Hydrogel based on radical polymerization and method for preparing the same

Interpenetrating network hydrogels were prepared by free radical polymerization, which solved the problem of the need for cross-linking agents in the preparation of existing hydrogels. This resulted in hydrogels with high mechanical strength and self-healing properties, suitable for temporary abdominal closure materials, and improved treatment efficacy.

CN117304517BActive Publication Date: 2026-11-20NINGXIA HUI AUTONOMOUS REGION PEOPLES HOSPITAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311420448.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-20
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Existing hydrogels require the addition of cross-linking agents during preparation, which leads to side effects and insufficient mechanical strength, making it difficult to meet the needs of temporary abdominal closure materials.

Method used

An interpenetrating network hydrogel is formed by copolymerizing 3-acryloylaminophenylboronic acid, acrylic acid, and sodium alginate using a free radical polymerization method, avoiding the use of traditional crosslinking agents and enhancing mechanical properties and self-healing ability.

Benefits of technology

The prepared hydrogel possesses excellent mechanical properties, water absorption properties, self-healing properties, and adhesive properties, making it suitable as a temporary abdominal closure material, reducing side effects, and improving treatment efficacy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004520932360000011
    Figure HDA0004520932360000011
  • Figure HDA0004520932360000012
    Figure HDA0004520932360000012
  • Figure HDA0004520932360000021
    Figure HDA0004520932360000021
Patent Text Reader

Abstract

A hydrogel based on radical polymerization and a preparation method thereof belong to the technical field of biomedical materials, and the preparation method comprises the following steps: (1) dissolving sodium alginate, acrylic acid, 3-acrylamido phenyl boronic acid and acrylic acid-N-succinimide in deionized water to obtain a precursor solution; (2) adding an initiator to the precursor solution, stirring and ultrasonic degassing to obtain a pre-polymer solution with a pH value of 2-2.2; and (3) solidifying the pre-polymer solution to obtain the multifunctional hydrogel. In the absence of a traditional crosslinking agent N,N-methylene bisacrylamide (MBAA), the 3-acrylamido phenyl boronic acid (AAPBA), acrylic acid (AAC) and sodium alginate (SA) with double bonds are formed into a hydrogel material with certain mechanical properties, water absorption properties, self-healing and adhesion properties by using a one-pot method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomedical materials technology, specifically relating to a hydrogel based on free radical polymerization and its preparation method. Background Technology

[0002] Postoperative intestinal leakage and complicated abdominal infection are expensive to treat, with a mortality rate of 20-60%. Open abdominal surgery (OA) involves actively opening the abdominal cavity without suturing the incision after damage control surgery, allowing organ function to recover before closure. This method effectively reduces intra-abdominal pressure, facilitates the removal of infected and necrotic tissue, and allows for timely detection and treatment of intra-abdominal organ damage, aligning with damage control principles. It has become an important clinical treatment for severe abdominal infections, intra-abdominal hypertension, and severe abdominal trauma. However, open abdominal surgery can lead to abdominal wall dysfunction, electrolyte loss, and lack of skin exposure of the intestines, potentially causing new intestinal air leaks, severely impacting treatment outcomes and threatening life. Clinically, temporary abdominal closure is necessary without increasing intra-abdominal pressure or damaging organ function. Due to the complexity of the wound caused by intestinal leakage and complicated abdominal infection, existing temporary closure materials are not entirely effective.

[0003] Hydrogels are three-dimensional network materials formed by chemical or physical cross-linking of hydrophilic polymers. They have a high water content, can absorb large amounts of water without dissolving, and possess physical properties similar to the cell matrix. Due to their excellent biocompatibility with tissues, hydrogels can provide a cell growth environment, mimicking human tissue structures and exhibiting high biomimetic properties. In clinical practice, hydrogels are frequently used for tissue repair, not only providing mechanical support for filling defects but also possessing adhesive, rheological, and exudate-absorbing properties, enabling tissue repair and reconstruction. Therefore, their preparation and application in temporary peritoneal opening materials have attracted widespread attention.

