Method of manufacturing a porous metal or ceramic component and component manufactured using the method
By manufacturing porous metal or ceramic components with different porosities, and utilizing suspension coating and sintering technologies, the problem of insufficient connection stability of porous components is solved, enabling the safe supply and discharge of media and energy, and enhancing the strength and stability of the components.
Patent Information
- Application Number
- CN202280032508.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-11
- Filing Date
- 2022-05-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-05-10
AI Technical Summary
Existing porous components suffer from insufficient stability during connection and make it difficult to achieve safe and permanent supply or discharge of media or energy, especially in electric heating elements or heat exchangers, where connection options are limited and joint breakage is common.
By manufacturing porous metal or ceramic components with three volume regions having different porosities, and using a suspension to coat the surface of the semi-finished product with metal or ceramic particles, a shape-locked connection is formed, including drying and sintering processes, ensuring stable bonding of each region.
Stable connection of porous components is achieved, enabling safe supply or discharge of media and energy, avoiding joint breakage, and enhancing the strength and stability of the components.
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing porous metal or ceramic components and a method for manufacturing using this method. Background Technology
[0002] Porous components are used in a wide variety of technical fields. They are used for filtering or receiving solid or liquid media, and also as heat exchangers. They are also frequently used as insulators or damping elements. In many applications, open-cell structures are desirable. However, the open-cell porosity leads to a loss of strength and stability, necessitating the use of supported, individual frame structures for many applications. While these structures ensure greater strength, they cannot bond with open-cell foams with sufficient durability or can only be bonded with great difficulty.
[0003] Furthermore, connection options that allow electrical contact with the porous body to supply electrical energy or allow the medium (especially fluids) to be supplied and / or discharged are difficult, for example, in the case of electric heating elements or heat exchangers, where connection with a porous body is required.
[0004] It is known to attach open-cell foam to frames or other components using shape-locking methods. However, permanent connections present problems because supports in the connection area may break due to mechanical stress. These issues are also not adequately addressed when using single or additional integral joints. Weak points or interfaces at the joints can arise due to welding, brazing, or bonding, potentially leading to joint failure.
[0005] Therefore, the object of the present invention is to provide options for increasing the stability of opening components, and / or to provide options for connection with opening structures, through which the safe and permanent supply or discharge of media or energy can be achieved. Summary of the Invention
[0006] According to the invention, this objective is achieved by a method having the features of the invention. The invention defines accordingly manufactured components.
[0007] When manufacturing the open-cell metal and / or ceramic component, which comprises at least three adjacent volume regions with different porosities, the process involves first preparing a semi-finished product having an open-cell structure, comprising an open-cell foam made of a polymer material, in a manner known per se. At the surface of the foam pillars, the polymer material is coated with a metallic coating or a coating formed of metal or ceramic particles in a manner that preserves the open-cell basic structure. This can be achieved, for example, by CVD or PVD methods known per se, electroplating, or according to the so-called Schwartzwalder method, in which the pillars are coated with a coating containing metal or ceramic particles. The semi-finished product obtained by the Schwartzwalder method should be dried to achieve sufficient green strength before further processing. Relevant known methods are described, for example, in US3090094B or US3111396B.
[0008] Preferably, a preform of mesh-like open-cell polyurethane foam is used as the open-cell foam formed from the polymer material. For this purpose, the cell sizes used can cover the entire range of mesh foams commercially classified according to pore size per inch (according to ASTM D3576-77), from 8 ppi to 100 ppi, but it is advantageous to use coarser foams in the range of 8 ppi to 30 ppi. The ppi values can be easily converted to pore size in mm using optical radiography or computed tomography.
[0009] However, other open-cell structures formed from polymers, such as nonwoven fabrics or mesh structures produced by additive manufacturing processes, can also be used.
