Method of forming a semiconductor structure

By performing multiple etching processes on the substrate and forming a protective layer on the sidewalls of the fins, the problem of morphology control during the scaling down of fin field-effect transistors was solved, the dimensional uniformity and stability of the fins were improved, and the performance of the semiconductor structure was enhanced.

CN117293089BActive Publication Date: 2026-11-24SEMICON MFG INT (SHANGHAI) CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210699664.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-20
Publication Date
2026-11-24
Estimated Expiration
2042-06-20

AI Technical Summary

Technical Problem

In the prior art, fin field-effect transistors face problems such as leakage current, short-channel effect and weakened gate control capability during the scaling process, and the fin morphology control is not good.

Method used

By performing several etching processes on the substrate, first and second fins are formed. Before each etching, the etched portion is protected and a protective layer is formed on the sidewall of the fin to avoid over-etching, reduce the difference in etching rate caused by different materials, and improve the fin size uniformity.

Benefits of technology

This achieves stability and uniformity in fin dimensions, improving the performance of the semiconductor structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117293089B_ABST
    Figure CN117293089B_ABST
Patent Text Reader

Abstract

A method for forming a semiconductor structure includes: providing a substrate, the substrate including a first region and a second region, the first region and the second region being made of different materials; forming a plurality of mutually discrete mask layers on the surface of the first region and the surface of the second region; after forming the mask layers, performing a plurality of etching processes on the exposed substrate to form a first fin in the first region and a second fin in the second region, each etching process including: etching the exposed substrate to form a transition first fin in the first region and a transition second fin in the second region; forming a first protective layer on the sidewall surface of the transition first fin and the transition second fin to reduce the difference in etching rate caused by the different materials of the first region and the second region during the etching process, thereby providing uniformity in the size of the formed first fin and the second fin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a semiconductor structure. Background Technology

[0002] In the existing semiconductor field, the FinFET is an emerging multi-gate device. Compared with the planar metal-oxide-semiconductor field-effect transistor (MOSFET), the FinFET has stronger short-channel rejection capability and higher operating current, and is now widely used in various semiconductor devices.

[0003] With the further development of semiconductor technology, transistor dimensions have shrunk to below a few nanometers, and fin field-effect transistors (FETs) are facing serious problems such as leakage current, short-channel effect, and weakened gate control capability. To improve the performance of FETs, morphological control of the fins has become crucial.

[0004] However, the technology for forming fins in fin-type field-effect transistor structures needs to be improved in the existing technology. Summary of the Invention

[0005] The technical problem solved by this invention is to provide a method for forming a semiconductor structure to improve the performance of the formed semiconductor structure.

[0006] To solve the above-mentioned technical problems, a method for forming a semiconductor structure is provided, comprising: providing a substrate, the substrate including a first region and a second region, the first region and the second region being made of different materials; forming a plurality of mutually discrete mask layers on the surface of the first region and the surface of the second region; after forming the mask layers, performing a plurality of etching processes on the exposed substrate to form a first fin in the first region and a second fin in the second region, wherein each etching process comprises: etching the exposed substrate to form a transitional first fin in the first region and a transitional second fin in the second region; and forming a first protective layer on the sidewall surface of the transitional first fin and the transitional second fin.

[0007] Optionally, the method for forming the first protective layer includes: forming a first protective material layer on the substrate surface, the surface of the transition first fin, and the surface of the transition second fin; and etching back the first protective material layer until the substrate surface is exposed.

[0008] Optional, the etching process includes dry etching.

[0009] Optional process parameters for dry etching include: etching gas including fluorocarbon gas, bias voltage range of 600V to 1300V, and etching power range of 100W to 500W.

[0010] Optionally, in the fluorocarbon gas, the ratio of carbon atoms to fluorine atoms ranges from 1.5:1 to 4:1.

[0011] Optionally, the material of the first protective material layer includes a dielectric material, which includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbon oxynitride, and silicon carbon oxynitride.

[0012] Optionally, the material of the first protective material layer includes silicon oxide; the formation process of the first protective material layer includes atomic layer deposition.

[0013] Optionally, the process parameters for atomic layer deposition include: the reaction gases include aminosilane and oxygen.

[0014] Optionally, the formation process of the first protective layer and several etching processes are carried out in the same reaction chamber.