[0004] However, existing hydrogel technologies require the addition of cross-linking agents to form a porous structure during preparation. These cross-linking agents have certain side effects on the body, are not easily degraded, and are detrimental to the environment. Furthermore, simple chemical cross-linking cannot provide sufficient mechanical strength, resulting in hydrogels with generally low toughness and low ductility. Therefore, there is an urgent need to develop a novel hydrogel material to provide a feasible solution for the design of temporary abdominal closure materials for intestinal leaks and abdominal infection wounds. Summary of the Invention

[0005] In view of this, the present invention provides a method for preparing hydrogels based on free radical polymerization, which can successfully prepare hydrogel materials without the addition of crosslinking agents.

[0006] The present invention also provides a hydrogel based on free radical polymerization, which has certain mechanical properties, water absorption properties, self-healing properties and adhesion properties.

[0007] The technical solution adopted by this invention to solve its technical problem is as follows: A method for preparing a hydrogel based on free radical polymerization includes the following steps: (1) Sodium alginate, acrylic acid, 3-acryloylaminophenylboronic acid, and N-succinimide acrylate were dissolved in deionized water to obtain a precursor solution; (2) An initiator is added to the precursor solution to initiate a free radical polymerization reaction. After stirring and ultrasonic degassing, a prepolymer solution with a pH of 2-2.2 is obtained. (3) The prepolymer solution is solidified to obtain the hydrogel.

[0008] Furthermore, the process also includes enhancing the hydrogel obtained in step (3). The specific steps of the enhancement process are as follows: the hydrogel is evaporated and dried to form a hydrogel film, and then immersed in a PBS solution with a pH of 7.3-7.5 until the length of the hydrogel returns to the length before drying.

[0009] Furthermore, in the prepolymer solution, the mass fraction of acrylic acid is 15%-30%, the mass fraction of sodium alginate is 0.5%-3%, the mass fraction of 3-acryloylaminophenylboronic acid is 0.5%-3%, the mass fraction of acrylic acid-N-succinimide is 1%, the mass fraction of initiator is 0.2%, and the remainder is deionized water.

[0010] Furthermore, in the prepolymer solution, the mass fraction of acrylic acid is 20%, the mass fraction of sodium alginate is 1%, the mass fraction of 3-acryloylaminophenylboronic acid is 1%, the mass fraction of acrylic-N-succinimide is 1%, the mass fraction of initiator is 0.2%, and the remainder is deionized water.

[0011] Furthermore, the initiator is α-ketoglutaric acid.

[0012] Furthermore, the ultrasonic degassing time is 20-30 minutes.

[0013] Furthermore, the specific operation of the curing is as follows: pour the prepolymer solution into a mold and irradiate it under ultraviolet light for 90-100 minutes.

[0014] A hydrogel based on free radical polymerization was prepared using the method described above.

[0015] This invention provides a hydrogel based on free radical polymerization and its preparation method. Compared with existing technologies, its advantages are as follows: This invention, without adding the traditional crosslinking agent N,N-methylenebisacrylamide (MBAA), uses a "one-pot" method to form a hydrogel with certain mechanical properties, water absorption properties, self-healing properties, and adhesive properties through free radical polymerization of 3-acryloylaminophenylboronic acid (AAPBA), acrylic acid (AAC), and sodium alginate (SA), which have double bonds. During the reaction, AAC, AAPBA, and AAC-NHS ester undergo free radical polymerization under the action of an initiator. AAPBA, as a monomer, undergoes free radical polymerization with AAC to form a long polymer chain P (AAC-AAPBA). When SA is added to the system, the short-chain SA and the long polymer chain form an interpenetrating network hydrogel through hydrogen bonding and chain entanglement, transforming the hydrogel from a linear material with a single network to a double network. This provides effective energy dissipation and extensibility, thereby improving the strain and toughness of the hydrogel. Attached Figure Description

[0016] Figure 1 This is a SEM image of the hydrogel prepared in Example 1.

[0017] Figure 2 These are the mechanical property test results of the hydrogels prepared in Example 1 and Comparative Examples 1-2.

[0018] Figure 3 This is a self-healing demonstration diagram of the hydrogel prepared in Example 1.

