Polypropylene separator and preparation method and application thereof
By modifying the polypropylene separator, the thermal stability and polar affinity issues of polyolefin separators are solved by using chemical bonds and electrostatic attraction formed by aramid and inorganic particles, thereby improving the safety and mechanical strength of the battery.
Patent Information
- Application Number
- CN202311222935.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing polyolefin separators have poor thermal dimensional stability, low polarity leading to poor affinity with electrolytes, posing a high-temperature safety hazard and being easily punctured by the electrode sheets.
A polypropylene separator modified with aramid and inorganic particles is used. By mixing acid-modified short aramid fibers with an inorganic particle suspension, chemical bonds are formed. Combined with electrostatic attraction and the positively charged polypropylene surface, the high temperature resistance and polar affinity of the separator are improved.
It improves the thermal stability and mechanical strength of the separator, enhances its affinity with the electrolyte, reduces the safety hazards of the battery at high temperatures, and improves the tensile properties and puncture strength of the separator.
Smart Images

Figure CN117276802B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery separator technology, and in particular to a polypropylene separator, its preparation method, and its application. Background Technology
[0002] Battery safety depends on the electrodes, electrolyte, separator material, battery structure, and protection system. The main function of the separator is to prevent physical contact between the anode and cathode electrodes, and it also serves as a lithium-ion transport channel within the battery. Currently, commercially available separators are mainly polyolefins such as polyethylene (PE) and polypropylene (PP). However, polyolefin separators still have some problems: (1) Polyolefins have low melting points, resulting in poor thermal dimensional stability of the separators, which poses a risk to the safety of batteries at high temperatures; (2) Polyolefin materials have low polarity and are intrinsically hydrophobic, resulting in poor affinity with highly polar electrolytes. Therefore, the stability and mechanical strength of porous separators are important factors affecting battery safety. However, during the production process, electrode shedding can often puncture the separator, causing contact between the anode and cathode electrodes, which can pose a safety hazard. Therefore, developing high-quality, high-temperature resistant battery separators is of great significance. Summary of the Invention
[0003] To address the aforementioned technical problems, this invention provides a polypropylene separator and its applications. This invention utilizes aramid fiber and inorganic particles (SiO2, ZrO2, etc.) to modify the polypropylene separator, resulting in a high-temperature resistant and thermally stable material. Aramid fiber is a high-temperature resistant, acid and alkali resistant, and lightweight polymer material, widely used in military and aerospace fields due to its high strength and corrosion resistance. The separator surface, after modification with inorganic particles (SiO2, ZrO2, etc.), contains a large number of polar groups, which improves its affinity with the electrolyte.
[0004] The first objective of this invention is to provide a method for preparing a polypropylene separator, comprising the following steps:
[0005] Functionalized modified short aramid fibers were obtained by using acid-modified short aramid fibers.
[0006] The obtained functionalized modified short aramid fibers were mixed and reacted with an inorganic particle suspension to obtain inorganic particle-modified short aramid fibers.
[0007] Polypropylene is mixed with a protonating reagent solution to obtain polypropylene with a positively charged surface.
[0008] The obtained short aramid fibers modified with inorganic particles were blended with the obtained positively charged polypropylene to prepare a polypropylene separator co-modified with aramid and inorganic particles.
[0009] In one embodiment of the present invention, the acid is selected from one or more of phosphoric acid, sulfuric acid and acetic acid, and the acid concentration is 40wt% to 60wt% of the mass concentration of H3PO4.
[0010] In one embodiment of the present invention, the short aramid fiber has a diameter of 2-5 μm and a length of 1-3 mm.
[0011] In one embodiment of the present invention, at least one or more of the following conditions are satisfied:
[0012] The concentration of the inorganic particle suspension is 30wt% to 50wt%.
[0013] The inorganic particles are selected from one or more of SiO2, ZrO2, TiO2, Al2O3, BaSO4, MgO2, BN, and ZnO2;
[0014] The inorganic particles have a particle size of 5–30 nm.
