indicate lower dislocation density and better crystal quality. The LED epitaxial wafer prepared using this invention can reduce the generation of defects in the epitaxial material during growth, lower the dislocation density of the material, significantly improve the quality of the epitaxial wafer material, improve the insufficient hole concentration in the active region, and increase the electron-hole matching degree in the multi-quantum-well light-emitting layer, thereby improving the radiative recombination efficiency in the active region of the light-emitting diode, i.e., the internal quantum efficiency. At the same time, it can significantly increase the proportion of photon efflux material in the active region, i.e., improve the light extraction efficiency of the chip.
[0125] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. An InGaN-based light-emitting diode epitaxial wafer, characterized in that, The substrate includes an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer, which are sequentially disposed on the substrate. The InGaN / GaN superlattice well preparation layer includes alternating layers of undoped InGaN and Si-doped GaN layers, with the number of alternating growth cycles being 2 to 10. The thickness of the undoped InGaN layer is 2.5 nm to 5 nm; The thickness of the Si-doped GaN layer is 7 nm to 16 nm. The thickness ratio of the undoped InGaN layer to the Si-doped GaN layer is 1:(3~5). The Si doping concentration of the Si-doped GaN layer is 5 × 10⁻⁶. 17 atoms / cm 3 ~8×10 18 atoms / cm 3 ; The porous InGaN / GaN superlattice hole reservoir consists of alternating layers of Mg-doped porous InGaN and a second undoped GaN layer, with the number of alternating growth cycles being 5 to 30. The thickness of the Mg-doped porous InGaN layer is 0.5 nm to 2 nm; The thickness of the second undoped GaN layer is 1 nm to 5 nm; The thickness ratio of the Mg-doped porous InGaN layer to the second undoped GaN layer is 1:(2~3). The Mg doping concentration of the Mg-doped porous InGaN layer is 2 × 10⁻⁶. 18 atoms / cm 3 ~5×10 19 atoms / cm 3 .
2. The InGaN-based light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The porous InGaN / GaN superlattice electron reserve layer comprises alternating layers of undoped porous InGaN and a first undoped GaN layer, with the number of alternating growth cycles being 5 to 30. The thickness of the undoped porous InGaN layer is 0.5 nm to 2 nm; The thickness of the first undoped GaN layer is 1 nm to 5 nm; The thickness ratio of the undoped porous InGaN layer to the first undoped GaN layer is 1:(2~3).
3. The InGaN-based light-emitting diode epitaxial wafer as described in claim 2, characterized in that, The undoped porous InGaN layer is obtained by etching an InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the InGaN layer is etched for 5s~50s to obtain an undoped porous InGaN layer.
4. The InGaN-based light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Mg-doped porous InGaN layer is obtained by etching the Mg-doped InGaN layer. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 5s~50s to obtain the Mg-doped porous InGaN layer.
5. A method for fabricating an InGaN-based light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Prepare the substrate; S2. Sequentially deposit an N-type semiconductor layer, a stress relief layer, a porous InGaN / GaN superlattice electron storage layer, an InGaN / GaN superlattice well preparation layer, a multi-quantum well light-emitting layer, a porous InGaN / GaN superlattice hole storage layer, an electron blocking layer, and a P-type semiconductor layer on the substrate.
6. The method for fabricating an InGaN-based light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The porous InGaN / GaN superlattice electron reserve layer was prepared by the following method: The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source and In source were introduced to grow InGaN layer; Then, the InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100torr~500torr, H2 gas and NH3 gas are introduced and the surface of the InGaN layer is etched for 5s~50s to obtain an undoped porous InGaN layer. The temperature of the reaction chamber is controlled at 800℃~900℃ and the pressure is controlled at 20 torr~300 torr. An N source and a Ga source are introduced to deposit a first undoped GaN layer on the undoped porous InGaN layer. The first undoped GaN layer fills the pores of the undoped porous InGaN layer. The undoped porous InGaN layer and the first undoped GaN layer are alternately stacked to obtain the porous InGaN / GaN superlattice electron reserve layer.
7. The method for fabricating an InGaN-based light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The porous InGaN / GaN superlattice hole reserve layer was prepared by the following method: The temperature of the reaction chamber was controlled at 780℃~880℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow Mg-doped InGaN layer; Then, the Mg-doped InGaN layer is etched. The etching process is as follows: under the conditions of gas treatment temperature of 800℃~950℃ and pressure of 100 torr~500 torr, H2 gas and NH3 gas are introduced and the surface of the Mg-doped InGaN layer is etched for 5s~50s to obtain a Mg-doped porous InGaN layer. The temperature of the reaction chamber is controlled at 800℃~900℃ and the pressure is controlled at 20 torr~300 torr. An N source and a Ga source are introduced to deposit a second undoped GaN layer on the Mg-doped porous InGaN layer. The second undoped GaN layer fills the pores of the Mg-doped porous InGaN layer. The porous InGaN / GaN superlattice hole reserve layer is obtained by alternately stacking the Mg-doped porous InGaN layer and the second undoped GaN layer.
8. An LED, characterized in that, The LED comprises an InGaN-based light-emitting diode epitaxial wafer as described in any one of claims 1 to 4.
Citation Information
Patent Citations
Light-emitting diode epitaxial wafer, preparation method thereof and LED
CN116799118A
Propagation of misfit dislocations from buffer / si interface into si
US20100046567A1