A polytetrafluoroethylene microporous membrane, a method for preparing the same, and an application thereof

By uniformly distributing free radical quenchers in polytetrafluoroethylene microporous membranes, the problem of poor chemical stability of composite proton exchange membranes is solved, and the durability and mechanical strength of proton exchange membranes are improved, making them suitable for the industrial production of fuel cells.

CN117304527BActive Publication Date: 2026-11-20STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311181131.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2026-11-20
Estimated Expiration
2043-09-13

Smart Images

  • Figure CN117304527B_ABST
    Figure CN117304527B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of fuel cells, and particularly relates to a polytetrafluoroethylene microporous membrane and a preparation method and application thereof. The preparation method of the polytetrafluoroethylene microporous membrane disclosed in the embodiment of the application comprises the following steps: (1) mixing an active substance and polytetrafluoroethylene resin to obtain a mixture F-PTFE, wherein the active substance comprises at least one of cerium nitrate, cerium acetate, cerium chloride, cerium sulfate, manganese sulfate, manganese nitrate and manganese acetate; (2) mixing the F-PTFE and an auxiliary oil, then performing maturation treatment, and then sequentially performing a casting blank process and an extrusion process to obtain a rod-shaped material, and then pressing the rod-shaped material into a coiled material; (3) performing degreasing treatment on the coiled material, and then performing longitudinal stretching to obtain a polytetrafluoroethylene film material; and (4) performing transverse stretching on the polytetrafluoroethylene film material, and then winding after cooling to obtain a polytetrafluoroethylene microporous membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of fuel cell technology, specifically relating to a polytetrafluoroethylene microporous membrane, its preparation method, and its application. Background Technology

[0002] A fuel cell is an energy conversion device that directly converts the chemical energy of fuel into electrical energy without combustion. It has advantages such as not being limited by the Carnot cycle and having a high energy conversion rate. A proton exchange membrane fuel cell (PEMFC) is a type of fuel cell that, in addition to the general characteristics of fuel cells, also has advantages such as no electrolyte loss, rapid low-temperature start-up, high specific power and specific energy, zero emissions, and being clean and environmentally friendly.

[0003] The proton exchange membrane (PEMFC) is a key component in PEMFCs, acting as a barrier between reactant gases and proton conduction. Therefore, an excellent PEMFC requires high proton conductivity, low electronic conductivity, low permeability, and excellent dimensional stability, mechanical strength, and thermal stability. As early as the last century, Gore pioneered the combination of polytetrafluoroethylene (PTFE) film, characterized by corrosion resistance, flexibility, good chemical stability, strong insulation, high strength, and high porosity, with perfluorosulfonic acid resin to obtain a composite PEMFC. This significantly improved the mechanical strength and dimensional stability of the PEMFC while reducing its thickness, resulting in a marked increase in proton conduction efficiency.

[0004] While the mechanical strength and proton conductivity of composite membranes have been improved, the main factors currently hindering the commercialization of fuel cells are their production cost and lifespan, especially under conditions of rapid start-up and shutdown, dry and wet conditions, and temperature changes, as well as the resulting mechanical and electrochemical aging, which severely affects the durability and stability of the membrane electrode assembly (MEA), a core component of fuel cells. Therefore, further improving the durability and stability of proton exchange membranes is a current research focus. Summary of the Invention