[0015] Optionally, after the mask layer is formed and before several etching processes, a second protective layer is formed on the sidewall surface of the mask layer.

[0016] Optionally, the method for forming the second protective layer includes: forming a second protective material layer on the substrate surface and the mask layer surface; and etching back the second protective material layer until the substrate surface is exposed.

[0017] Optionally, the material of the second protective layer includes silicon oxide; the formation process of the second protective material layer includes atomic layer deposition.

[0018] Optionally, the etching process includes dry etching; the process parameters for dry etching include: etching gas including fluorocarbon gas, bias voltage range of 600V to 1300V, and etching power range of 100W to 500W.

[0019] Optionally, the substrate includes a base, with the first region and the second region located on the base.

[0020] Optionally, the material of the first region includes silicon; the material of the second region includes germanium-silicon.

[0021] Optionally, the etching process includes dry etching; the process parameters for dry etching are as follows: the etching gas includes one or more of hydrogen, hydrocarbon, fluorine, SF6, and HBr, the gas flow rate ranges from 100 sccm to 400 sccm, and the power ranges from 100 W to 500 W.

[0022] Optionally, the number of etching processes ranges from 2 to 20.

[0023] Optionally, the etching process has an etching selectivity ratio of 1:1 to 1.2:1 for the first region and the second region; and an etching selectivity ratio of 2:1 to 10:1 for the first region and the first protective layer.

[0024] Optionally, the thickness of the first protective layer ranges from 0.2 nm to 0.6 nm.

[0025] Compared with the prior art, the technical solution of the embodiments of the present invention has the following beneficial effects:

[0026] In the semiconductor structure formation method provided by the present invention, the exposed substrate is subjected to several etching processes to form a first fin in a first region and a second fin in a second region. Each etching process includes: etching the exposed substrate to form a transitional first fin in the first region and a transitional second fin in the second region; and forming a first protective layer on the sidewall surfaces of the transitional first and second fins. In this method, the first and second fins are formed by multi-segment etching. Before each etching step, the already etched portions are protected to avoid over-etching of the etched areas, thereby reducing the difference in etching rate caused by the different materials of the first and second regions during the etching process, and providing uniformity in the dimensions of the formed first and second fins.

[0027] Furthermore, before forming the mask layer and before several etching processes, the method further includes forming a second protective layer on the sidewall surface of the mask layer. The second protective layer is used to protect the sidewall of the mask layer, preventing the mask layer from being consumed during the etching process, which would lead to a reduction in the size of the formed first fin (second fin), and improving the dimensional stability of the formed first fin and second fin. Attached Figure Description

[0028] Figures 1 to 2 This is a schematic cross-sectional view of the semiconductor structure formation process;

[0029] Figures 3 to 15 This is a schematic diagram of the steps in the method for forming a semiconductor structure according to an embodiment of the present invention;

[0030] Figure 16 This is a flowchart of the etching process steps in the semiconductor structure formation method of the present invention. Detailed Implementation

[0031] It should be noted that the terms "surface" and "on" in this specification are used to describe the relative spatial position and are not limited to whether there is direct contact.

[0032] As described in the background section, the performance of semiconductor structures formed using existing finned transistor (FMT) technology urgently needs improvement. This section will now illustrate and analyze one such semiconductor structure.

[0033] Figures 1 to 2 This is a cross-sectional schematic diagram of the semiconductor structure formation process.

[0034] Please refer to Figure 1A substrate 100 is provided, the substrate 100 includes a first region I and a second region II; a first channel material layer 101 is formed in the first region I; a second channel material layer 102 is formed in the second region II; a hard mask layer 103 is formed on the first channel material layer 101 and the second channel material layer 102, the hard mask layer 103 exposing a portion of the surface of the first channel material layer 101 and a portion of the surface of the second channel material layer 102.

[0035] Please refer to Figure 2 Using a hard mask layer 103 as a mask, a first channel material layer 101, a second channel material layer 102, and a substrate 100 are etched to form a first fin 104 and a second fin 105. The first fin 104 includes a first bottom structure 104a and a first channel layer 104b, and the second fin 105 includes a second bottom structure 105a and a second channel layer 105b. The first channel layer 104b is formed using the first channel material layer 101, and the second channel 105b is formed using the second channel material layer 102.

