Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode
By employing a porous AlN and AlGaN layer stack structure and roughening treatment in the epitaxial wafer of a light-emitting diode (LED), stress is released, dislocation density is reduced, lattice mismatch and thermal mismatch problems are solved, and the luminous efficiency and brightness of the LED are improved.
Patent Information
- Application Number
- CN202311243177.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing light-emitting diodes suffer from high stress due to lattice mismatch and thermal mismatch between heterogeneous substrates and epitaxial materials, leading to dislocation defects and reduced luminous efficiency.
A porous AlN layer and a porous AlGaN layer stack structure are adopted. By roughening the porous AlGaN layer with H₂ and/or NH₃, a rough surface is formed, which induces stress relief pores in the Si-doped porous GaN layer. These pores are then filled by an undoped GaN layer. Combined with the periodic structure of InGaN and low-doped N-GaN layers, stress is released and dislocation density is reduced.
It effectively releases the stress of epitaxial materials, improves the quality of epitaxial layer materials, reduces defects, and enhances the luminous efficiency and brightness of light-emitting diodes.
Smart Images

Figure CN117276431B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology
[0002] Currently, all LEDs used in the market are fabricated using heterogeneous substrate epitaxy. Due to the significant lattice and thermal mismatch between the heterogeneous substrate (including sapphire, silicon carbide, and silicon substrates) and the epitaxial material, the epitaxial material is subjected to considerable stress during growth, making it prone to dislocation formation and defects, thus reducing the luminous efficiency of the LED. Therefore, to improve the luminous efficiency of LEDs, it is essential to improve the quality of the epitaxial material by optimizing the epitaxial structure and process. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode.
[0004] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.
[0005] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate, and a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer sequentially stacked on the substrate; the buffer layer comprises a porous AlN layer and a porous AlGaN layer sequentially stacked on the substrate; the N-type semiconductor layer comprises a Si-doped porous GaN layer, an undoped GaN layer, and a heavily doped N-type GaN layer sequentially stacked on the buffer layer;
[0006] The porous AlN layer has multiple V-shaped holes that extend to the substrate, and the V-shaped holes extend to the Si-doped porous GaN layer and are filled by the undoped GaN layer.
[0007] The porous AlGaN layer is roughened by H2 and / or NH3 to form a rough surface, thereby inducing the Si-doped porous GaN layer to generate multiple stress-relieving pores, which are then filled by the undoped GaN layer.
[0008] As an improvement to the above technical solution, the distribution density of the V-shaped holes is 2×10⁻⁶. 8 cm -2 ~5×10 11 cm -2 The distribution density of the stress relief holes is 2×10⁻⁶. 8 cm -2 ~5×10 12 cm-2 .
[0009] As an improvement to the above technical solution, the thickness of the porous AlN layer is 1nm to 20nm;
[0010] The thickness of the porous AlGaN layer is 50 nm to 500 nm, and the Al content is 0.05 to 0.6%.
[0011] As an improvement to the above technical solution, the thickness of the Si-doped porous GaN layer is 10 nm to 500 nm, and its Si doping concentration is 5 × 10⁻⁶. 16 cm -3 ~2×10 18 cm -3 ;
[0012] The thickness of the undoped GaN layer is 0.2 μm to 2 μm;
[0013] The N-type dopant element in the heavily doped N-type GaN layer is Si, and the doping concentration is 3 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 Its thickness is 2μm to 8μm.
[0014] As an improvement to the above technical solution, the porous AlN layer is doped with Mg at a concentration of 2 × 10⁻⁶. 15 cm -3 ~5×10 18 cm -3 .
[0015] As an improvement to the above technical solution, H2 is used to roughen the porous AlGaN layer. The roughening temperature is 950℃~1250℃, the pressure is 100torr~500torr, and the time is 2min~5min.
[0016] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:
[0017] A substrate is provided on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer are sequentially grown. The buffer layer comprises a porous AlN layer and a porous AlGaN layer sequentially stacked on the substrate. The N-type semiconductor layer comprises a Si-doped porous GaN layer, an undoped GaN layer, and a heavily doped N-type GaN layer sequentially stacked on the buffer layer.
[0018] The porous AlN layer has multiple V-shaped holes that extend to the substrate, and the V-shaped holes extend to the Si-doped porous GaN layer and are filled by the undoped GaN layer.