[0005] This invention is based on the inventor's discovery and understanding of the following facts and problems: During the operation of a fuel cell, proton exchange membranes inevitably experience anode and cathode gas permeation, leading to hydrogen contacting air to generate H2O2, while metal ions (such as Fe) inside the membrane... 2+The presence of hydroxyl radicals (H₂O· and H₂O·) induces an electro-Fenton reaction, generating a large number of H₂O· and H₂O· free radicals. These free radicals attack the α-carbon of the aromatic groups of the resin, the ether bonds on the side chains, or the branch points and terminal carboxyl groups of the resin, causing degradation of the proton exchange membrane's chemical structure, resulting in reduced thickness and even pinholes. In related technologies, introducing free radical quenchers into the perfluorosulfonic acid resin matrix or components outside the proton exchange membrane can reduce the diffusion of hydroxyl radicals to the proton exchange membrane, thereby improving the membrane's resistance to free radicals. For composite proton exchange membranes with microporous membrane reinforcement layers, the portion where the e-PTFE microporous membrane is bonded to the perfluorosulfonic acid resin contains a large number of voids, and there are numerous contact interfaces between the perfluorosulfonic acid resin and the microporous membrane. This results in the perfluorosulfonic acid resin having a very large specific surface area in this region. This large specific surface area exacerbates the destructive effect of hydroxyl radicals on the perfluorosulfonic acid resin, leading to performance degradation of the composite proton exchange membrane. Some existing technologies also improve the durability of proton exchange membranes in battery systems by loading free radical quenchers onto catalysts, gas diffusion layers, bipolar plates, or other locations on membrane electrodes. However, in currently widely used composite proton exchange membranes, the microporous membrane and perfluorosulfonic acid resin composite region has a problem where the volume and mass content of free radical quenchers and / or antioxidants are lower than in other regions, resulting in poor chemical stability.

[0006] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention propose a method for preparing a polytetrafluoroethylene (PTFE) microporous membrane. This method involves thoroughly mixing a free radical quencher with a polymer material to obtain a composite, and then biaxially stretching the composite to obtain a PTFE microporous membrane. This imparts free radical quenching capability to the PTFE microporous membrane. When used to prepare a proton exchange membrane, the content of the free radical quencher in the composite region of the PTFE microporous membrane and perfluorosulfonic acid resin is controllable, which can improve the chemical durability of the proton exchange membrane.

[0007] The method for preparing the polytetrafluoroethylene microporous membrane according to an embodiment of the present invention includes the following steps:

[0008] (1) The active material and polytetrafluoroethylene resin are mixed to obtain a mixture F-PTFE, wherein the active material includes at least one of cerium nitrate, cerium acetate, cerium chloride, cerium sulfate, manganese sulfate, manganese nitrate and manganese acetate;

[0009] (2) The F-PTFE obtained in step (1) is mixed with the additive oil and then subjected to aging treatment. Then, it is subjected to casting and extrusion processes to obtain rod-shaped material. The rod-shaped material is then pressed and calendered to obtain coil material.

[0010] (3) After degreasing the roll material obtained in step (2), it is stretched longitudinally to obtain polytetrafluoroethylene film material;

[0011] (4) The polytetrafluoroethylene film material obtained in step (3) is stretched laterally, cooled and then wound up to obtain a polytetrafluoroethylene microporous membrane.

[0012] The advantages and technical effects of the polytetrafluoroethylene (PTFE) microporous membrane preparation method of this invention are as follows: 1. In the method of this invention, the soluble active material can be uniformly dispersed in PTFE resin, giving the PTFE microporous membrane free radical quenching ability, which can improve the durability of the proton exchange membrane when applied to its preparation; 2. In the method of this invention, some of the added active material can be thermally decomposed during processing to obtain its oxide, reducing the rate of loss of active material in the membrane module during actual operation; 3. The method of this invention is simple to operate, can adopt mature existing industrial production technology, is easy to scale up, and can meet the requirements of research and industrial production applications.

[0013] In some embodiments, in step (1), the amount of the active substance added is 0.1 to 25% of the polytetrafluoroethylene resin.

[0014] In some embodiments, in step (2), the mass ratio of F-PTFE to additive oil is 5:1 to 3:2.

[0015] In some embodiments, in step (2), the curing temperature is 60-70°C and the curing time is 20-24 hours; and / or, the diameter of the rod-shaped material is 14-20 mm; the thickness of the roll material is 0.2-0.4 mm and the width is 100-130 mm.

[0016] In some embodiments, in step (3), the thickness of the polytetrafluoroethylene film material is 0.15 mm to 0.2 mm.

[0017] In some embodiments, in step (4), during the transverse stretching, the temperature of the preheating zone of the transverse stretching equipment is 100-250°C, the temperature of the stretching zone is 180-280°C, and the temperature of the heat setting zone is 330-380°C; and / or, the final stretching ratio of the polytetrafluoroethylene microporous membrane is 24-40 times.