[0019] Figure 4 This refers to the self-healing efficiency of the hydrogel prepared in Example 1.

[0020] Figure 5 This is a schematic diagram of the adhesion between the hydrogel prepared in Example 1 and different substrates.

[0021] Figure 6 This is an SEM image of the hydrogel prepared in Example 2.

[0022] Figure 7 These are the mechanical property test results of the hydrogel prepared in Example 2.

[0023] Figure 8 This is a self-healing demonstration diagram of the hydrogel prepared in Example 2.

[0024] Figure 9 The amplitude scanning results are those of the hydrogel prepared in Example 2.

[0025] Figure 10 These are the results of the overlap and shear adhesion test of the hydrogel prepared in Example 2.

[0026] Figure 11The diode light emission states of the hydrogel prepared in Example 2 are shown when it is broken, healed, stretched after healing, and when the hydrogel participates in a closed circuit.

[0027] Figure 12 The results are the cytotoxicity (NIH3T3) results of the hydrogel prepared in Example 2.

[0028] Figure 13 The results are the live / dead cell staining (NIH3T3) results of the hydrogel prepared in Example 2. Detailed Implementation

[0029] The technical solutions and effects of the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0030] This invention provides a method for preparing hydrogels based on free radical polymerization, comprising the following steps: (1) Sodium alginate, acrylic acid, 3-acryloylaminophenylboronic acid, and N-succinimide acrylate were dissolved in deionized water to obtain a precursor solution; (2) An initiator is added to the precursor solution to initiate a free radical polymerization reaction. After stirring and ultrasonic degassing, a prepolymer solution with a pH of 2-2.2 is obtained. (3) The prepolymer solution is solidified to obtain the hydrogel.

[0031] This invention utilizes a one-pot method to polymerize 3-acryloylaminophenylboronic acid (AAPBA), acrylic acid (AAC), and sodium alginate (SA) with double bonds via free radical polymerization, without the addition of the traditional crosslinking agent N,N-methylenebisacrylamide (MBAA), to form a hydrogel with certain mechanical properties, water absorption, self-healing, and adhesive properties. During the reaction, AAC, AAPBA, and AAC-NHS ester undergo free radical polymerization under the action of an initiator. AAPBA, as a monomer, polymerizes with AAC to form a long polymer chain. When SA is added to the system, the short-chain SA forms an interpenetrating network hydrogel with the long polymer chain through hydrogen bonding and chain entanglement. This transforms the hydrogel from a linear material with a single network to a dual network, providing effective energy dissipation and ductility, thereby improving the strain and toughness of the hydrogel.

[0032] Furthermore, the pH value of the prepolymer solution is 2-2.2. On the one hand, under low pH conditions, due to weak hydrogen bonding and easily hydrolyzed borate ester bonds, the crosslinking density of the hydrogel is relatively low, which increases its swelling ratio at swelling equilibrium, thus giving it excellent ability to absorb exudate. On the other hand, under low pH conditions, the solution viscosity is low, which is more conducive to operation during transfer and solidification, and is less likely to generate bubbles.

[0033] Furthermore, the process also includes enhancing the hydrogel obtained in step (3). The specific steps of the enhancement process are as follows: the hydrogel is evaporated and dried to form a hydrogel film, and then immersed in a PBS solution with a pH of 7.3-7.5 until the length of the hydrogel is restored to the length before drying.

[0034] The prepolymer solution exhibits protonation and instability of borate ester bonds under low pH conditions, which negatively impacts its mechanical properties. Therefore, this invention addresses this issue by drying the hydrogel to form a thin film, then immersing it in PBS solution until the hydrogel's length returns to its pre-drying length and the pH reaches approximately 7.4, without increasing the viscosity of the prepolymer solution. Immersion in PBS enhances hydrogen bonding in the hydrogel and promotes the formation of more stable borate ester bonds, resulting in excellent self-healing and rheological properties.

[0035] Furthermore, in the prepolymer solution, the mass fraction of acrylic acid is 15%-30%, the mass fraction of sodium alginate is 0.5%-3%, the mass fraction of 3-acryloylaminophenylboronic acid is 0.5%-3%, the mass fraction of acrylic acid-N-succinimide is 1%, the mass fraction of initiator is 0.2%, and the remainder is deionized water.