[0019] The porous AlGaN layer is roughened by H2 and / or NH3 to form a rough surface, thereby inducing the Si-doped porous GaN layer to generate multiple stress-relieving pores, which are then filled by the undoped GaN layer.
[0020] As an improvement to the above technical solution, the growth temperature of the porous AlN layer is 800℃~1050℃, and the growth pressure is 50 torr~200 torr;
[0021] The growth temperature of the porous AlGaN layer is 1050℃~1250℃, and the growth pressure is 150 torr~500 torr.
[0022] As an improvement to the above technical solution, the growth temperature of the Si-doped porous GaN layer is 950℃~1150℃, and the growth pressure is 100 torr~300 torr;
[0023] The growth temperature of the undoped GaN layer is 1100℃~1250℃, and the growth pressure is 10 torr~300 torr.
[0024] The growth temperature of the heavily doped N-type GaN layer is 1100℃~1250℃, and the growth pressure is 10 torr~300 torr.
[0025] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.
[0026] Implementing this invention has the following beneficial effects:
[0027] The buffer layer in the epitaxial wafer of the light-emitting diode of the present invention is a stacked structure formed by a porous AlN layer and a porous AlGaN layer, and it is provided with multiple V-shaped holes penetrating to the substrate. The N-type semiconductor layer includes a Si-doped porous GaN layer, an undoped GaN layer, and a heavily doped N-type GaN layer stacked sequentially. Firstly, this buffer layer is beneficial for fully releasing the stress of the epitaxial layer material, which can effectively reduce the defects caused by large stress on the subsequent epitaxial layer material, thereby improving the quality of the epitaxial layer material. Secondly, the roughened surface of the porous AlGaN layer formed by H2 and / or NH3 induces multiple stress-relieving holes in the subsequently grown Si-doped porous GaN layer, further fully releasing the stress of the epitaxial layer material, thereby improving the quality of the epitaxial layer material. At the same time, the treatment of the porous AlGaN layer also decomposes the material with poor surface crystal quality, which is beneficial for improving the crystal quality of the subsequently deposited epitaxial material. Thirdly, the undoped GaN layer is a merging layer, completely filling the V-shaped holes and stress-relieving holes. During the merging process of the V-shaped holes and stress-relieving holes, some dislocation defects will continuously deflect and merge, reducing the dislocation density of the epitaxial layer material, thereby improving the quality of the epitaxial material. In summary, the LED epitaxial wafer prepared using this invention can effectively release the mismatch stress caused by lattice mismatch and thermal mismatch between the sublayers of the epitaxial material, reduce the generation of defects in the epitaxial material during growth, reduce the dislocation density of the material, significantly improve the quality of the epitaxial wafer material, and thus improve the yield and brightness performance of the LED. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;
[0029] Figure 2 This is a schematic diagram of the structure of the buffer layer and the N-type semiconductor layer in one embodiment of the present invention;
[0030] Figure 3 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0032] refer to Figure 1 and Figure 2This invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 100, a buffer layer 200, an N-type semiconductor layer 300, a stress-relieving layer 400, a multiple quantum well layer 500, an electron blocking layer 600, and a P-type semiconductor layer 700 sequentially stacked on the substrate 100; wherein, the buffer layer 200 comprises a porous AlN layer 201 and a porous AlGaN layer 202 sequentially stacked on the substrate 100. The porous AlN layer 201 has a plurality of V-shaped holes 800 of substantially the same size and uniformly distributed.
[0033] The thickness of the porous AlN layer 201 is 1 nm to 20 nm, with exemplary thicknesses of 2 nm, 5 nm, 8 nm, 12 nm, 15 nm, or 18 nm, but not limited thereto. A preferred thickness is 5 nm to 15 nm. The distribution density of the V-shaped pores 800 is 2 × 10⁻⁶. 8 cm -2 ~5×10 11 cm -2 An example is 4×10 8 cm -2 9×10 8 cm -2 3×10 9 cm -2 2×10 10 cm -2 8×10 10 cm -2 Or 3×10 11 cm -2 However, it is not limited to this. A preferred value is 5×10. 9 cm -2 ~5×10 10 cm -2 .