[0036] In the above method, the first channel material layer 101 is made of silicon, the second channel material layer 102 is made of germanium-silicon, the first channel 104b is used to form the channel for an N-type device, and the second channel 105b is used to form the channel for a P-type device. The second channel 105b is made of germanium-silicon, and the second bottom structure 105a is made of silicon. Due to the lattice mismatch between germanium-silicon and silicon, compressive stress is generated on the second channel 105. This compressive stress can reduce the effective conductivity of holes in the channel direction and improve the speed of the PMOS device.

[0037] The etching process of the first channel material layer 101 and the second channel material layer 102 typically employs a halogen-based plasma etching gas. However, during the etching process, the etching rate for germanium-silicon materials is greater than that for silicon materials. This can lead to over-etching of the second fin 105 relative to the first fin 104, resulting in a smaller size for the second fin 105 and potentially causing it to have a pointed, conical shape, which is detrimental to controlling the uniformity of the fin size.

[0038] To address the aforementioned technical problems, the present invention provides a method for forming a semiconductor structure. This method involves performing several etching processes on an exposed substrate to form a first fin in a first region and a second fin in a second region. Each etching process includes: etching the exposed substrate to form a transitional first fin in the first region and a transitional second fin in the second region; and forming a first protective layer on the sidewall surfaces of the transitional first and second fins. In this method, the first and second fins are formed by multi-segment etching. Before each etching step, the already etched portions are protected to prevent over-etching of the etched areas. This reduces the difference in etching rate caused by the different materials in the first and second regions during the etching process, thus ensuring the uniformity of the dimensions of the formed first and second fins.

[0039] To make the above-mentioned objectives, features and beneficial effects of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0040] Figures 3 to 15 This is a schematic diagram of the steps in the method for forming a semiconductor structure according to an embodiment of the present invention.

[0041] Please refer to Figure 3 A substrate is provided, the substrate includes a first region 201 and a second region 202, the materials of the first region 201 and the second region 202 are different; a plurality of mutually discrete mask layers 203 are formed on the surface of the first region 201 and the surface of the second region 202.

[0042] The first region 201 is used to form the first fin; the second region 201 is used to form the second fin.

[0043] In this embodiment, the substrate includes a base 200, and a first region 201 and a second region 202 are located on the base 200.

[0044] The substrate 200 can be made of monocrystalline silicon, polycrystalline silicon, or amorphous silicon, or it can be a semiconductor material such as silicon, germanium, silicon germanide, or gallium arsenide, or it can be a semiconductor-on-insulator structure. In this embodiment, the substrate 200 is made of monocrystalline silicon.

[0045] In this embodiment, the material of the first region 201 includes silicon; the material of the second region 202 includes germanium-silicon. Specifically, the first region 201 is used to form an N-type device, and the second region 202 is used to form a P-type device.

[0046] In this embodiment, the hard mask layer 203 includes a first hard mask layer 203a and a second hard mask layer 203b located on the first hard mask layer 203a.

[0047] The material of the hard mask layer 203 is a dielectric material, which includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbon oxynitride, and silicon carbon oxynitride.

[0048] Specifically, in this embodiment, the material of the first hard mask layer 203a includes silicon nitride; the material of the second hard mask layer 203b includes silicon oxide.

[0049] The method for forming the hard mask layer 203 includes: forming a first hard mask material layer (not shown in the figure) on the surface of a substrate; forming a second hard mask material layer (not shown in the figure) on the first hard mask material layer; forming a patterned layer (not shown in the figure) on the second hard mask material layer, wherein the patterned layer exposes a portion of the second hard mask layer; and etching the second hard mask material layer and the first hard mask material layer using the patterned layer as a mask until the substrate surface is exposed.

[0050] In this embodiment, an etch stop layer 204 is formed on the substrate surface before the first hard mask material layer is formed. Specifically, the second hard mask material layer and the first hard mask material layer are etched using the patterned layer as a mask until the etch stop layer 204 on the substrate surface is exposed.

[0051] Subsequently, after the mask layer 203 is formed, the exposed substrate is etched several times to form the first fin in the first region 201 and the second fin in the second region 202.

