An antibacterial stain-resistant film and a method of manufacturing the same
By introducing quaternary ammonium salt groups into the membrane structure, the problems of membrane susceptibility to bacterial adhesion and acidic environment have been solved, achieving highly efficient antibacterial and antifouling performance and improving the membrane's performance.
Patent Information
- Application Number
- CN202311059845.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-22
AI Technical Summary
Existing polymer membrane separation technologies are susceptible to bacterial adhesion and growth during operation, leading to decreased membrane flux and impaired separation performance, which limits their development in industrial applications.
Quaternary ammonium salts are introduced into the membrane structure, and then reacted with pyromellitic trimethylol chloride via an amino compound containing ammonium groups to form a polyamide filter membrane with quaternary ammonium salt groups, thereby improving the membrane's antibacterial and acid-resistant properties.
It improves the water flux and desalination rate of the membrane, while enhancing the membrane's antibacterial properties and acid resistance, reducing microbial adhesion, and extending the membrane's service life.
Smart Images

Figure CN117298874B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of water treatment membranes, specifically relating to an antibacterial and fouling-resistant membrane and its preparation method. Background Technology
[0002] Membrane separation technology boasts advantages such as high separation efficiency, small footprint, low energy consumption, and ease of operation, making it one of the most important methods in separation science. However, membrane fouling has consistently hindered the further development of polymer membrane separation technology. In particular, during operation, the adhesion and growth of bacteria in the feed solution on the membrane surface causes a sharp decline in membrane flux, damaging separation performance and limiting the application of membrane separation technology in many industries.
[0003] There are currently some reports on the antibacterial and antifouling modification of polymer separation membranes. For example, invention patent CN104524986A involves immersing a base membrane in a dopamine solution, utilizing the self-polymerization of dopamine to form a polydopamine layer on the surface of the base membrane, then reacting it with a polyethyleneimine aqueous solution, and finally undergoing a cationization reaction to obtain a hydrophilic antibacterial membrane. Invention patent CN104190274A uses polyvinylidene fluoride, silver ions, and zwitterionic monomers as main raw materials to prepare a silver nanoparticle zwitterionic polymer brush, which is grafted onto the surface of a polyvinylidene fluoride membrane to achieve antibacterial effects. Invention patent CN 108927018A prepares an antifouling and antibacterial forward osmosis membrane by immersing a polysulfone base membrane in a solution of m-phenylenediamine, trimesoyl chloride, polyethyleneimine, and nano-silver colloid.
[0004] Quaternary ammonium salts, as a class of broad-spectrum bactericides, are characterized by high efficiency, low toxicity, minimal susceptibility to pH changes, and stable chemical properties. Amphoteric polymers are polymers containing both positive and negative ion groups. They bind water molecules through electrostatic forces between these groups, forming a stable hydration layer that effectively prevents or reduces contact between membrane fouling substances and the membrane surface. Patent CN 112870990 A discloses an antibacterial and fouling-resistant reverse osmosis composite membrane, comprising a polyamide reverse osmosis membrane, an intermediate layer formed on the surface of the polyamide reverse osmosis membrane, and an antibacterial and fouling-resistant layer formed on the side of the intermediate layer facing away from the polyamide reverse osmosis membrane. Polyphenol monomers are used to improve the adhesion between the polyamide reverse osmosis membrane and the polyquaternary ammonium salt. However, this method involves surface coating and is prone to loss during subsequent operation. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide an antibacterial and antifouling membrane and its preparation method. By introducing quaternary ammonium salts into the membrane structure, the membrane effectively achieves the purpose of acid resistance, antibacterial and antifouling properties. At the same time, by using an amino compound containing an ammonium group as a reactant monomer to react with trimesoyl chloride, not only is the water flux and desalination rate of the membrane improved, but the acid resistance of the membrane is also enhanced.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A method for preparing an antibacterial and antifouling membrane includes the following steps:
[0008] S1. Immerse the support layer membrane in an aqueous solution with pH > 10, and remove it to remove excess solution;
[0009] S2. Coat the oil phase solution on one side of the membrane in step S1 to form a separation layer by interfacial polymerization, and drain the residual solution from the surface.