[0034] Preferably, in one embodiment of the present invention, the porous AlN layer 201 is doped with Mg at a doping concentration of 2 × 10⁻⁶. 15 cm -3 ~5×10 18 cm -3 Based on this setting, the size and distribution uniformity of the V-holes 800 can be optimized, thus better releasing stress.
[0035] The porous AlGaN layer 202 inherits the V-shaped hole 800 structure of the porous AlN layer 201, effectively releasing thermal stress and stress caused by lattice mismatch. Specifically, the thickness of the porous AlGaN layer 202 is 50nm to 500nm. If its thickness is <50nm, there will be virtually no remaining porous AlGaN layer 202 after subsequent roughening treatment. If its thickness is >500nm, it will partially fill the V-shaped holes 800, which is not conducive to fully releasing stress. For example, the thickness of the porous AlGaN layer 202 is 80nm, 120nm, 230nm, 340nm, or 450nm, but is not limited to these. Preferably, it is 100nm to 300nm. In addition, Al is introduced into the porous AlGaN layer 202, which helps to reduce the lattice mismatch between the porous AlN layer 201 and the subsequent N-type semiconductor layer 300. Specifically, the proportion of Al component in the porous AlGaN layer 202 is 0.05 to 0.6%, with exemplary values of 0.1, 0.23, 0.24, 0.33, 0.37, or 0.44, but not limited thereto. Preferably, it is 0.35 to 0.45.
[0036] After the porous AlGaN layer 202 is grown, it undergoes roughening treatment with H2 and / or NH3 to form a rough surface. Specifically, the roughening treatment temperature is 950℃~1250℃, the pressure is 100torr~500torr, and the time is 2min~5min. Based on these conditions, the formation of subsequent stress-relieving pores can be better induced.
[0037] The N-type semiconductor layer 300 comprises a Si-doped porous GaN layer 301, an undoped GaN layer 302, and a heavily doped N-type GaN layer 303 sequentially stacked on the buffer layer 200. The Si-doped porous GaN layer 301 not only inherits the V-shaped holes 800, but also, due to the rough surface of the porous AlGaN layer 202, forms multiple stress-relieving holes 900 of essentially the same size and uniformly distributed, further effectively releasing stress. The undoped GaN layer 302 fills and merges the V-shaped holes 800 and the stress-relieving holes 900, causing dislocation defects to continuously segregate and merge, thereby significantly reducing the dislocation density.
[0038] The thickness of the Si-doped porous GaN layer 301 is 10 nm to 500 nm, with exemplary thicknesses of 40 nm, 100 nm, 180 nm, 320 nm, or 440 nm, and preferably 20 nm to 150 nm. The Si doping concentration in the Si-doped porous GaN layer 301 is 5 × 10⁻⁶. 16 cm -3 ~2×10 18 cm -3 The preferred value is 5×10 16 cm -3 ~5×10 17 cm-3 .
[0039] The distribution density of the stress relief holes 900 is 2×10⁻⁶. 8 cm -2 ~5×10 12 cm -2 An example is 5×10 8 cm -2 4×10 9 cm -2 5×10 10 cm -2 6×10 11 cm -2 Or 3×10 12 cm -2 However, it is not limited to this. A preferred value is 1×10. 10 cm -2 ~3×10 12 cm -2 .
[0040] The undoped GaN layer 302 has a thickness of 0.2 μm to 2 μm. Based on this thickness range, the V-shaped holes 800 and stress-relieving holes 900 can be effectively filled, reducing dislocation density. For example, the thickness of the undoped GaN layer 302 can be 0.5 μm, 0.9 μm, 1.3 μm, or 1.7 μm, but is not limited to these. Preferably, it is 1 μm to 2 μm.
[0041] In the heavily doped N-type GaN layer 303, the N-type dopant element is Si, and the doping concentration is 3×10⁻⁶. 18 cm -3 ~5×10 19 cm -3 An example is 5×10 18 cm -3 3×10 18 cm -3 1×10 19 cm -3 Or 3×10 19 cm -3 However, it is not limited to this. The thickness of the heavily doped N-type GaN layer 303 is 2 μm to 8 μm, with exemplary thicknesses of 2.6 μm, 3.2 μm, 3.8 μm, 4.5 μm, 6 μm, or 7.2 μm, but not limited to this. Preferably, it is 3 μm to 5 μm.
[0042] The substrate 100 is a sapphire substrate, a silicon substrate, or a silicon carbide substrate, but is not limited to these. A sapphire substrate is preferred.