[0052] After the mask layer 203 is formed, and before several etching processes, the method further includes forming a second protective layer on the sidewall surface of the mask layer 203. For the method of forming the second protective layer, please refer to [reference needed]. Figures 4 to 5 .

[0053] Please refer to Figure 4 A second protective material layer 205 is formed on the substrate surface and the mask layer 203 surface.

[0054] The material of the second protective layer 205 includes silicon oxide.

[0055] The formation process of the second protective material layer 205 includes atomic layer deposition (ALD). ALD is beneficial for improving the surface smoothness of the formed second protective material layer 205.

[0056] Please refer to Figure 5 Then, etch back the second protective material layer 205 until the substrate surface is exposed.

[0057] The second protective layer 206 is used to protect the sidewalls of the mask layer 203, preventing the mask layer 203 from being consumed during the etching process, which would lead to a reduction in the size of the formed first fin (second fin) and improve the dimensional stability of the formed first fin and second fin.

[0058] The etch-back process includes dry etching. The process parameters for dry etching include: etching gas (fluorocarbon gas), bias voltage ranging from 600V to 1300V, and etching power ranging from 100W to 500W. The process conditions of dry etching facilitate directional etching, improve the uniformity of the formed second protective layer (206 film thickness), and enhance the accuracy of subsequent pattern transfer.

[0059] The etching process includes dry etching; the process parameters for dry etching are as follows: the etching gas includes one or more of hydrogen, hydrocarbon, fluorine, SF6, and HBr, the gas flow rate ranges from 100 sccm to 400 sccm, and the power ranges from 100 W to 500 W.

[0060] Figure 16 This is a flowchart of the etching process steps in the semiconductor structure formation method of the present invention.

[0061] Please refer to Figure 16 After the mask layer 203 is formed, the exposed substrate is etched several times to form a first fin in the first region 201 and a second fin in the second region 202. The method for each etching process includes the following steps:

[0062] Step 301: Etch the exposed substrate to form a transition first fin in the first region and a transition second fin in the second region;

[0063] Step 302: A first protective layer is formed on the sidewall surfaces of the transition first fin and the transition second fin.

[0064] Next, each step will be analyzed and explained.

[0065] The number of etching processes ranges from 2 to 20. In this embodiment, the number of etching processes is 3.

[0066] In this embodiment, after the mask layer 203 is formed, the exposed substrate is etched three times to form the first fin in the first region 201 and the second fin in the second region 202. Please refer to [reference needed]. Figures 6 to 14 Specifically, please refer to the instructions for the first etching process. Figures 6 to 8 For the second etching process, please refer to [the relevant documentation / reference]. Figures 9 to 11 For the third etching process, please refer to [the relevant documentation / reference]. Figures 12 to 14 .

[0067] Please refer to Figure 6 And continue to refer to Figure 16 First etching process: The exposed substrate is etched to form a transition first fin 207 in the first region 201 and a transition second fin 208 in the second region 202.

[0068] The etching process selectivity ratio for the first region 201 and the second region 202 ranges from 1:1 to 1.2:1.

[0069] In this embodiment, the second protective layer 206 is consumed during the etching process.

[0070] In the subsequent first etching process, a first protective layer is formed on the sidewall surfaces of the transition first fin 207 and the transition second fin 208. Please refer to [reference needed] for the method of forming the first protective layer. Figures 7 to 8 .

[0071] Please refer to Figure 7 And continue to refer to Figure 16 First etching process: A first protective material layer 209 is formed on the substrate surface, the transition first fin 207 and the transition second fin 208.

[0072] The material of the first protective material layer 209 includes a dielectric material, which includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbon oxynitride, and silicon carbon oxynitride.

[0073] In this embodiment, the material of the first protective material layer 209 includes silicon oxide.

[0074] In this embodiment, the formation process of the first protective material layer 209 includes atomic layer deposition (ALD). ALD is beneficial for improving the surface smoothness of the first protective material layer 209.

[0075] In this embodiment, the process parameters of the atomic layer deposition process include: the reaction gases include aminosilane and oxygen. The atomic layer deposition process uses aminosilane and oxygen to react, which does not consume material for the transition first fin 207 and the transition second fin 208, and therefore does not damage the transition first fin 207 and the transition second fin 208, which is beneficial to improving the dimensional stability of the first fin and the second fin.