[0036] Optimally, in the prepolymer solution, the mass fraction of acrylic acid is 20%, the mass fraction of sodium alginate is 1%, the mass fraction of 3-acryloylaminophenylboronic acid is 1%, the mass fraction of acrylic-N-succinimide is 1%, the mass fraction of initiator is 0.2%, and the remainder is deionized water.

[0037] Furthermore, the initiator is α-ketoglutaric acid.

[0038] Furthermore, the ultrasonic degassing time is 20-30 minutes.

[0039] Furthermore, the specific operation of the curing is as follows: pour the prepolymer solution into a mold and irradiate it under ultraviolet light for 90-100 minutes.

[0040] A hydrogel based on free radical polymerization was prepared using the method described above.

[0041] The following are preparation examples and comparative examples: Example 1

[0042] (1) At 50°C, sodium alginate was dissolved by heating and stirring with deionized water, and then acrylic acid, 3-acrylamide phenylboronic acid and acrylic-N-succinimide were added. The mixture was stirred thoroughly at room temperature until homogeneous to obtain the precursor solution. (2) Add an initiator to the precursor solution, stir and degas by sonication for 20 min to obtain a prepolymer solution with a pH of 2.1; (3) The prepolymer solution was poured into a mold made of two 150×75×2mm glass plates and a 3mm thick silicone pad, and irradiated under a 48W ultraviolet lamp for 90 minutes to obtain the hydrogel; named A20-S1-P1.

[0043] In the prepolymer solution, the mass fraction of acrylic acid is 20%, the mass fraction of sodium alginate is 1%, the mass fraction of 3-acryloylaminophenylboronic acid is 1%, the mass fraction of acrylic-N-succinimide is 1%, the mass fraction of initiator is 0.2%, the initiator is α-ketoglutaric acid, and the remainder is deionized water. Example 2

[0044] Hydrogels were prepared using the same polymerization method as in Example 1, except that the hydrogels obtained in step (3) were evaporated and dried to form a hydrogel film, which was then soaked in a PBS solution with a pH of 7.3-7.5 until the length of the hydrogel returned to its original length before drying. Example 3

[0045] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of 3-acryloylaminophenylboronic acid was 0.5%. Example 4

[0046] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of 3-acryloylaminophenylboronic acid was 3%. Example 5

[0047] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of sodium alginate was 0.5%. Example 6

[0048] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of sodium alginate was 3%. Example 7

[0049] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of acrylic acid was 15%. Example 8

[0050] The hydrogel was prepared using the same polymerization method as in Example 1, except that the mass fraction of acrylic acid was 30%.

[0051] Comparative Example 1 A20-P1 hydrogel was prepared using the same polymerization method as in Example 1, except that sodium alginate was not added, and the mass fractions of acrylic acid and 3-acryloylaminophenylboronic acid were 20% and 1%, respectively.

[0052] Comparative Example 2 A20-P1-M0.0058 hydrogel was prepared using the same polymerization method as in Example 1, except that sodium alginate was replaced with the traditional crosslinking agent N,N-methylenebisacrylamide (MBAA), wherein the mass fractions of acrylic acid, 3-acryloylaminophenylboronic acid, and N,N-methylenebisacrylamide were 20%, 1%, and 0.0058%, respectively.

[0053] The performance test results are as follows: The surface morphology of the hydrogel prepared in Example 1 was observed. See SEM results. Figure 1 The hydrogel exhibits a distinct and regular network structure in its cross-section, with pore sizes of approximately 10 μm. This highly porous structure provides excellent water absorption, which is fundamental for absorbing some exudate from open abdominal wounds. Furthermore, the complex layered porous structure enables extremely high efficiency and minimizes energy consumption for material transfer and exchange during cell metabolism, and provides space for cell attachment, growth, migration, secretion, invasion, differentiation, and vascularization.