[0043] Among them, the stress relief layer 400 is made of In a Ga 1-aThe periodic structure obtained by overlapping N-layers (a = 0.1–0.2) and low-doped N-GaN layers has a period number of 3–10. Among them, a single In... a Ga 1-a The thickness of the N-layer is 2nm to 5nm, with exemplary thicknesses of 2.4nm, 2.8nm, 3.2nm, 3.6nm, 4nm, 4.4nm, or 4.8nm, but not limited thereto. The thickness of a single low-doped N-GaN layer is 5nm to 10nm, with exemplary thicknesses of 6nm, 7nm, 8nm, or 9nm, but not limited thereto. The doping element of the low-doped N-GaN layer is Si or Ge, but not limited thereto, with Si being preferred. The doping concentration of the low-doped N-GaN layer is 1×10⁻⁶. 17 cm -3 ~1×10 18 cm -3 An example is 2×10 17 cm -3 4×10 17 cm -3 6×10 17 cm -3 8×10 17 cm -3 Or 9×10 17 cm -3 However, it is not limited to this.
[0044] The multi-quantum-well layer 500 has a periodic structure with 3 to 15 periods. Each period includes sequentially stacked InGaN quantum well layers and GaN quantum barrier layers. The thickness of a single InGaN quantum well layer is 2 nm to 5 nm, and its In content is 0.12 to 0.25%. The thickness of a single GaN quantum barrier layer is 6 nm to 15 nm.
[0045] The electron blocking layer 600 is an AlGaN layer or an InAlGaN layer, but is not limited to these. Preferably, it is an AlGaN layer. The thickness of the electron blocking layer 600 is 30nm to 100nm, and exemplary thicknesses are 40nm, 50nm, 60nm, 70nm, 80nm, or 90nm, but are not limited to these.
[0046] Among them, the P-type semiconductor layer 700 is a P-type GaN layer, and its P-type doping element is Mg, but it is not limited to this. The P-type doping concentration in the P-type GaN layer 700 is 1×10⁻⁶. 19 cm -3 ~1×10 21 cm -3 The thickness of the p-type GaN layer 700 is 100nm to 500nm, with examples of 140nm, 220nm, 240nm, 300nm, 400nm or 450nm, but not limited to these.
[0047] Accordingly, refer to Figure 3 The present invention also provides a method for preparing a light-emitting diode epitaxial wafer, which specifically includes the following steps:
[0048] S1: Provides a substrate;
[0049] S2: A buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer are sequentially grown on the substrate;
[0050] Specifically, step S2 includes:
[0051] S21: Growing a porous AlN layer on a substrate;
[0052] Among them, porous AlN layers are grown by MOCVD at a growth temperature of 800℃~1050℃ and a growth pressure of 50 torr~200 torr.
[0053] S22: A porous AlGaN layer is grown on a porous AlN layer to obtain a buffer layer;
[0054] Among them, porous AlGaN layers are grown by MOCVD at a growth temperature of 1050℃~1250℃ and a growth pressure of 150 torr~500 torr.
[0055] Specifically, after growth, a roughening treatment is performed under an H2 and / or NH3 atmosphere to form a rough surface. Specifically, the roughening treatment temperature is 950℃~1250℃, the pressure is 100torr~500torr, and the time is 2min~5min.
[0056] S23: Growing a Si-doped porous GaN layer on the buffer layer;
[0057] Among them, Si-doped porous GaN layers are grown by MOCVD at a growth temperature of 950℃~1150℃ and a growth pressure of 100 torr~300 torr.
[0058] S24: Growing an undoped GaN layer on a Si-doped porous GaN layer;
[0059] Among them, undoped GaN layers are grown by MOCVD at a growth temperature of 1100℃~1250℃ and a growth pressure of 10 torr~300 torr.
[0060] S25: Grow a heavily doped N-type GaN layer on an undoped GaN layer to obtain an N-type semiconductor layer;
[0061] Among them, the heavily doped N-type GaN layer is grown by MOCVD at a growth temperature of 1100℃~1250℃ and a growth pressure of 10 torr~300 torr.