[0076] Please refer to Figure 8 And continue to refer to Figure 16 First etching process: Etching back the first protective material layer 209 until the substrate surface is exposed.

[0077] The thickness of the first protective layer 210 ranges from 0.2 nm to 0.6 nm.

[0078] The etching process includes dry etching.

[0079] The process parameters for dry etching include: etching gas (fluorocarbon gas), bias voltage ranging from 600V to 1300V, and etching power ranging from 100W to 500W. The process conditions of dry etching facilitate directional etching, improve the uniformity of the first protective layer 209 thickness, and enhance the accuracy of subsequent pattern transfer.

[0080] In fluorocarbon gases, the ratio of carbon atoms to fluorine atoms ranges from 1.5:1 to 4:1. Different fin etching morphologies can be obtained by adjusting the ratio of carbon atoms to fluorine atoms in the fluorocarbon gas.

[0081] In this embodiment, the formation process of the first protective layer 210 and the several etching processes are carried out within the same reaction chamber. The formation process of the first protective layer 210 and the several etching processes do not require transfer between different reaction chambers, avoiding the introduction of unnecessary impurities and improving the quality and uniformity of the film thickness of the first protective layer 210.

[0082] Next, a second etching process is performed on the exposed substrate. Please refer to [link / reference]. Figures 9 to 11 .

[0083] Please refer to Figure 9 And continue to refer to Figure 16 The second etching process involves etching the exposed substrate to form a transition first fin 207 in the first region 201 and a transition second fin 208 in the second region 202.

[0084] The etching process selectivity ratio for the first region 201 and the second region 202 ranges from 1:1 to 1:1.2.

[0085] The etching process selectivity ratio for the first region 201 and the first protective layer 210 ranges from 2:1 to 10:1. The purpose of selecting this etching selectivity range is to allow for the selection of a suitable etching process so that the first protective layer 210 can be removed after the formation of the transition first fin 207 and the transition second fin 208. This facilitates the uniformity of the thickness of the first protective layer 210 formed on the sidewall surfaces of the transition first fin 207 and the transition second fin 208 in the next etching process, thereby improving the accuracy of subsequent pattern transfer and enhancing the morphology of the formed first and second fins.

[0086] In the subsequent second etching process, a first protective layer 210 is formed on the sidewall surfaces of the transition first fin 207 and the transition second fin 208. For the method of forming the first protective layer 210, please refer to [reference needed]. Figures 10 to 11 And continue to refer to Figure 16 The method for forming the first protective layer 210 in the second etching process is the same as that in the first etching process.

[0087] Next, please refer to Figures 12 to 14 And continue to refer to Figure 16 The third etching process is the same as the previous two etching processes, and will not be described in detail here.

[0088] In this embodiment, the etching process is performed three times. In other embodiments, the number of etching processes ranges from two to twenty times. The number of etching processes can be adjusted based on actual production costs, etching effects, etc.

[0089] Thus, the exposed substrate is etched several times to form the first fin 211 in the first region 201 and the second fin 212 in the second region 202. The first fin 211 and the second fin 212 are etched in multiple segments. Before each etching, the etched part is protected to avoid over-etching of the etched area, thereby reducing the difference in etching rate caused by the different materials of the first region 201 and the second region 202 during the etching process, and providing uniformity in the size of the formed first fin 211 and second fin 212.

[0090] In this embodiment, please refer to the following examples. Figures 14 to 15 .

[0091] Please refer to Figure 14 A third protective layer 213 is formed on the sidewall surface of the first fin 211 and the second fin 212.

[0092] The material of the third protective layer 213 includes a dielectric material, which includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbonate, silicon carbonitride, and silicon carbonitride. In this embodiment, the material of the third protective layer 213 is silicon oxide.

[0093] Please refer to Figure 15 After forming the third protective layer 213, the substrate 200 is etched to form a first bottom structure 214 located at the bottom of the first fin 211 and a second bottom structure 215 located at the bottom of the second fin 212 within the substrate 200.

[0094] In this embodiment, the etching process for the substrate 200 includes a dry etching process. The dry etching process is beneficial for improving the morphology of the formed first bottom structure 214 and second bottom structure 215.