[0015] In one embodiment of the present invention, the mass ratio of the functionalized modified short aramid fiber to the inorganic particulate suspension is 1:25 to 1:10.
[0016] In one embodiment of the present invention, the conditions for the mixed reaction are: a reaction temperature of 40–80°C and a reaction time of 10–14 h.
[0017] In one embodiment of the present invention, the mass ratio of the polypropylene to the protonating reagent in the protonating reagent solution is 10:1 to 20:1; and the concentration of the protonating reagent solution is 0.01 to 0.04 g / mL.
[0018] In one embodiment of the present invention, the mass ratio of the inorganic particle-modified short aramid fiber to the obtained positively charged polypropylene is 1:8 to 1:4.
[0019] A second objective of this invention is to provide a polypropylene separator obtained by the aforementioned preparation method.
[0020] A third object of the present invention is to provide a battery comprising the aforementioned polypropylene separator.
[0021] The technical solution of the present invention has the following advantages over the prior art:
[0022] (1) The modified PP separator obtained by the present invention can improve the high temperature resistance of the polyolefin separator and improve its thermal stability, thereby reducing the safety hazards caused by the battery when it is used at high temperature.
[0023] (2) The short aramid fibers of the modified PP diaphragm of the present invention form polar amino groups, which can improve the polarity of the PP diaphragm and improve its affinity with the electrolyte.
[0024] (3) In the modified PP membrane of the present invention, SiO2 and the modified short aramid fiber are connected together by chemical bonds, which enhances the interaction between them and makes them less susceptible to damage.
[0025] Compared with existing technologies, this invention utilizes chemical bonds to effectively combine SiO2 and short aramid fibers, and simultaneously utilizes electrostatic attraction between positive and negative charges to effectively combine the modified short aramid fibers with polypropylene, resulting in a modified PP membrane. This improves both the tensile and high-temperature resistance of the PP membrane, while also enhancing the affinity between the membrane and the electrolyte. Attached Figure Description
[0026] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein...
[0027] Figure 1 This is a flowchart of the reaction mechanism of the present invention.
[0028] Figure 2 This is a SEM image of the short aramid fiber and SiO2 modified PP material from Example 1 of the present invention.
[0029] Figure 3 This is a SEM image of the aramid and SiO2 modified PP material prepared according to the present invention. Detailed Implementation
[0030] To address the technical problems mentioned in the background section, this invention provides a polypropylene diaphragm, its preparation method, and its application.
[0031] This invention is achieved through the following scheme:
[0032] The first objective of this invention is to provide a method for preparing a polypropylene separator, comprising the following steps:
[0033] Functionalized modified short aramid fibers were obtained by using acid-modified short aramid fibers.
[0034] The obtained functionalized modified short aramid fibers were mixed and reacted with an inorganic particle suspension to obtain inorganic particle-modified short aramid fibers.
[0035] Polypropylene is mixed with a protonating reagent solution to obtain polypropylene with a positively charged surface.
[0036] The obtained short aramid fibers modified with inorganic particles were blended with the obtained positively charged polypropylene to prepare a polypropylene separator co-modified with aramid and inorganic particles.
[0037] In a specific embodiment, the short aramid fiber is pretreated as follows: the short aramid fiber is ultrasonically cleaned with a mixed solvent to remove surface oil and other organic impurities; then it is dried in a vacuum drying oven.
[0038] Furthermore, the mixed solvent includes acetone, ethanol, and deionized water.
[0039] In a specific embodiment, the acid is selected from one or more of phosphoric acid, sulfuric acid, and acetic acid, and the concentration of the acid is 40wt% to 60wt% of the mass concentration of H3PO4. If the concentration is too low (less than 40wt%), too few carboxyl groups will be formed, and if the concentration is too high (greater than 60wt%), the internal structure of the polymer will be destroyed.
[0040] The reaction mechanism of this invention involves the amide group donating electrons, enhancing the reactivity of ortho- and para-hydrogen bonds with aromatic carbons. Then, upon the influence of an electrophile (such as a Lewis acid), electrophilic substitution occurs, subsequently generating a hydroxyl group. Simultaneously, a small amount of the amide group can hydrolyze, leading to the formation of a polar amino group.