[0010] The suspension, composed of metal or ceramic particles, liquid, and polymer binder, comes into contact with the surface of the foam and contains air bubbles previously formed in the suspension. A predetermined shape is then formed on a predetermined surface area of the resulting semi-finished product. During this process, a portion of the suspension permeates into openings in the edge layer region of the foam, which is the semi-finished product.
[0011] Then, a drying process is carried out using heat treatment, in which the liquid contained in the suspension is first drained, and then or simultaneously the polymer components are removed, especially the polymer components of the binder and the polymer material of the foam, followed by a sintering process.
[0012] During sintering, a first volume region is formed from a metal or ceramic material derived from the suspension, having a smaller porosity than the semi-finished product, its porosity being solely due to the presence of air bubbles in the suspension. Adjacent to this first volume region is a second volume region, which is also porous or may be porous. This second volume region is formed from a coating of metal or ceramic from the support structure of the semi-finished product and from the metal or ceramic of the suspension, wherein these metals and / or ceramics are integrally and shape-locked together within the second volume region. As a result, in the edge layer region forming the third volume region, the second volume region connects the first volume region to the metal or ceramic open-cell structure of the third volume region derived from the openings of the coated foam, the third volume region having a larger porosity than the first volume region.
[0013] The suspension used to generate the first and second volume regions of the component can be manufactured in a manner known per se. For this purpose, a suitable liquid comprising at least one polymer binder and a proportion of metal or ceramic powdered solid can be used. Air bubbles can be introduced into the suspension by mechanical stirring or by other methods, such as those known from DE102010039322A1. Other gases or gas mixtures besides air can also be used, which may also exhibit inertness, thus preventing any adverse effects on the specific metal or ceramic of the final formed component.
[0014] Typically, binders already used in such suspensions, such as polyvinyl alcohol, can be used as polymer binders. In any case, the use of defoamers should be avoided. Preferably, water can be used as the liquid. However, other liquids are also suitable, preferably those with a lower boiling point than water.
[0015] Preferably, a suspension with a viscosity of at least 0.1 mPas should be used to generate the first and second volume regions. Furthermore, the suspension should preferably have shear-thinning flow characteristics with a pronounced flow limit. Alone or additionally, air bubbles should be present in the suspension, with a bubble volume percentage of at least 5% to a maximum of 50% of the total suspension volume.
[0016] Advantageously, the support of the semi-finished product should be coated with the same metal or ceramic as the metal or ceramic used to form the suspension for generating the first and second volume regions. This can be a pure metal of a chemical element or a corresponding alloy. If an alloy is used, the alloy composition of the coating of the semi-finished product can differ from the alloy composition of the particles used for the suspension.
[0017] However, different materials can be used for the coating of the pillars of the semi-finished product and the suspension used to form the first and second volume regions. The coefficients of thermal expansion of the materials should be on the same order of magnitude, and their thermal behavior according to the sintering temperature should be similar. This is the case, for example, when stainless steel and zirconia ceramics are used. In this respect, the term "similar" should be understood as a deviation of less than 10% between them. When the sintering temperatures and coefficients of thermal expansion of different materials make this possible, the second volume region can be formed by a combination of metallic and ceramic materials.
[0018] The suspension used to form the first and second volume regions can be added to at least one recess, depression, or perforation formed on the semi-finished product before heat treatment (during which the part can be finally completed), and / or added to the interior of a molding tool that can be attached to a particular semi-finished product. For example, this can thus reinforce certain surface or edge layer areas of a particular part, or establish a connection there. The molding tool can be temporarily attached to the semi-finished product, or the semi-finished product can be inserted into a frame-shaped molding tool, such that a suspension containing air bubbles can be added to at least one gap between the surface of the semi-finished product and the inner wall of the particular molding tool, so that the first volume region can be created there, and a second volume region directly adjacent to the first volume region can be created due to the suspension penetrating into the openings of the semi-finished product.