[0010] S3. The membrane obtained in step S2 is treated with sulfuric acid solution, rinsed with water, and then immersed in glycerol solution for protection.
[0011] The aqueous phase solution consists of an amino compound monomer containing quaternary ammonium salt groups, camphor sulfonic acid, triethylamine, sodium hydroxide, nonylphenol polyoxyethylene ether, and water; the oil phase solution consists of pyromellitic trimethylol chloride, toluene, and naphtha.
[0012] The amino compound monomer containing quaternary ammonium salt groups in the aqueous phase is selected from any one of the following compounds having the following structures:
[0013]
[0014] Preferably, the aqueous phase solution comprises, by mass percentage: 0.8–2.0% amino compound monomer containing quaternary ammonium salt groups, 1.0–1.4% camphor sulfonic acid, 0.5–0.7% triethylamine, 0.28–0.70% sodium hydroxide, 0.08–0.12% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.18–0.22% trimesoyl chloride, 3–7% toluene, and the balance being naphtha.
[0015] This application utilizes the quaternization reaction of substrates containing tertiary amines and diamino groups with alkyl bromides to synthesize a series of ammonium-containing di(poly)amino compounds. In this synthetic route, the two primary amino groups in di(aminoethyl)amine form a Schiff base with benzaldehyde under basic conditions, thus protecting the amino group. By adding excess bromoethane, a quaternary ammonium group is formed, and after deprotection of the amino group under acidic conditions, a diamino compound containing an ammonium group is obtained. Using the same method, tri(2-aminoethyl)amine, linear polyethyleneamine, and dendritic polyethyleneamine as substrates, corresponding amino-containing quaternary ammonium salt compounds can be obtained. The specific reactions are shown in the following equations:
[0016]
[0017] Two (or more) amino groups in a compound containing a quaternary ammonium salt group can undergo an amidation reaction with an acyl chloride. The synthesized amino compound containing a quaternary ammonium salt group is reacted with trimesoyl chloride to prepare an ammonium-functionalized polyamide filter membrane.
[0018] Preferably, the support layer membrane in step S1 is one of polysulfone, polyethersulfone, and polyethylene ultrafiltration membrane.
[0019] Preferably, the membrane in step S1 is immersed in the aqueous solution for 1 min to 2 min.
[0020] Preferably, in step S2, the oil phase solution is coated on one side of the membrane in step S1 for 10s to 30s.
[0021] Preferably, the concentration of the sulfuric acid solution in step S3 is 0.3% to 0.7%, and the treatment time is 1 min to 3 min.
[0022] Another object of the present invention is to provide an antibacterial and antifouling membrane prepared by the above method.
[0023] Preferably, the antibacterial agent targets bacteria of the genera Escherichia, Bacillus, and Pseudomonas.
[0024] The present invention also provides the application of the above-mentioned antibacterial and fouling-resistant membrane in water treatment, which can be applied to water treatment methods, water treatment elements or devices.
[0025] Preferably, the aqueous solution used in the water treatment is acidic.
[0026] Compared with the prior art, the beneficial effects of the present invention are reflected in:
[0027] This invention involves an amidation reaction between ammonium monomers and acyl chlorides, which imparts quaternary ammonium salt groups to the surface of the polymer membrane, making it unfavorable for microbial growth. Furthermore, the membrane's hydrophilicity decreases, making it difficult for microorganisms to adhere, thus improving its antibacterial properties. At the same time, the membrane's acid resistance is significantly enhanced. Attached Figure Description
[0028] Figure 1 This is a schematic diagram illustrating the synthesis of the antibacterial and antifouling nanofiltration membrane of the present invention.
[0029] Figure 2 The images show the effects of nanofiltration membranes prepared in the embodiments and comparative examples of this invention on the growth of three bacterial solutions.
[0030] Figure 3 The images show the morphology of blank membranes and membranes after culturing different bacterial solutions, as well as comparative examples. Detailed Implementation
[0031] The present invention will be described in detail below with reference to specific embodiments, but this does not limit the scope of the invention. It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.