[0018] In some embodiments, step (5) further includes a secondary sintering and shaping process for the polytetrafluoroethylene microporous membrane obtained in step (4).

[0019] In some embodiments, in step (5), the temperature of the secondary sintering and shaping is 330-340°C, and the time of the secondary sintering and shaping is 60-180s; and / or, the heating method of the secondary sintering and shaping includes at least one of roller heating, hot air circulation heating, and infrared radiation heating.

[0020] This invention also provides a polytetrafluoroethylene microporous membrane, which is prepared using the above-described preparation method.

[0021] The present invention also provides a proton exchange membrane, comprising a polytetrafluoroethylene microporous membrane prepared by the above preparation method or the above-described polytetrafluoroethylene microporous membrane. Attached Figure Description

[0022] Figure 1 This is a scanning electron microscope image of the microporous membrane F-ePTFE1 prepared in Example 1, with a magnification of 5000x.

[0023] Figure 2 This is a scanning electron microscope image of the microporous membrane FH-ePTFE2 prepared in Example 2, with a magnification of 5000x.

[0024] Figure 3 The image shown is a scanning electron microscope (SEM) image of the H-ePTFE9 microporous membrane prepared in Comparative Example 2, with a magnification of 5000x. Detailed Implementation

[0025] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0026] The method for preparing the polytetrafluoroethylene microporous membrane according to an embodiment of the present invention includes the following steps:

[0027] (1) The active material and polytetrafluoroethylene resin are mixed to obtain a mixture F-PTFE, wherein the active material includes at least one of cerium nitrate, cerium acetate, cerium chloride, cerium sulfate, manganese sulfate, manganese nitrate and manganese acetate;

[0028] (2) The F-PTFE obtained in step (1) is mixed with the additive oil and then subjected to aging treatment. Then, it is processed through casting and extrusion processes to obtain rod-shaped material, and then the rod-shaped material is pressed into rolls.

[0029] (3) After degreasing the roll material obtained in step (2), it is stretched longitudinally to obtain polytetrafluoroethylene film material;

[0030] (4) The polytetrafluoroethylene film material obtained in step (3) is stretched laterally, cooled and then wound up to obtain a polytetrafluoroethylene microporous membrane.

[0031] The method for preparing polytetrafluoroethylene (PTFE) microporous membranes according to embodiments of the present invention allows soluble active substances to be uniformly dispersed in PTFE resin, endowing the PTFE microporous membrane with free radical quenching ability. When applied to the preparation of proton exchange membranes, this method can improve the durability of the proton exchange membranes. Some of the added active substances can be thermally decomposed during processing to obtain their oxides, reducing the rate of loss of active substances in the membrane module during actual operation. The method is simple to operate, can adopt mature existing industrial production technologies, is easy to scale up, and can meet the requirements of research and industrial production applications.

[0032] In some embodiments, preferably, in step (1), the amount of the active substance added is 0.1 to 25 wt% of the polytetrafluoroethylene resin. More preferably, the amount of the active substance added is 0.1 to 10 wt% of the polytetrafluoroethylene resin. Even more preferably, the amount of the active substance added is 0.1 to 5 wt% of the polytetrafluoroethylene resin. More preferably, it is 0.1 to 1 wt%.

[0033] In this embodiment of the invention, the preferred amount of added active material is beneficial to improving the overall performance of the polytetrafluoroethylene microporous membrane. If the amount of added active material is too small, the improvement on the durability of the polytetrafluoroethylene microporous membrane is very limited. If the amount of added active material is too large, it may accumulate in the polytetrafluoroethylene resin, which will ultimately have an adverse effect on the film-forming effect and mechanical strength of the polytetrafluoroethylene microporous membrane.

[0034] In some embodiments, preferably, in step (1), the mixing of the active material and the polytetrafluoroethylene resin includes: adding the active material to a polytetrafluoroethylene emulsion with a solid content of 60%, dispersing it evenly and co-coagulating it, and then drying it.

[0035] In this embodiment of the invention, a wet mixing method is preferably used to mix the active material and polytetrafluoroethylene resin, which can promote the uniform dispersion of the active material in the polytetrafluoroethylene resin. Moreover, this method is simple to operate and easy to scale up.