[0041] The mechanism steps are as follows:
[0042]
[0043] In a specific embodiment, the short aramid fiber has a diameter of 2-5 μm and a length of 1-3 mm.
[0044] In a specific embodiment, at least one or more of the following conditions are met:
[0045] The concentration of the inorganic particle suspension is 30wt% to 50wt%.
[0046] The inorganic particles are selected from one or more of SiO2, ZrO2, TiO2, Al2O3, BaSO4, MgO2, BN, and ZnO2;
[0047] The inorganic particles have a particle size of 5–30 nm. Adding inorganic particles can enhance the puncture resistance of the diaphragm.
[0048] In a specific embodiment, the mass ratio of the functionalized modified short aramid fiber to the inorganic particle suspension is 1:25 to 1:10. When the ratio is less than this range, there will be fewer inorganic particles, resulting in a less significant improvement in the diaphragm puncture strength; when the ratio is greater than this range, too many inorganic particles will agglomerate on the surface of the short aramid fiber, causing pore blockage.
[0049] In a specific embodiment, the conditions for the mixed reaction are: a reaction temperature of 40–80°C and a reaction time of 10–14 h.
[0050] In a specific embodiment, the mass ratio of the polypropylene to the protonating reagent in the protonating reagent solution is 10:1 to 20:1; the concentration of the protonating reagent solution is 0.01 to 0.04 g / mL.
[0051] In a specific embodiment, the mass ratio of the inorganic particle-modified short aramid fiber to the obtained positively charged polypropylene is 1:8 to 1:4.
[0052] This invention provides a polypropylene separator obtained by the aforementioned preparation method.
[0053] The present invention also provides a lithium-ion battery comprising the aforementioned polypropylene separator.
[0054] In a specific embodiment, the lithium-ion battery further includes a positive electrode, a negative electrode, and an electrolyte.
[0055] Furthermore, the positive electrode active material in the positive electrode sheet is a conventional positive electrode active material in the art, and is not particularly limited here. For example, it can be one or a combination of lithium iron phosphate (LFP), lithium manganese iron phosphate (LFMP), lithium manganese oxide (LMO), lithium nickel manganese oxide (LNMO), lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), and lithium-rich manganese base oxides (LLOs).
[0056] Furthermore, the negative electrode active material in the negative electrode sheet is a conventional negative electrode active material in the art, and is not particularly limited here. For example, it can be one or a combination of several of lithium metal, lithium metal alloy, carbon silicon composite material, graphite, lithium metal nitride, antimony oxide, and carbon germanium composite material; the positive electrode active material in the positive electrode sheet is at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese phosphate, lithium iron manganese phosphate, and lithium iron phosphate.
[0057] Furthermore, the electrolyte is a conventional electrolyte in the art and is not particularly limited.
[0058] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0059] Example 1
[0060] This embodiment provides a method for preparing a PP separator and its application, as described below:
[0061] 1. The preparation method of PP membrane, the specific steps are as follows:
[0062] (1) First, 5 mg of short aramid fibers with a diameter of 2–5 μm and a length of 1–3 mm were ultrasonically cleaned for 60 min using acetone, ethanol, and deionized water, respectively (to remove surface oil and other organic impurities). Then, they were dried in a vacuum drying oven at 80 °C for 12 h. After drying, they were immersed in 50 wt% H3PO4 for 6 h (at 40 °C). Then, the fibers were repeatedly washed with distilled water to remove unreacted H3PO4 until the pH of the short aramid fiber surface was neutral. The treated short aramid fibers were then placed in a vacuum oven and dried at 110 °C for 6 h to obtain modified short aramid fibers. The materials obtained at three different concentrations were subsequently evaluated.