[0062] S26: Growing a stress-relieving layer on an N-type semiconductor layer;
[0063] In particular, periodic growth of In in MOCVD a Ga 1-a N-layers and lightly doped N-GaN layers are then applied until a stress-relieving layer is obtained. In... a Ga 1-a The growth temperature of the N-layer is 750℃~850℃, and the growth pressure is 100 torr~200 torr. The growth temperature of the low-doped N-GaN layer is 850℃~900℃, and the growth pressure is 100 torr~200 torr.
[0064] S27: Growth of multiple quantum well layers on stress relief layers;
[0065] In this process, InGaN quantum well layers and GaN quantum barrier layers are periodically grown using MOCVD until a multi-quantum well layer is obtained. The growth temperature of the InGaN quantum well layer is 750℃–800℃, and the growth pressure is 100 torr–500 torr. The growth temperature of the GaN quantum barrier layer is 850℃–900℃, and the growth pressure is 100 torr–500 torr.
[0066] S28: An electron blocking layer is grown on a multi-quantum-well layer;
[0067] In one embodiment of the present invention, an AlGaN layer is grown by MOCVD as an electron blocking layer at a growth temperature of 1000℃~1100℃ and a growth pressure of 100 torr~300 torr.
[0068] S29: Grow a P-type semiconductor layer on the electron blocking layer;
[0069] In one embodiment of the present invention, a P-type GaN layer is grown by MOCVD as a P-type semiconductor layer, with a growth temperature of 900°C to 1000°C and a growth pressure of 100 torr to 300 torr.
[0070] The present invention will be further described below with reference to specific embodiments:
[0071] Example 1
[0072] refer to Figure 1 and Figure 2This embodiment provides a light-emitting diode epitaxial wafer, which includes a substrate 100, and a buffer layer 200, an N-type semiconductor layer 300, a stress relief layer 400, a multiple quantum well layer 500, an electron blocking layer 600 and a P-type semiconductor layer 700 sequentially stacked on the substrate 100.
[0073] The substrate 1 is a sapphire substrate. The buffer layer 200 includes a porous AlN layer 201 and a porous AlGaN layer 202 sequentially stacked on the substrate 100; the porous AlN layer 201 has multiple V-shaped holes 800 penetrating into the substrate 100; the thickness of the porous AlN layer 201 is 18 nm, and the distribution density of the V-shaped holes 800 is 4 × 10⁻⁶. 8 cm -2 The porous AlGaN layer 202 has a thickness of 450 nm and an Al content of 0.5%. The porous AlGaN layer is roughened by H2 to form a rough surface.
[0074] The N-type semiconductor layer 300 includes a Si-doped porous GaN layer 301, an undoped GaN layer 302, and a heavily doped N-type GaN layer 303 sequentially stacked on the buffer layer 200. Multiple stress-relieving holes 900 are formed on the Si-doped porous GaN layer 301. The thickness of the Si-doped porous GaN layer 301 is 210 nm, and the Si doping concentration is 1 × 10⁻⁶. 18 cm -3 The distribution density of stress relief holes 900 is 3 × 10⁻⁶. 9 cm -2 The thickness of the undoped GaN layer 302 is 0.8 μm. The Si doping concentration in the heavily doped N-type GaN layer 303 is 4 × 10⁻⁶. 19 cm -3 Its thickness is 6μm.
[0075] Among them, the stress relief layer 400 is made of In a Ga 1-a The periodic structure obtained by overlapping N-layers (a = 0.11) and low-doped N-GaN layers has a period number of 8. Among them, a single In... a Ga 1-a The thickness of the N-layer is 2.5 nm, and the thickness of a single low-doped N-GaN layer is 9 nm, with a Si doping concentration of 8 × 10⁻⁶. 17 cm -3 .
[0076] The multi-quantum-well layer 500 has a periodic structure with 10 periods. Each period consists of sequentially stacked InGaN quantum well layers and GaN quantum barrier layers. The InGaN quantum well layers are 3 nm thick with an In content of 0.2%. The GaN quantum barrier layers are 10 nm thick.
[0077] Among them, the electron blocking layer 600 is an AlGaN layer with a thickness of 65nm.
[0078] The P-type semiconductor layer is a P-type GaN layer with a Mg doping concentration of 3 × 10⁻⁶. 20 cm -3 Its thickness is 220nm.
[0079] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:
[0080] (1) Provide a substrate.