[0095] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that, include: A substrate is provided, the substrate comprising a first region and a second region, the first region and the second region being made of different materials; Several mutually independent mask layers are formed on the surface of the first region and the surface of the second region; After forming the mask layer, the exposed substrate is subjected to several etching processes to form a first fin in the first region and a second fin in the second region. The method for each etching process includes: The exposed substrate is etched to form a transition first fin in the first region and a transition second fin in the second region; A first protective layer is formed on the sidewall surface of the first transition fin and the second transition fin. The first protective layer is used to protect the first transition fin and the second transition fin in the next etching process to reduce the difference in etching rate caused by the different materials of the first region and the second region.

2. The method for forming a semiconductor structure as described in claim 1, characterized in that, The method for forming the first protective layer includes: forming a first protective material layer on the surface of the substrate, the first transition fin, and the second transition fin; and etching back the first protective material layer until the substrate surface is exposed.

3. The method for forming a semiconductor structure as described in claim 2, characterized in that, The etching process includes dry etching.

4. The method for forming a semiconductor structure as described in claim 3, characterized in that, The process parameters of the dry etching process include: etching gas including fluorocarbon gas, bias voltage range of 600 V to 1300 V, and etching power range of 100 W to 500 W.

5. The method for forming a semiconductor structure as described in claim 4, characterized in that, In the fluorocarbon gas, the ratio of carbon atoms to fluorine atoms ranges from 1.5:1 to 4:

1.

6. The method for forming a semiconductor structure as described in claim 2, characterized in that, The material of the first protective material layer includes a dielectric material, which includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbon oxynitride, and silicon carbon oxynitride.

7. The method for forming a semiconductor structure as described in claim 2, characterized in that, The material of the first protective material layer includes silicon oxide; the formation process of the first protective material layer includes atomic layer deposition.

8. The method for forming a semiconductor structure as described in claim 7, characterized in that, The process parameters of the atomic layer deposition process include: the reaction gases include aminosilane and oxygen.

9. The method for forming a semiconductor structure as described in claim 1, characterized in that, The formation process of the first protective layer and the several etching processes are carried out in the same reaction chamber.

10. The method for forming a semiconductor structure as described in claim 1, characterized in that, After the mask layer is formed and before the etching processes, the method further includes forming a second protective layer on the sidewall surface of the mask layer.

11. The method for forming a semiconductor structure as described in claim 10, characterized in that, The method for forming the second protective layer includes: forming a second protective material layer on the substrate surface and the mask layer surface; and etching back the second protective material layer until the substrate surface is exposed.

12. The method for forming a semiconductor structure as described in claim 11, characterized in that, The material of the second protective material layer includes silicon oxide; the formation process of the second protective material layer includes atomic layer deposition.

13. The method for forming a semiconductor structure as described in claim 11, characterized in that, The process of etching back the second protective material layer includes a dry etching process; the process parameters of the dry etching process include: the etching gas includes a fluorocarbon gas, the bias voltage range is 600 V to 1300 V, and the etching power range is 100 W to 500 W.

14. The method for forming a semiconductor structure as described in claim 1, characterized in that, The substrate includes a base, and the first region and the second region are located on the base.

15. The method for forming a semiconductor structure as described in claim 1, characterized in that, The material of the first region includes silicon; the material of the second region includes germanium-silicon.

16. The method for forming a semiconductor structure as described in claim 1, characterized in that, The etching process includes dry etching; the process parameters for dry etching are as follows: the etching gas includes one or more of hydrogen, hydrocarbon, fluorine, SF6, and HBr, the gas flow rate ranges from 100 sccm to 400 sccm, and the power ranges from 100 W to 500 W.

17. The method for forming a semiconductor structure as described in claim 1, characterized in that, The number of etching processes ranges from 2 to 20.

18. The method for forming a semiconductor structure as described in claim 1, characterized in that, The etching process has an etching selectivity ratio of 1:1 to 1.2:1 for the first region and the second region; and an etching selectivity ratio of 2:1 to 10:1 for the first region and the first protective layer.

19. The method for forming a semiconductor structure as described in claim 1, characterized in that, The thickness of the first protective layer ranges from 0.2 nm to 0.6 nm.

Citation Information

Patent Citations

  • Semiconductor structure and forming method thereof

    CN114156233A

  • Semiconductor fins with dielectric isolation at fin bottom

    US20190311955A1