[0019] For this purpose, the molding tool can completely surround the semi-finished product. Alternatively, the molding tool can be fixed to a sub-area of the semi-finished product's surface, and then a suspension can be added to the gap or cavity between the semi-finished product's surface and the inner wall of the molding tool. In this way, for example, a hollow profile with a circular or angular cross-section that can surround the semi-finished product can be used as the molding tool. However, a corresponding segment of such a profile, such as a circular segment, can also be used as the molding tool.
[0020] Demolding can be performed before heat treatment or only after sintering is complete.
[0021] The penetration depth of the suspension into the pores of the semi-finished product from its surface can be influenced by externally applied forces, thereby intentionally affecting the thickness or width of the edge layer region forming the second volumetric region. The thickness or width should be at least 3 mm from the surface of the semi-finished product inwards. As already proposed, this thickness or width can also be chosen to be smaller or larger. However, it should be large enough that the three volumetric regions can bond to each other with sufficient strength and that sharp interfaces between the first and third volumetric regions can be avoided to the greatest extent possible. The required thickness or width can be based on the cell width or pore diameter of the semi-finished product and should be at least three times the cell size or pore diameter of the semi-finished product.
[0022] For this purpose, the semi-finished product itself, or a semi-finished product with a molding tool attached thereto, can be vibrated during the process, and / or pressure can be applied to the suspension. In this way, a medium (gas or liquid) at an increased pressure compared to ambient pressure can be used, where the higher pressure acts on the surface of the suspension, pushing the suspension into openings in the semi-finished product. To use vibration for this purpose, a vibration table can be used, on which the semi-finished product comprising the suspension and possibly at least one molding tool can be placed. Depending on the amplitude and duration of the vibration, the width or thickness of the second volume region can be affected. This can also be achieved by a vibrator coupled to the molding tool or the semi-finished product.
[0023] Semi-finished products with a porosity in the range of 60% to 95% can be used, and / or suspensions can be used to form a first volume region and / or a second volume region with a porosity in the range of 0% to 55% at the component.
[0024] Advantageously, corrosion-resistant FeCrAl alloys can be used as metals. Both oxide and non-oxide ceramics can be used as ceramic materials.
[0025] The component manufactured according to the invention includes a first volume region formed of a metal or ceramic derived from a suspension. The first volume region has a smaller porosity than a third volume region formed by an open structure of a semi-finished metal or ceramic support, wherein the first volume region is formed solely of a metal or ceramic derived from a suspension containing air bubbles. The porosity is determined by the number and size of the air bubbles present in the suspension. Adjacent to the first volume region is a second volume region, which may also be porous but can be dense. The second volume region is formed of a coated metal and / or ceramic from a semi-finished support and a metal or ceramic from the suspension, wherein these metals and / or ceramics are integrally and shape-locked together. Consequently, the second volume region connects to an open metal or ceramic open structure of an open third volume region derived from the coated semi-finished product and having a larger porosity than the first volume region.
[0026] The third volume region should have a porosity of at least 65%, and the porosity of the second volume region arranged between the first and third volume regions should be less than the porosity of the first and third volume regions of the component.
[0027] Multiple first volume regions and second volume regions may exist at the component, and these first volume regions and second volume regions are arranged spaced apart from each other.
[0028] At least one connector for supplying electrical energy or for removing media from components can be created using at least a first volume region, which can be accessed externally. In this way, it can represent a connector used as an electrical contact for a resistance heating element. In the case of a resistance heating element, it is advantageous that the first volume region has sufficiently high strength. The first volume region can be connected to a third volume region in a form-locked and integral manner via a second volume region, and the third volume region enables improved heating, particularly due to its large specific surface area.
[0029] By utilizing the first volume region and the second volume region, areas can also be formed on the component that can perform the pin function for anchoring elements (such as screws).
[0030] When the first and second volume regions are circumferentially or at least partially circumferentially formed around the outer edge of the third volume region, a frame can be formed, and the perforated structure can be held and protected in the frame in a shape-locked and integral manner.