[0081] (2) Grow a buffer layer on the substrate;
[0082] Among them, porous AlN layers were grown by MOCVD at a growth temperature of 950℃ and a growth pressure of 100 torr.
[0083] (3) A porous AlGaN layer is grown on the porous AlN layer to obtain a buffer layer;
[0084] Among them, porous AlGaN layers were grown by MOCVD at a growth temperature of 1150℃ and a growth pressure of 400 torr.
[0085] Specifically, after growth, a roughening treatment is performed under an H2 atmosphere to form a rough surface. Specifically, the roughening treatment temperature is 1200℃, the pressure is 300 torr, and the time is 4 minutes.
[0086] (4) A Si-doped porous GaN layer is grown on the buffer layer;
[0087] Among them, Si-doped porous GaN layers were grown by MOCVD at a growth temperature of 1050℃ and a growth pressure of 200 torr.
[0088] (5) Growing an undoped GaN layer on a Si-doped porous GaN layer;
[0089] Among them, undoped GaN layers were grown by MOCVD at a growth temperature of 1100℃ and a growth pressure of 50 torr.
[0090] (6) A heavily doped N-type GaN layer is grown on an undoped GaN layer to obtain an N-type semiconductor layer;
[0091] Among them, a heavily doped N-type GaN layer was grown by MOCVD at a growth temperature of 1220℃ and a growth pressure of 200 torr.
[0092] (7) A stress-relieving layer is grown on the N-type semiconductor layer;
[0093] In particular, periodic growth of In in MOCVDa Ga 1-a N-layers and lightly doped N-GaN layers are then applied until a stress-relieving layer is obtained. In... a Ga 1-a The growth temperature of the N-layer is 760℃, and the growth pressure is 140 torr. The growth temperature of the low-doped N-GaN layer is 860℃, and the growth pressure is 140 torr.
[0094] (8) Grow a multi-quantum well layer on the stress relief layer;
[0095] In this process, InGaN quantum well layers and GaN quantum barrier layers are periodically grown using MOCVD until a multi-quantum well layer is obtained. The InGaN quantum well layer is grown at a temperature of 780℃ and a growth pressure of 200 torr. The GaN quantum barrier layer is grown at a temperature of 870℃ and a growth pressure of 200 torr.
[0096] (9) An electron blocking layer on a multi-quantum-well layer;
[0097] In this method, an AlGaN layer was grown using MOCVD as an electron blocking layer. The growth temperature of the electron blocking layer was 1050℃, and the growth pressure was 200 torr.
[0098] (10) Grow a P-type semiconductor layer on the electron blocking layer;
[0099] Among them, a P-type GaN layer was grown by MOCVD as a P-type semiconductor layer at a growth temperature of 950℃ and a growth pressure of 200 torr.
[0100] Example 2
[0101] refer to Figure 1 and Figure 2 This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the thickness of the porous AlN layer 201 is 10 nm, and the distribution density of the V-shaped holes 800 is 8 × 10⁻⁶. 9 cm -2 The porous AlGaN layer 202 has a thickness of 220 nm and an Al content of 0.4%. The porous AlGaN layer is roughened with H2 to form a rough surface. The distribution density of stress-relieving pores 900 is 9 × 10⁻⁶. 9 cm -2 .
[0102] Everything else is the same as in Example 1.
[0103] Example 3
[0104] refer to Figure 1 and Figure 2This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that the thickness of the Si-doped porous GaN layer 301 is 120 nm, and the Si doping concentration is 3 × 10⁻⁶. 17 cm -3 The distribution density of stress relief holes 900 is 4 × 10⁻⁶. 10 cm -2 The thickness of the undoped GaN layer 302 is 1.5 μm. The thickness of the heavily doped N-type GaN layer 303 is 4.2 μm.
[0105] Everything else is the same as in Example 2.
[0106] Example 4
[0107] refer to Figure 1 and Figure 2 This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that the porous AlN layer 201 is doped with Mg, and the doping concentration is 4 × 10⁻⁶. 16 cm -3 .
[0108] Comparative Example 1
[0109] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the buffer layer 200 is an AlN layer with a thickness of 50 nm and does not have V-shaped holes. It is fabricated by PVD.
[0110] The N-type semiconductor layer 300 does not include a Si-doped porous GaN layer.
[0111] Everything else is the same as in Example 1.