[0032] Unless otherwise specified in the examples, preparations were carried out under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0033] The linear polyethyleneamine and dendritic polyethyleneamine used in the embodiments of the present invention have the following structural formulas:
[0034]
[0035] Linear polyethyleneamine, dendritic polyethyleneamine
[0036] Example 1
[0037] An antibacterial and antifouling membrane is prepared by the following steps:
[0038] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0039] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0040] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0041] The aqueous phase solution comprises, by mass percentage: 1.4% tris(2-aminoethyl)amine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic methyl chloride, 5% toluene, and the balance being naphtha.
[0042] Example 2
[0043] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0044] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0045] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0046] The aqueous phase solution comprises, by mass percentage: 0.8% tris(2-aminoethyl)amine, 1.0% camphor sulfonic acid, 0.5% triethylamine, 0.28% sodium hydroxide, 0.08% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.18% pyromellitic acid chloride, 3% toluene, and the balance being naphtha.
[0047] Example 3
[0048] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0049] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0050] S3. The membrane obtained in step S2 is treated with 0.7% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0051] The aqueous phase solution comprises, by mass percentage: 2.0% tris(2-aminoethyl)amine, 1.4% camphor sulfonic acid, 0.7% triethylamine, 0.7% sodium hydroxide, 0.12% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.22% pyromellitic methyl chloride, 7% toluene, and the balance being naphtha.
[0052] Example 4
[0053] S1. Immerse the polysulfone support layer film in an aqueous solution with pH 11 for 2 minutes, then remove it and use a rubber roller to remove excess solution.
[0054] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 30 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0055] S3. The membrane obtained in step S2 is treated with 0.7% sulfuric acid solution for 3 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0056] The aqueous phase solution comprises, by mass percentage: 1.4% tris(2-aminoethyl)amine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic methyl chloride, 5% toluene, and the balance being naphtha.
[0057] Example 5
[0058] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0059] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0060] S3. The membrane obtained in step S2 is treated with 0.7% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0061] The aqueous phase solution comprises, by mass percentage: 2.0% linear polyethyleneamine (Mw = 25000), 1.4% camphor sulfonic acid, 0.7% triethylamine, 0.7% sodium hydroxide, 0.12% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.22% pyromellitic acid chloride, 7% toluene, and the balance being naphtha.
[0062] Example 6
[0063] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0064] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0065] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0066] The aqueous phase solution comprises, by mass percentage: 1.4% dendritic polyethyleneamine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic trimethylol chloride, 5% toluene, and the balance being naphtha.
[0067] Comparative Example 1
[0068] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0069] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0070] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0071] The aqueous phase solution comprises, by mass percentage: 1.4% piperazine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic trimethylol chloride, 5% toluene, and the balance being naphtha.
[0072] Comparative Example 2
[0073] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0074] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0075] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0076] The aqueous phase solution comprises, by mass percentage: 0.4% tris(2-aminoethyl)amine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic methyl chloride, 5% toluene, and the balance being naphtha.
[0077] Comparative Example 3
[0078] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0079] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0080] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0081] The aqueous phase solution comprises, by mass percentage: 0.7% tris(2-aminoethyl)amine, 0.7% piperazine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic methyl chloride, 5% toluene, and the balance being naphtha.
[0082] Comparative Example 4
[0083] S1. Immerse the polysulfone support layer membrane in an aqueous solution with pH 11 for 1 minute, then remove it and use a rubber roller to remove excess solution.
[0084] S2. Coat the polysulfone side of the membrane in step S1 with the oil phase solution for 10 seconds to perform interfacial polymerization and form a separation layer. Drain the residual solution from the surface.
[0085] S3. The membrane obtained in step S2 is treated with 0.3% sulfuric acid solution for 1 min, rinsed with water for 2 min, and then immersed in glycerol solution for 1 min for protection.
[0086] The aqueous phase solution comprises, by mass percentage: 1.4% tris(2-aminoethyl)amine, 1.2% camphor sulfonic acid, 0.6% triethylamine, 0.49% sodium hydroxide, 0.1% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.2% pyromellitic acid chloride, 5% toluene, and the balance being ethylcyclohexane.