[0031] Furthermore, this invention can also be used to manufacture components for use in lightweight structures, automotive engineering, electrical engineering, and aerospace. Detailed Implementation
[0032] The invention will now be described in more detail based on embodiments.
[0033] Example 1
[0034] A metal foam board comprising two compact rectangular direct foam contacts is prepared as follows and used as a component. To manufacture this component, a board in the form of a rough rectangular metal foam with dimensions of 125mm × 75mm × 20mm is used as a semi-finished product. Two first volume regions are arranged on opposite sides, allowing a finished component with an overall square shape of 125mm × 125mm × 20mm to be obtained. The rough foam used as the semi-finished product has a cell width of approximately 4.5mm and a density of approximately 10% of the metal density of the semi-finished product. The two first volume regions, formed solely by suspension, achieve a sintering density of approximately 50%, and therein achieve an average pore size between 100µm and 1500µm and a porosity of 50%.
[0035] According to the molding method, a rough foam is produced as a semi-finished product by coating an open-cell polymer foam with a corresponding cell width using an extrusion-calendering method (Schwartzwalder method). For this purpose, FeCrAl metal powder with an average particle size of 7 µm is first stirred with a polymer binder (e.g., a polyvinyl alcohol formulation, commercially available from Zschimmer & Schwarz) and additives for defoaming and rheological property adjustment (e.g., a fatty alcohol formulation, Zschimmer & Schwarz) and water to obtain a suspension with a metal solids content of approximately 86%. The foam material is impregnated with this suspension and then extruded by calendering until the desired loading is achieved on the support surface of the foam structure. The coated and dried foam forms a semi-finished product and is subsequently inserted centrally into a separable molding tool, such that an edge with a width of 25 mm is retained on both sides between the inner wall of the molding tool and the surface of the semi-finished product in the area where a first volume region is to be additionally generated. The molding tool and the semi-finished product are placed on a vibrating plate.
[0036] The suspensions to be used to form the first and second volume regions are produced separately using a batch process. The base is formed from the same suspension composition made of metal powder, organic binder, and rheology additives, except that no defoamer is used here.
[0037] Instead, add up to 5% by mass of a surfactant (e.g., a fatty alcohol sulfate formulation, Zschimmer & Schwarz) as a foaming agent. Foam the mixture in a beaker at 1000 rpm for 10 minutes, seeking an approximately 50% volume increase.
[0038] The foaming suspension, in which the air bubbles are distributed as evenly as possible, is then added to the free edge region between the inner wall of the molding tool and the surface of the semi-finished product using a spatula. The flow behavior of the resulting foamed suspension is adjusted so that it flows freely when the molding tool is gently vibrated by a vibrating plate, but remains in place when not moved by external force. In this way, the penetration of the air-bubble-containing suspension into the pores of the rough metal foam forming the semi-finished product can be controlled, and a combination area of 1 to 2 pore levels (approximately 4.5 mm to 9 mm) can be adjusted as a second volume region. After the edge region of the semi-finished product where the second volume region will be generated has been filled, a drying process is carried out at approximately 40°C for approximately 24 hours, after which the molding tool can be removed. For this purpose, it is recommended to use a molding tool composed of multiple separable individual parts, wherein separable molding tools are generally preferred. After the drying process, a debinding step is performed to remove organic components, and then the metal is sintered. A component can be manufactured comprising, on each of its opposite sides, an outwardly facing first volumetric region, the porosity of which is less than that of a third volumetric region, the porosity of which is predetermined by the porosity of a semi-finished product. A second volumetric region is formed between the first and third volumetric regions, the first and third volumetric regions being connected via the second volumetric region in a form-locked and integral manner, and the second volumetric region having no porosity or having a porosity smaller than that of the first volumetric region. A connector for electrical contact can be created using the first volumetric region. All three volumetric regions are formed using the same metal.