[0063] (2) The modified short aramid fibers obtained in step (1) were placed in a 35 wt% SiO2 suspension (the mass ratio of short aramid fibers to SiO2 suspension was 1:15, with suspended particle diameters ranging from 5 to 30 nm) and reacted at 60°C for 12 h. The solid was collected and vacuum dried at 80°C for 12 h to obtain SiO2-modified short aramid fibers. The structure of the obtained SiO2-modified short aramid fibers was characterized, and the results are shown in [Figure 1]. Figure 2 ,from Figure 2 A large number of particles can be clearly seen on the surface of the short aramid fibers. The prepared aramid fibers were placed in SiO2 solutions with a mass ratio of 1:25 and 1:10, which can be used as Examples 2 and 3.
[0064] (3) Soak 3g of PP (polypropylene) in 10mL of 0.02g / mL dopamine solution (dopamine will produce a protonation reaction) to make the PP surface contain a large number of protons, and obtain modified polypropylene with a positively charged surface.
[0065] (4) The SiO2-modified short aramid fibers obtained in step (2) are blended with the positively charged polypropylene obtained in step (3). The blend of the prepared SiO2-modified short aramid fibers and positively charged polypropylene is fed into the screw of the twin-screw extruder from the hopper. Under the action of the screw pump at a speed of 25 rpm, it is conveyed forward by the friction between the inner wall of the barrel and the surface of the screw. In the screw feeding section, the material fills the screw groove. As the material is continuously conveyed, it is compacted. When the material enters the compression section, due to the gradual shallowing of the screw groove depth and the resistance of the die head, the material gradually forms high pressure and is further compacted. At the same time, the material begins to melt when the barrel is heated to an external temperature of 205°C. A PP membrane co-modified with aramid and silica is prepared. The structure of the PP membrane is characterized, and the results are shown in the figure. Figure 3 As can be seen from the figure, the modified short aramid fibers and the PP separator are well composited. The material surface also shows that a large gap is formed between the modified short aramid fibers and the PP, which is beneficial for electrolyte wetting and lithium ion shuttle passage.
[0066] Example 2
[0067] Similar to the preparation method in Example 1, the difference is that the mass ratio of short aramid fibers to SiO2 suspension is 1:25, while the other reaction conditions remain unchanged.
[0068] Example 3
[0069] Similar to the preparation method in Example 1, the difference is that the mass ratio of short aramid fibers to SiO2 suspension is 1:10, while the other reaction conditions remain unchanged.
[0070] Comparative Example 1
[0071] The diaphragm provided in this comparative example is a standard PP diaphragm that can be purchased directly from the market.
[0072] Comparative Example 2
[0073] The preparation method of the diaphragm provided in this comparative example is similar to that in Example 1, except that: the PP was not modified with short aramid fibers, and a SiO2 modified PP diaphragm was obtained.
[0074] Comparative Example 3
[0075] The preparation method of the diaphragm provided in this comparative example is similar to that in Example 1, except that: SiO2 modification was not performed, resulting in a PP diaphragm modified with short aramid fibers.
[0076] Battery Applications
[0077] (1) Preparation of electrolyte: Ethyl carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed organic solvent. Then, fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare the electrolyte.
[0078] (1) The battery includes: positive electrode, negative electrode, electrolyte and modified PP separator obtained in the examples and comparative examples.
[0079] The positive electrode active material of the positive electrode sheet is a ternary material, and the positive electrode active material of the negative electrode sheet is graphite. The preparation methods of the positive electrode sheet and the negative electrode sheet are as follows:
[0080] Preparation of the active slurry for the positive electrode: according to 97.2wt% LiN 0.6 C 0.2 M 0.2O2 (ternary material), 0.9 wt% PVDF, 1.4 wt% SP, and 0.5 wt% CNT were mixed to obtain a mixed material. This mixed material was then thoroughly stirred in NMP to obtain the corresponding active slurry for the positive electrode. The positive electrode slurry was coated onto both sides of the positive electrode current collector aluminum foil, resulting in a thickness of 128 μm and a single-sided density of 0.02 g / cm³. 2 The negative electrode is coated with a homogenized slurry, dried, and pressed to obtain the positive electrode sheet.