[0087] Experimental Example 1: Nanofiltration Performance Analysis
[0088] The water flux and desalination rate of the membrane prepared according to the embodiments and comparative examples of this invention were measured according to GB / T 34242-2017 Nanofiltration Membrane Test Method: magnesium sulfate and sodium chloride concentration 2000 mg / L, under the conditions of pressure 0.70 MPa and temperature 25℃. The water flux F and desalination rate R of the nanofiltration membrane were measured, and the water flux F was calculated using the following formula:
[0089] F = V / (A·t), where F is the water flux in L / (m³). 2 ·h), V is the volume of permeate collected in time t (L), and A is the effective membrane area of the nanofiltration membrane (m²). 2 ), where t is the time (h) used to collect volume V of permeate.
[0090] The desalination rate R is calculated using the following formula:
[0091] R = (Cf - Cp) / Cf × 100%, where R is the desalination rate, Cp is the ion content in the permeate (mg / L), and Cf is the ion content in the test solution (mg / L).
[0092] The test results are shown in Table 1.
[0093] Table 1
[0094]
[0095]
[0096] As shown in Table 1, the membranes prepared in Examples 1-6 exhibit significant overall nanofiltration performance, with high rejection rates for divalent ions and low rejection rates for monovalent ions. In Comparative Example 1, replacing quaternized ammonium salts with piperazine as the monomer resulted in decreased water flux and increased rejection rates for monovalent ions, failing to achieve effective separation. In Comparative Example 2, reducing the amount of quaternary ammonium salt monomer weakened the membrane performance. Comparative Examples 3 and 4 demonstrate that altering the aqueous and oil phase compositions could not achieve the superior performance of the nanofiltration membranes of this invention.
[0097] Acid Resistance Analysis of Experiment Example 2
[0098] Test method: The membranes prepared in the embodiments and comparative examples of the present invention were immersed in 10% sulfuric acid solution at room temperature, and then rinsed with pure water before testing.
[0099] The test results are shown in Table 2.
[0100] Table 2
[0101]
[0102]
[0103] Table 2 shows that the membranes prepared in Examples 1-6 exhibit significantly improved acid resistance, with no significant change in desalination rate after 7d / 28d soaking. In Comparative Example 1, piperazine was used instead of quaternized monomer, resulting in nanofiltration membranes with poor acid resistance; the membranes were damaged after soaking in acid solution, and their performance significantly decreased. In Comparative Example 2, reducing the amount of quaternary ammonium salt monomer weakened the acid resistance of the resulting membrane. Comparative Examples 3 and 4 demonstrate that changing the aqueous and oil phase compositions could not achieve the excellent acid resistance of the nanofiltration membranes of this invention.
[0104] Test Example 3 Antibacterial Performance Test
[0105] Test methods and procedures: The antibacterial effects of different membrane materials were investigated using three different bacteria: Escherichia coli, Bacillus pacificus H4, and Pseudomonas gessardii NL7. Strain H4 was a Gram-positive bacterium, while the other two were Gram-negative bacteria.
[0106] The membranes prepared in the embodiments and comparative examples of the present invention, namely, Example 6 (membrane 1), Comparative Example 1 (membrane 2), and Example 1 (membrane 3), were cut into 1cm x 1cm pieces and added to each well of a 24-well cell culture plate with 100μL of OD. 600 Different bacterial suspensions with a concentration of 0.5 μL and 1.9 mL of LB liquid medium were incubated at 30°C for 24 hours, and then the OD of the bacterial suspensions was measured. 600The value was adjusted, and excess bacterial culture was removed. Biofilm growth on the membrane was observed under a microscope and compared with membranes cultured without bacterial culture. The growth of biofilm on the membrane was quantitatively measured at a wavelength of 595 nm using crystal violet staining. A membrane without bacterial culture was used as a blank control to eliminate the adsorption of crystal violet by the membrane itself.
[0107] Results Analysis
[0108] After 24 hours of incubation, the growth of the three bacteria is as follows: Figure 2 As shown, Pseudomonas gessardii NL7 showed the best growth, followed by Bacillus pacificus H4, with all bacterial cultures having an OD of [missing information]. 600 Both values are greater than 0.5 and less than 2.0, indicating that the bacteria are in a normal growth state, meeting the conditions for membrane biofilm attachment, and that the membrane material has no significant effect on the growth of free bacteria.
[0109] The crystal violet staining results are shown in Table 3; the smaller the value, the less biofilm there is. Membrane 1 showed the best antibacterial effect, while membrane 2 showed the worst. Membranes 1 and 3 themselves have a certain adsorption capacity for crystal violet.