[0039] Example 2
[0040] As an alternative to metal components, ceramic components will be produced according to the same principle. For this purpose, a water-based ceramic suspension is prepared. This suspension has a bimodal SiC particle size distribution prepared by mixing SiC powders with average particle sizes of 0.8 µm and 3.0 µm in a 70:30 ratio, and additionally contains 0.6% boron (carbide) and 11% water-soluble polysaccharide (corresponding to 4% carbon after pyrolysis) as sintering additives. The suspension is adjusted to a solids content of 78%.
[0041] To prepare the foam ceramic, a polyurethane foam material with a cell width of 30 ppi (pores per inch) is impregnated with a suspension, and then excess suspension is removed using a centrifuge. As an example, a 200mm × 250mm × 10mm board is used as a semi-finished product, having two symmetrically arranged rectangular recesses of 20mm × 50mm at its outer edge. A foamed suspension is added to these recesses, which represent cavities similar to the interior of a molding tool, to create a tighter contact bond. The recesses can be introduced into the foam body, for example, by laser or waterjet cutting, which should preferably be done before coating the polymer foam to produce the semi-finished product.
[0042] Furthermore, the procedures and the consistency of the semi-finished products and suspensions are at least substantially the same as those in Example 1. In contrast to the preparation of the bubble-containing foaming suspension used in Example 1, air in the form of bubbles is introduced into the suspension via an apparatus, such as the one described in DE102010039322A1. The ceramic suspension used for impregnating the polymer foam is slightly modified by adding a plasticizer (e.g., polymeric polysaccharide, Zschimmer & Schwarz) in addition to the surfactant, which improves the processing properties of the suspension used to generate the first and second volume regions. The apparatus comprises a hollow steel cylinder 182 mm long, 70 mm in outer diameter, and 2.9 mm thick. This cylinder has an interface for a controlled compressed air supply. At the end face, the tube is provided with a metal disc with a concentric nozzle, which can also serve as a hose interface. The rear of the tube is also sealed with a metal disc having a through-hole with a diameter of 10 mm. A porous hollow cylinder is housed within a steel cylinder, clamped between two caps by a sealing ring, and has an outer diameter of approximately 25 mm and a wall thickness of approximately 2 mm. The tube, made of stainless steel, has a porosity of approximately 43%. An SMX series (SulzerChemtech AG) static mixer, approximately 20 mm in diameter, is located at the center of the tube. The metal powder suspension is guided through this porous inner tube with the static mixer, while being subjected to a pressure of approximately 0.3 MPa by compressed air at a volumetric flow rate of approximately 600 ml / min. As a result, uniform bubbles are generated in the suspension.
[0043] By turning the foaming device on and off, the foamed suspension can be added to the recesses that have been pre-formed on the semi-finished product. The thickness of the edge region forming the second volume region should be approximately 4 mm to achieve a shape-locked integral connection between the second and third volume regions after the sintering process.
[0044] Subsequently, the material is gently dried in a drying oven at 40°C for at least 12 hours. After drying, the polymer foam inside the support of volume 1 is burned off at 800°C under an inert gas atmosphere. The remaining SiC powder support is sintered at 2100°C under reduced pressure in an argon atmosphere, thereby obtaining a component made of SiC according to the invention.
Claims
1. A method for manufacturing porous metal and / or ceramic components, characterized in that, The component comprises at least three adjacent volume regions with different porosities, wherein The open-cell foam formed of polymer material has a metal coating or a coating formed of ceramic particles on the surface of the foam support in a manner that maintains the open-cell basic structure. as well as The suspension comes into contact with the surface of the foam body as a semi-finished product, and then forms a predetermined shape at a predetermined surface area of the resulting semi-finished product, wherein a portion of the suspension permeates the openings of the foam body as a semi-finished product in the edge layer region, wherein the suspension is formed using metal or ceramic particles, liquid and polymer binder and wherein previously formed bubbles are also present; and Then, a drying process using heat treatment is performed, in which the liquid contained in the suspension is discharged and the polymer components are removed, followed by a sintering process, wherein... During sintering, a first volume region is formed from metal or ceramic material derived from the suspension, the first volume region having a small porosity due only to the presence of air bubbles in the suspension, and a second volume region adjacent to the first volume region is generated. The second volume region is also porous and is formed from the metal or ceramic coating of the pillars of the semi-finished product and the metal or ceramic of the suspension. These metals and / or ceramics are integrally joined to each other in a shape-locked manner within the second volume region, thereby connecting the second volume region to the metal or ceramic open-cell structure of an open third volume region derived from the coated foam and having a larger porosity than the first volume region, wherein the second volume region has a smaller porosity than the first volume region.