[0054] The tensile properties of the hydrogels prepared in Example 1 and Examples 1-2 were tested. Before the experiment, rectangular strips with a length of 30 mm, a width of 10 mm, and a thickness of 3 mm were cut. The samples were clamped between the tensile fixtures of a universal testing machine. A 50 N sensor was used, and the hydrogel samples were stretched to fracture at a speed of 50 mm / min to analyze the tensile properties of the hydrogels. Then, stress versus strain was plotted. All samples were tested at least three times. The toughness of the hydrogel was calculated by integrating the area of ​​the stress-strain curve. The tensile stress (σ) is: σ = F / A; where F is the tensile load and A is the cross-sectional area. The tensile strain (ε) is: ε = (L - L0) / L 0 × 100%; the elongation ratio (λ) is: λ=L / L0, where L is the length after deformation and L0 is the original length.

[0055] See results. Figure 2In Comparative Example 1, without the addition of SA, the hydrogel forms a simple single-network linear hydrogel through free radical polymerization of AAC. Due to the low mechanical strength of the A20-P1 hydrogel, quantitative testing was not possible. After adding a small amount of the crosslinking agent MBAA to the precursor solution (Comparative Example 2), although the mechanical strength of the hydrogel improved, the fracture strain value was very small, approximately 40%, indicating low toughness. This is because although a small amount of crosslinking agent was added, the hydrogel was still composed of a simple linear polymer. When the hydrogel was subjected to external force, the long-chain network broke, resulting in poor ductility and thus poor toughness. When SA was added to the system, the hydrogen bonds and chain entanglements between the short-chain SA network and the long-chain polyacrylic acid network provided effective energy dissipation and ductility, thereby improving the strain and toughness of the hydrogel. When AAPBA was added to the system, the fracture stress of the AAC-SA-AAPBA (A20-S1-P1) hydrogel increased to 14.61 kPa, the fracture strain was 1420%, and the toughness was 143.8 kJ / m. 3 This indicates that AAPBA and AAC interact during copolymerization, giving the hydrogel good mechanical properties and improving its tensile strength. The toughness of A20-S1-P1 hydrogel is 23 times that of A20-P1-M0.0058 hydrogel and 3.8 times that of A20-S1 hydrogel.

[0056] The self-healing properties of the hydrogel prepared in Example 1 were analyzed. For example... Figure 3 As shown, the prepared A20-S1-P1 rectangular hydrogel was cut into two pieces, and two of the pieces were assembled together. Under no external stimuli, the hydrogel was able to self-heal. When the healed hydrogel was stretched, it could be seen that the hydrogel strip could be stretched without being destroyed, and after stretching, the two colors could be clearly observed to permeate each other at the cut. This indicates that the hydrogel can achieve self-healing at room temperature without any external stimuli.

[0057] The self-healing efficiency of the hydrogel prepared in Example 1 was tested. A rectangular sheet-like sample with a length of 30 mm, a width of 10 mm, and a thickness of 3 mm was cut in half with a knife. The cut surfaces were then allowed to heal without any external intervention. The healed sample was placed between the tensile clamps of a universal testing machine. By comparing the tensile strength of the hydrogel before and after healing, its self-healing efficiency can be characterized. The results are as follows: Figure 4As shown, this hydrogel, without external stimulation, completes repair within 3 minutes, and its tensile strength almost recovers to its original strength, with a self-healing efficiency approaching 91.4%. This is because AAPBA is in a non-dissociated state under low pH conditions, so the hydrogel is mainly formed through hydrogen bonding between SA and P (AAC-AAPBA); when the hydrogel heals, the reconstruction of hydrogen bond crosslinking points can be achieved within 3 minutes. In application, the self-healing hydrogel material can be cut open first, and pus can be drained using negative pressure assisted technology. Due to its excellent self-healing properties, the hydrogel material can self-repair, providing a possibility for timely drainage of pus in intestinal leaks and complex abdominal wounds, while also extending the protective period of the hydrogel material and expanding its application range.