[0110] Table 3
[0111]
[0112] Under the microscope, the morphology of the blank membrane and the membrane after different bacterial cultures are as follows: Figure 3 As shown, the membrane itself has many grooves. After bacterial culture, a small amount of bacterial culture accumulated on the membrane surface. The bacteria did not adhere well and no obvious biofilm formed, but there was some aggregation in the grooves of the membrane. It can be seen that the coverage of the antibacterial coating on the membrane directly affects the aggregation of biofilm on the membrane surface.
[0113] Experimental Example 4: Pollution Resistance
[0114] The membrane sheets from Example 1 and Comparative Example 1 were rolled into membrane elements, and sodium alginate was used as a pollutant source for treatment. The flux decline of the membrane elements was tested. After one month of continuous operation, the flux of Example 1 decreased by 10.6%, and the flux of Comparative Example 1 decreased by 30.8%.
[0115] The above embodiments of the present invention are merely examples to clearly illustrate the technical solutions of the present invention, and are not intended to limit the specific implementation of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the claims of the present invention should be included within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an antibacterial and stain-resistant membrane, characterized in that, Includes the following steps: S1. Immerse the support layer membrane in an aqueous solution with pH > 10, and remove it to remove excess solution; S2. Coat the oil phase solution on one side of the membrane in step S1 to form a separation layer by interfacial polymerization, and drain the residual solution from the surface. S3. The membrane obtained in step S2 is treated with sulfuric acid solution, rinsed with water, and then immersed in glycerol solution for protection. The aqueous phase solution consists of an amino compound monomer containing quaternary ammonium salt groups, camphor sulfonic acid, triethylamine, sodium hydroxide, nonylphenol polyoxyethylene ether, and water; the oil phase solution consists of pyromellitic trimethylol chloride, toluene, and naphtha. The amino compound monomer containing quaternary ammonium salt groups in the aqueous phase is selected from one of the compounds having the following structures: 、 、 ; The aqueous phase solution comprises, by mass percentage: 0.8%~2% amino compound monomers containing quaternary ammonium groups, 1.0%~1.4% camphor sulfonic acid, 0.5%~0.7% triethylamine, 0.28%~0.70% sodium hydroxide, 0.08%~0.12% nonylphenol polyoxyethylene ether, and the balance being water; the oil phase solution comprises, by mass percentage: 0.18%~0.22% trimesoyl chloride, 3%~7% toluene, and the balance being naphtha.
2. The method for preparing an antibacterial and antifouling membrane according to claim 1, characterized in that, The support layer membrane in step S1 is one of polysulfone, polyethersulfone, or polyethylene ultrafiltration membrane.
3. The method for preparing an antibacterial and stain-resistant membrane according to claim 1, characterized in that, In step S1, the membrane is immersed in an aqueous solution for 1 to 2 minutes.
4. The method for preparing an antibacterial and stain-resistant membrane according to claim 1, characterized in that, Step S2: Immerse the membrane in the oil phase solution for 10s~30s.
5. The method for preparing an antibacterial and stain-resistant membrane according to claim 1, characterized in that, The sulfuric acid solution concentration in step S3 is 0.3%~0.7%, and the treatment time is 1min~3min.
6. An antibacterial and antifouling membrane prepared by the method according to any one of claims 1-5.
7. The antibacterial and stain-resistant membrane according to claim 6, characterized in that, The antibacterial agents target bacteria of the genera Escherichia, Bacillus, and Pseudomonas.
8. The application of the antibacterial and fouling-resistant membrane according to claim 6 in acidic water treatment.
Citation Information
Patent Citations
Antibacterial polyvinylidene fluoride membrane and preparation method thereof
CN104190274A
Preparation method of hydrophilic antimicrobial film of which surface is coated with dopamine and polyethyleneimine cations
CN104524986A
Fouling-resistant antibacterial composite forward-osmosis membrane with positive surface charges and preparation method therefor
CN108927018A
Antibacterial and pollution-resistant reverse osmosis composite membrane and preparation method thereof
CN112870990A
Preparation method of composite nanofiltration membrane and composite nanofiltration membrane
CN115703046A