2. The method according to claim 1, characterized in that, The foam formed from the polymer material used to produce the semi-finished product is coated with a suspension containing metal or ceramic particles at its pillars, or metal is coated by CVD, PVD, or electroplating. The semi-finished product obtained by coating with the suspension is dried before the suspension used to produce the first and second volume regions is applied thereon to obtain sufficiently high green strength to ensure that the coated pillars have sufficient strength to avoid damage when the surface areas come into contact with the suspension containing air bubbles.
3. The method according to claim 1 or 2, characterized in that, The pillar of the semi-finished product is coated with the same metal or ceramic as the metal or ceramic used to form the suspension for generating the first volume region and the second volume region.
4. The method according to claim 1, characterized in that, The first volume region and the second volume region are generated using a suspension in which air bubbles are present and the volume percentage of the air bubbles is 5% to 50% of the total volume of the suspension.
5. The method according to claim 1, characterized in that, The suspension is added to at least one recess or perforation formed on the semi-finished product, and / or added to the interior of a molding tool capable of being attached to the semi-finished product, to create the first volume region and the second volume region.
6. The method according to claim 1, characterized in that, The penetration depth of the suspension from the surface of the semi-finished product into the pores of the semi-finished product is affected by externally applied forces.
7. The method according to claim 6, characterized in that, The semi-finished product itself, or a semi-finished product with molding tools attached thereto, is subjected to vibration and / or pressure on the suspension during the process.
8. The method according to claim 1, characterized in that, The semi-finished product used has a porosity in the range of 60% to 95%, and / or the suspension is used to generate a first volume region and / or a second volume region on the component having a porosity in the range of 0% to 55%.
9. The method according to claim 1, characterized in that, The metal used is an FeCrAl alloy.
10. A component manufactured using the method according to any one of claims 1 to 9, characterized in that, A first volume region is formed from a metal or ceramic material derived from the suspension, having a small porosity due solely to the presence of air bubbles in the suspension. Adjacent to the first volume region is a second volume region, which is also porous, formed from a metal or ceramic coating of the pillars of the semi-finished product and a metal or ceramic of the suspension. These metals and / or ceramics are integrally joined to each other in a shape-locked manner, thereby connecting the second volume region to a metal or ceramic open-cell structure of the semi-finished product that forms a third volume region with a larger porosity than the first volume region, wherein the second volume region has a smaller porosity than the first volume region.
11. The component according to claim 10, characterized in that, The third volume region has a porosity of at least 65%, and the porosity of the second volume region disposed between the first volume region and the third volume region is less than the porosity of the first volume region and the third volume region of the component.
12. The component according to claim 10 or 11, characterized in that, At least one connector is created using the first volume area, which is capable of external access for electrical power or for supplying and / or removing media from the component.
13. The component according to claim 10, characterized in that, The component has multiple first volume regions and multiple second volume regions arranged at intervals from each other.
14. The component according to claim 10, characterized in that, The third volume region has a porosity in the range of 80% to 93%.
Citation Information
Patent Citations
Continuous production of foams, comprises introducing foaming material continuously, transporting material to be foamed and processing the back pressure of the porous hollow body wall and material to be foamed
DE102010039322A1
Method of making porous ceramic articles
US3090094A
Method of making a porous material
US3111396A
Open-cell ceramic and / or metal foams having a rough enveloping surface and a method for the production thereof
WO2010066648A1