[0058] The self-adhesive properties of the hydrogel prepared in Example 1 were analyzed. See the results below. Figure 5 As shown, the A20-S1-P1 hydrogel prepared by this invention possesses excellent self-adhesion and can directly adhere to materials such as polylactic acid, polypropylene, glass, polyester resin, polystyrene, and pigskin. The adhesion of this hydrogel to high-energy surfaces is due to the interaction between the carboxyl groups in the hydrogel and the active sites (such as hydroxyl groups) on the substrate surface. Adhesion to pigskin tissue is mainly achieved through the formation of covalent bonds between the carboxyl groups and the primary amine bonds between the carboxyl groups and the tissue, as well as interfacial hydrogen bonds. This excellent self-adhesion prevents detachment during use, expanding the application range of this hydrogel material in various fields.

[0059] The surface morphology of the hydrogel prepared in Example 2 was observed. See SEM results. Figure 6 The cross-sectional image of the hydrogel after PBS treatment shows that the hydrogel network ranges from loose and porous to smooth with fine filaments, which is due to the formation of stable borate ester bonds. The porous structure of the hydrogel also provides space for cell growth and has good water absorption properties.

[0060] The mechanical properties of the hydrogel prepared in Example 2 were tested. See the results below. Figure 7 , Figure 7(a) shows the stress-strain curve of A20-S1-P1 hydrogel after PBS treatment; (b) shows the corresponding fracture stress and toughness. It can be seen that by drying and then treating the A20-S1-P1 hydrogel with PBS, the hydrogel is restored to its original length before drying. At low pH, there are more free hydrogen ions, and these flexible free hydrogen ions combine with negatively charged atoms on the hydrogel, leading to a decrease in hydrogen bonds. When the pH of the hydrogel increases to 7.4, due to the enhanced hydrogen bonding and the stable existence of borate ester bonds, the fracture strain, fracture stress, and toughness of the hydrogel are significantly improved. Specifically, the fracture stress increases from 14.6 kPa to 48.6 kPa, the fracture strain from 1420% to 3016%, and the toughness increases from 143.8 kJ / m. 3 Rising to 858.6 kJ / m 3 The viscosity was increased by approximately 6 times. This indicates that the hydrogel treated with PBS not only exhibits good mechanical properties, but also facilitates the manipulation of the low viscosity of its precursor solution, avoiding difficulties such as degassing and transfer caused by high viscosity in large-scale production.

[0061] The self-healing properties of the hydrogel prepared in Example 2 were tested. Figure 8 This illustrates the self-healing process of hydrogel after PBS treatment. Figure 8 (a) Cutting; (b) Contact; (c) Healing; (d) Stretching. The prepared A20-S1-P1 hydrogel was first cut into two pieces, then the cut surfaces were placed together and left to stand for 24 hours without any external force. As shown in the figure, there is obvious color penetration at the contact surface, indicating that the two hydrogel pieces have re-fused together, achieving self-healing and withstanding a certain tensile force. After drying and immersion in PBS, the A20-S1-P1 hydrogel can achieve self-repair at room temperature without any external stimuli due to hydrogen bonding and the reversibility of borate ester bonds.

[0062] The rheological properties of the hydrogel prepared in Example 2 were tested. The results are as follows: Figure 9 As shown in (a), the modulus of the hydrogel material treated with PBS showed a corresponding increase, further demonstrating the stability of the boronic acid ester bonds and the enhanced hydrogen bonding. Furthermore, as... Figure 9 As shown in (b), a step scan was performed at a fixed frequency of 6.28 rad / s to test the rheological recovery behavior of the hydrogel. At a shear strain of 1000% (above the critical strain), the storage modulus G' of the hydrogel was lower than the loss modulus G, indicating that the hydrogel network structure was broken. Subsequently, when a lower strain of 0.1% was applied to the hydrogel, G' immediately increased, showing that the hydrogel has good self-healing properties.