[0081] Preparation of the active slurry for the negative electrode: A mixture of 96.4 wt% graphite, 1.7 wt% binder, 0.9 wt% CMC, and 1 wt% SP was obtained. This mixture was then thoroughly stirred in deionized water to obtain the corresponding active slurry for the positive electrode. The negative electrode slurry was coated onto both sides of the copper foil used as the negative electrode current collector, resulting in a slurry with a thickness of 154 μm and a single-sided density of 0.012 g / cm³. 2 The negative electrode paste coating is dried and pressed into a sheet to obtain the negative electrode sheet.
[0082] (3) Assembly of lithium-ion batteries:
[0083] The negative electrode, separator, and positive electrode are wound together to obtain the battery cell. The battery cell is then assembled into a battery case, dried, injected with electrolyte, sealed, formed, and tested for capacity to obtain a lithium-ion battery.
[0084] (4) Battery performance testing
[0085] The batteries obtained from the examples and comparative examples were subjected to initial tests for coulombic efficiency, powder resistance, and cycle capacity retention.
[0086] At room temperature (25℃), with initial and cutoff voltages of 2.8V and 4.35V respectively, the battery was charged at 1C to 4.35V, then charged at a constant voltage of 4.35V until the current decreased to 0.05C, then discharged at 0.5C to 2.8V. This process was repeated, charging again at 1C to 4.35V, then charging at a constant voltage of 4.35V until the current decreased to 0.05C, and finally discharging at 0.5C to 2.8V. The capacity retention after 300 cycles was calculated. The experimental results are shown in Table 2.
[0087] (5) Diaphragm performance test
[0088] The diaphragms obtained in the examples and comparative examples were subjected to heat distortion temperature tests, tensile strength tests, tensile strength tests, and liquid absorption rate tests.
[0089] (A) Test method for heat distortion temperature: A weight is suspended from the diaphragm and placed in an oven at a set heating rate (2℃ / min). The temperature and time when the weight falls are recorded. The heat resistance characteristics of the diaphragm are qualitatively evaluated by the time from a certain temperature point to the weight falling. The experimental results are shown in Table 1.
[0090] (B) Tensile Strength Test Method: Place the specimen in the universal tensile testing machine fixture and directly test the tensile strength of the diaphragm using the universal tensile testing machine. Specific method: Cut the diaphragm into strips 15mm wide and 200mm long. Clamp the top and bottom ends of the diaphragm on the tensile testing machine. Stretch in a 180° direction at a speed of 250mm / min. The gauge length of the specimen is 100mm. The tensile test continues until the diaphragm breaks. Obtain the tensile strength value of this experiment on the tensile testing machine. The experimental results are shown in Table 1.
[0091] (C) Test method for liquid absorption rate: Take a 5×5cm sample from each group. 2 The diaphragm, weighed and recorded as 'a', was immersed in the electrolyte for 1 hour to allow it to fully absorb the electrolyte. After absorption, the diaphragm was suspended for 5 minutes to dry the electrolyte adhering to its surface, and weighed again and recorded as 'b'. The electrolyte absorption rate of the diaphragm was (b~a) / a×100%. The experimental results are shown in Table 1.
[0092] (D) Puncture Strength Test Method: Using a diaphragm puncture testing machine, the diaphragm is cut into strips, the width of which must be greater than 100mm. A 100mm wide test piece is mounted on the membrane fixing ring, and then a steel needle with a diameter of 1mm and a tip radius of 0.5mm is used to puncture the test piece at a speed of 50mm / min. The load of the needle penetrating the test piece is recorded. The experimental results are shown in Table 1.
[0093] Table 1. Performance test results of the diaphragms obtained in the examples and comparative examples.
[0094]
[0095]
[0096] Table 2. Performance test results of the batteries in the examples and comparative examples.
[0097] Group Information Internal resistance / mΩ First-efficacy / % cycle Comparative Example 1 21.3 80.5 85.6% Comparative Example 2 16.8 83.7 87.2% Comparative Example 3 17.6 84.5 88.3% Example 1 10.8 90.8 92.8% Example 2 13.2 86.7 91.2% Example 3 14.5 85.2 90.5%
[0098] Note: Cyclic performance refers to the capacity retention rate of batteries prepared with each group of separators after 300 battery cycles.