[0112] The luminous intensity of the epitaxial wafers obtained in Examples 1 to 4 and Comparative Example 1 was tested. Based on the data from Comparative Example 1, the improvement rate of luminous intensity was calculated, and the specific results are shown in the table below.
[0113] Brightness improvement rate (%) Example 1 5.8 Example 2 6.3 Example 3 8.6 Example 4 8.9
[0114] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light-emitting diode epitaxial wafer, characterized in that, The device includes a substrate, and a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer sequentially stacked on the substrate; the buffer layer includes a porous AlN layer and a porous AlGaN layer sequentially stacked on the substrate; the N-type semiconductor layer includes a Si-doped porous GaN layer, an undoped GaN layer, and a heavily doped N-type GaN layer sequentially stacked on the buffer layer; The porous AlN layer has multiple V-shaped holes that extend to the substrate, and the V-shaped holes extend to the Si-doped porous GaN layer and are filled by the undoped GaN layer. The porous AlGaN layer is roughened by H2 and / or NH3 to form a rough surface, thereby inducing the Si-doped porous GaN layer to generate multiple stress-relieving pores, which are then filled by the undoped GaN layer. The thickness of the Si-doped porous GaN layer is 10 nm to 500 nm, and its Si doping concentration is 5 × 10⁻⁶. 16 cm -3 ~2×10 18 cm -3 ; The thickness of the undoped GaN layer is 0.2 μm to 2 μm; The N-type dopant element in the heavily doped N-type GaN layer is Si, and the doping concentration is 3 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 Its thickness is 2μm~8μm.
2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The distribution density of the V-shaped holes is 2×10⁻⁶. 8 cm -2 ~5×10 11 cm -2 The distribution density of the stress relief holes is 2×10⁻⁶. 8 cm -2 ~5×10 12 cm -2 .
3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the porous AlN layer is 1 nm to 20 nm. The thickness of the porous AlGaN layer is 50nm~500nm, and its Al composition ratio is 0.05~0.6%.
4. The light-emitting diode epitaxial wafer as described in any one of claims 1 to 3, characterized in that, The porous AlN layer is doped with Mg at a concentration of 2 × 10⁻⁶. 15 cm -3 ~5×10 18 cm -3 .
5. The light-emitting diode epitaxial wafer as described in any one of claims 1 to 3, characterized in that, The porous AlGaN layer was roughened using H2 at a temperature of 950℃ to 1250℃, a pressure of 100 torr to 500 torr, and a time of 2 min to 5 min.
6. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1 to 5, characterized in that, include: A substrate is provided on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer are sequentially grown. The buffer layer comprises a porous AlN layer and a porous AlGaN layer sequentially stacked on the substrate. The N-type semiconductor layer comprises a Si-doped porous GaN layer, an undoped GaN layer, and a heavily doped N-type GaN layer sequentially stacked on the buffer layer. The porous AlN layer has multiple V-shaped holes that extend to the substrate, and the V-shaped holes extend to the Si-doped porous GaN layer and are filled by the undoped GaN layer. The porous AlGaN layer is roughened by H2 and / or NH3 to form a rough surface, thereby inducing the Si-doped porous GaN layer to generate multiple stress-relieving pores, which are then filled by the undoped GaN layer. The thickness of the Si-doped porous GaN layer is 10 nm to 500 nm, and its Si doping concentration is 5 × 10⁻⁶. 16 cm -3 ~2×10 18 cm -3 ; The thickness of the undoped GaN layer is 0.2 μm to 2 μm; The N-type dopant element in the heavily doped N-type GaN layer is Si, and the doping concentration is 3 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 Its thickness is 2μm~8μm.
7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the porous AlN layer is 800℃~1050℃, and the growth pressure is 50 torr~200 torr. The growth temperature of the porous AlGaN layer is 1050℃~1250℃, and the growth pressure is 150 torr~500 torr.
8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the Si-doped porous GaN layer is 950℃~1150℃, and the growth pressure is 100 torr~300 torr. The growth temperature of the undoped GaN layer is 1100℃~1250℃, and the growth pressure is 10 torr~300 torr. The growth temperature of the heavily doped N-type GaN layer is 1100℃~1250℃, and the growth pressure is 10 torr~300 torr.
9. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Preparation method for semiconductor light-emitting device
CN104795472A
Nitride semiconductor laser element
JP2000049415A