[0063] The adhesion properties of the hydrogel prepared in Example 2 were tested. Figure 10As shown, Figure 10 (a) shows a schematic diagram of adhesion; (b) shows a standard adhesion curve; (c) shows an adhesion test photograph and curve; (d) shows adhesion curves with different biological tissues; and (e) shows the adhesion strength with different biological tissues. The hydrogel strip was pressurized between tissue samples for 30 seconds (applying a pressure of 1 kPa) to ensure the hydrogel swelled to equilibrium in a humid environment. All mechanical tests on the adhered samples were performed 24 hours after initial pressing. This shear test allowed for the determination of the adhesion strength of the hydrogel to different biological tissues. Its adhesion strength on pig skin, liver, heart, and muscle reached 46 ± 3.4 kPa, 11 ± 1.6 kPa, 26 ± 2.3 kPa, and 5.6 ± 0.8 kPa, respectively. This is because the hydrogel strip adsorbs and removes interfacial water through a dry crosslinking mechanism, then the carboxyl groups in the hydrogel form covalent bonds with the primary amine groups in the biological tissue, and hydrogen bonds are formed between the hydrogel and the surface of the biological tissue, thus achieving wet adhesion to the biological tissue in a humid environment.

[0064] The self-healing conductivity of the hydrogel prepared in Example 2 was tested. Figure 11 This describes the diode's luminescence state when the hydrogel is broken, healed, stretched after healing, and when it participates in a closed circuit. When the hydrogel is cut, the circuit breaks, causing the LED bulb to turn off. However, when two cut hydrogels heal, and when stretched under a certain external force after healing, the bulb can light up immediately. In this circuit, the hydrogel acts as the switch in a closed circuit; when the broken hydrogels come into contact with each other, the circuit is closed, and the bulb lights up. Stretching the healed hydrogel does not affect the bulb's state. Due to the complexity of intestinal leakage and peritoneal infection wounds, the pH of the wound microenvironment changes at different stages. This hydrogel not only possesses conductivity after self-healing but also, due to the pH sensitivity of its borate ester bonds, has the potential to respond to the pH of the microenvironment of open peritoneal wounds.

[0065] The cell compatibility of the hydrogel prepared in Example 2 was tested. The specific testing procedure was as follows: The A20-S1-P1 hydrogel treated with PBS was sterilized under UV light for 30 min, and then incubated in culture medium at 37°C for 24 hours at extraction ratios of 62.5 mg / mL, 125 mg / mL, 250 mg / mL, and 500 mg / mL, respectively. The hydrogel was then removed to obtain the sample extraction medium. After resuscitation and culture, NIH3T3 cells in the logarithmic growth phase were digested to obtain a cell suspension, which was then diluted with complete culture medium to a cell density of 1×10⁻⁶. 4After the cells were cultured at a density of 100 μL / mL, they were seeded into 96-well plates. The plates were then placed in a 37°C incubator containing 5% CO2. After cell attachment (24 h), the cell culture supernatant was discarded. The control group received 200 μL of complete culture medium; the experimental groups received 200 μL of different concentrations of extraction buffer (62.5, 125, 250, 500 mg / mL). After 24 h of incubation, the supernatant was discarded, and the cells were rinsed with PBS. Then, 200 μL of 0.5 mg / mL MTT was added to each well under dark conditions. The cells were incubated for another 4 h. The MTT-containing medium was carefully discarded, and 150 μL of DMSO was added. After shaking for 10 min, the absorbance of the 96 wells at 570 nm was measured using a microplate reader.

[0066] Figure 12 The cell viability of the control group, cells cultured with NIT3H3 at different concentration gradients for 24 hours was demonstrated. All experimental samples were repeated three times with the control group. As shown in the figures, compared to the empty control group, the cell viability of cells cultured with different concentrations of extracts for 24 hours was above 98%. According to international standard ISO 10993-5 (2009), this hydrogel material can be determined to be non-cytotoxic; therefore, this hydrogel exhibits good cell biocompatibility.

[0067] To further evaluate the cytotoxicity of the A20-S1-P1 hydrogel after PBS treatment, NH3T3 cells were co-cultured with the extract of the hydrogel and stained with Calcein / PI. Specifically, mouse embryonic fibroblasts (NH3T3) were cultured in DMEM high-glucose medium containing 10% FBS, maintaining the incubator temperature at 37°C and CO2 at 5%. Cell samples were collected at a quantity of 1 × 10⁻⁶ cells. 4 Cells were seeded in 96-well plates at 100 μL per well. The plates were placed in a 5% CO2, 37°C incubator. After cell attachment (24 h), the cell culture supernatant was discarded. The control group and cells containing 62.5 mg / mL extract were incubated with the cells for 48 h. The culture medium was carefully removed, and 200 μL of staining working solution was added and incubated with the cells at 4°C in the dark for 15-20 minutes. The cells were washed with PBS, and the results were examined using a laser confocal microscope. The Calcein laser wavelength was 488 nm, and the excitation wavelength of the dye-DNA complex was 552 nm.