[0099] Table 1 shows that the PP separator modified with SiO2 and short aramid fibers exhibits thermal deformation at 230℃, which is significantly higher than the thermal deformation temperature of conventional PP separators in the prior art. This indicates that dual modification with SiO2 and short aramid fibers can improve the thermal stability of the PP separator. Similarly, tensile strength, puncture strength, and liquid absorption rate are all greatly improved, demonstrating that dual modification with SiO2 and short aramid fibers can solve the problems of separator puncture resistance and the compatibility between the separator and the electrolyte.
[0100] Table 2 shows that the battery modified with both SiO2 and short aramid fibers effectively reduces internal resistance compared to the battery with a pure PP separator; at the same time, the battery's initial efficiency is also significantly improved, increasing by 10.3% compared to the pure PP separator. The cycle life of the dual-modified separator is 7.2% higher than that of the pure PP separator.
[0101] Similarly, the tensile strength of the modified PP membrane can be enhanced by dual modification with SiO2 and short aramid fibers, increasing by 85% compared to the pure PP membrane, showing significant improvement. Simultaneously, the liquid absorption rate is also significantly improved, increasing by 60% compared to the pure PP membrane, demonstrating that the PP membrane obtained by this invention has excellent compatibility with the electrolyte. The puncture strength of the dual-modified membrane is increased by 63% compared to the pure PP membrane, indicating that the modified PP membrane obtained by this invention can effectively prevent puncture.
[0102] In summary, this invention enhances the thermal stability of the modified diaphragm, improves its tensile strength and liquid absorption rate, and enhances the mechanical strength of the PP diaphragm while increasing its thermal stability and puncture strength through the synergistic effect of SiO2 and short aramid fibers.
[0103] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A method for preparing a polypropylene diaphragm, characterized in that, Includes the following steps: Functionalized modified short aramid fibers were obtained by using acid-modified short aramid fibers. The obtained functionalized modified short aramid fibers are mixed and reacted with an inorganic particle suspension to obtain inorganic particle-modified short aramid fibers; wherein, the inorganic particles are selected from one or more of SiO2, ZrO2, TiO2, Al2O3, BaSO4, MgO, BN, and ZnO; the mass ratio of functionalized modified short aramid fibers to inorganic particle suspension is 1:25 to 1:10; Polypropylene is mixed with a protonating reagent solution to obtain polypropylene with a positively charged surface. The obtained short aramid fibers modified with inorganic particles were blended with the obtained positively charged polypropylene to prepare a polypropylene separator co-modified with aramid and inorganic particles.
2. The preparation method according to claim 1, characterized in that, The acid is selected from one or more of phosphoric acid, sulfuric acid and acetic acid, and the mass concentration of the acid is 40wt% to 60wt%.
3. The preparation method according to claim 1, characterized in that, The short aramid fibers have a diameter of 2~5μm and a length of 1~3mm.
4. The preparation method according to claim 1, characterized in that, At least one of the following conditions must be met: The concentration of the inorganic particulate suspension is 30wt%~50wt%; The inorganic particles have a particle size of 5~30nm.
5. The preparation method according to claim 1, characterized in that, The conditions for the mixed reaction are: reaction temperature of 40~80℃ and reaction time of 10~14h.
6. The preparation method according to claim 1, characterized in that, The mass ratio of the protonating reagent in the polypropylene to the protonating reagent solution is 10:1 to 20:1; the concentration of the protonating reagent solution is 0.01 to 0.04 g / mL.
7. The preparation method according to claim 1, characterized in that, The mass ratio of the inorganic particle-modified short aramid fiber to the obtained positively charged polypropylene is 1:8 to 1:
4.
8. A polypropylene separator, characterized in that, Obtained by the preparation method according to any one of claims 1 to 7.
9. A battery, characterized in that, Includes the polypropylene diaphragm as described in claim 8.
Citation Information
Patent Citations
Organic fiber reinforced polyethylene lithium battery diaphragm and preparation method thereof
CN112467304A
Preparation method and application of porous polyolefin composite membrane
CN115347322A