[0068] The results are as follows Figure 13As shown, after 48 hours of culture, NIH3T3 cells were evenly distributed. Compared with the control group, the number of viable cells in the hydrogel material group was comparable (both greater than 98%), with a large number of live cells and very few dead cells present in the field of view. These results further demonstrate that the A20-S1-P1 hydrogel material treated with PBS has good biocompatibility and is non-cytotoxic when applied to human tissues.

[0069] In summary, the hydrogel prepared by this invention possesses certain mechanical properties, preventing external contamination and restoring the physiological environment within the abdominal cavity; good water absorption, retaining a certain amount of moisture for easy absorption of exudate; excellent self-healing properties, facilitating abdominal exploration and, when combined with negative pressure drainage, extending the protection period for the abdominal wound; adhesive properties, adhering to various moist biological tissues without requiring secondary clinical fixation; and post-healing electrical conductivity, with the potential to respond to the pH value of the microenvironment of the open abdominal wound. This invention provides a feasible solution for the design of temporary abdominal closure materials for intestinal leakage and abdominal infection wounds.

[0070] The above-disclosed embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of the invention. Those skilled in the art will understand that implementing all or part of the above-described embodiments and making equivalent changes in accordance with the claims of the present invention are still within the scope of the invention.

Claims

1. A method for preparing a hydrogel based on free radical polymerization, characterized in that: Includes the following steps: (1) Sodium alginate, acrylic acid, 3-acryloylaminophenylboronic acid, and N-succinimide acrylate were dissolved in deionized water to obtain a precursor solution; (2) An initiator is added to the precursor solution to initiate a free radical polymerization reaction. After stirring and ultrasonic degassing, a prepolymer solution with a pH of 2-2.2 is obtained. (3) The prepolymer solution is solidified to obtain the hydrogel; in the prepolymer solution, the mass fraction of acrylic acid is 15%-30%, the mass fraction of sodium alginate is 0.5%-3%, the mass fraction of 3-acrylamide phenylboronic acid is 0.5%-3%, the mass fraction of acrylic acid-N-succinimide is 1%, the mass fraction of initiator is 0.2%, and the remainder is deionized water.

2. The method for preparing hydrogels based on free radical polymerization as described in claim 1, characterized in that: It also includes enhancing the hydrogel obtained in step (3). The specific steps of the enhancement treatment are: evaporating and drying the hydrogel to form a hydrogel film, immersing it in a PBS solution with a pH of 7.3-7.5 until the length of the hydrogel recovers to the length before drying, and then taking it out.

3. The method for preparing hydrogels based on free radical polymerization as described in claim 2, characterized in that: The prepolymer solution contains 20% acrylic acid, 1% sodium alginate, 1% 3-acryloylaminophenylboronic acid, 1% acrylate-N-succinimide, 0.2% initiator, and the remainder is deionized water.

4. The method for preparing hydrogels based on free radical polymerization as described in claim 1, characterized in that: The initiator is α-ketoglutaric acid.

5. The method for preparing a hydrogel based on free radical polymerization as described in claim 1, characterized in that: The ultrasonic degassing time is 20-30 minutes.

6. The method for preparing a hydrogel based on free radical polymerization as described in claim 1, characterized in that: The specific operation of the curing is as follows: pour the prepolymer solution into the mold and irradiate it under ultraviolet light for 90-100 minutes.

7. A hydrogel based on free radical polymerization, prepared by the method described in any one of claims 1-6.

Citation Information

Patent Citations

  • Hydrogel composition with dynamic bond self-healing function as well as preparation method and application of hydrogel composition

    CN114736394A

  • Injectable hydrogel as well as preparation method and application thereof

    CN115109367A