[0036] In some embodiments, preferably, in step (2), the mass ratio of F-PTFE to auxiliary oil is 5:1 to 3:2. More preferably, in step (2), the curing temperature is 60 to 70°C, and the curing time is 20 to 24 hours; and / or, the diameter of the rod-shaped material is 14 to 20 mm; the thickness of the roll material is 0.2 to 0.4 mm, and the width is 100 to 130 mm.

[0037] In some embodiments, preferably, in step (3), the thickness of the polytetrafluoroethylene film material is 0.15 mm to 0.2 mm.

[0038] In some embodiments, preferably, in step (4), during the transverse stretching, the temperature of the preheating zone of the transverse stretching equipment is 100–250°C, the temperature of the stretching zone is 180°C–280°C, and the temperature of the heat-setting zone is 330–380°C; and / or, the final stretching ratio of the polytetrafluoroethylene microporous membrane is 24–40 times. More preferably, the width of the preheating zone track is 60–100 mm, the width of the stretching zone track gradually increases from 60–100 mm to 1800–2400 mm, and the width of the heat-setting zone track is 1800–2400 mm. Even more preferably, the running speed of the polytetrafluoroethylene film material in the transverse stretching equipment is 5–15 m / min.

[0039] In some embodiments, preferably, step (5) further includes a secondary sintering and shaping treatment of the polytetrafluoroethylene microporous membrane obtained in step (4). More preferably, in step (5), the secondary sintering and shaping temperature is 330–340°C, and the secondary sintering and shaping time is 60–180 s; and / or, the heating method for the secondary sintering and shaping includes at least one of roller heating, hot air circulation heating, and infrared radiation heating. Even more preferably, the running speed of the polytetrafluoroethylene microporous membrane during the secondary sintering and shaping treatment is 5–15 m / min.

[0040] In this embodiment of the invention, secondary sintering and reshaping of the polytetrafluoroethylene (PTFE) microporous membrane can release the internal stress generated during the stretching process, reduce the thermal shrinkage rate of the membrane, promote an appropriate increase in nodes and thickening of fibers, thereby improving the strength and modulus of the PTFE membrane. The preferred temperature for secondary sintering and reshaping is slightly higher than the melting point of PTFE (326°C). This allows for secondary sintering and structural reshaping of the membrane material, improving the strength of the PTFE microporous membrane, while avoiding energy waste and reducing production costs.

[0041] This invention also provides a polytetrafluoroethylene microporous membrane, which is prepared using the above-described preparation method.

[0042] The present invention also provides a proton exchange membrane, comprising a polytetrafluoroethylene microporous membrane prepared by the above preparation method or the above-described polytetrafluoroethylene microporous membrane.

[0043] The method for preparing the proton exchange membrane includes the following steps:

[0044] (a) Dispersing ion exchange resin in a molding solvent to obtain an ion exchange resin dispersion;

[0045] (b) The ion exchange membrane resin dispersion prepared in step (a) is coated on a PET base film, and then a polytetrafluoroethylene microporous membrane is covered on the wet film surface, and then dried to obtain a composite membrane.

[0046] (c) In the composite membrane obtained in step (b), the other side of the polytetrafluoroethylene microporous membrane facing away from the wet membrane is coated again with ion exchange membrane resin dispersion, and after drying, a composite proton exchange membrane is obtained.

[0047] The method for preparing the proton exchange membrane in this embodiment of the invention enables a better bonding force between the filled modified microporous membrane and the ion exchange resin, thereby ensuring that the proton exchange membrane has better performance. The method is simple and easy to operate, and is convenient for application in industrial production.

[0048] In some embodiments, preferably, in step (a), the molding solvent includes at least one of water, a highly polar organic solvent, tetrahydrofuran, a fatty alcohol, and a nonpolar liquid alkane; the highly polar organic solvent includes at least one of ethylene glycol, propylene glycol, glycerol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoric triamine, and N-methylpyrrolidone; the fatty alcohol includes at least one of methanol, ethanol, isopropanol, n-propanol, tert-butanol, and n-butanol; and the nonpolar liquid alkane includes at least one of n-hexane and cyclohexane.

[0049] In some embodiments, preferably, in step (b), the drying temperature is 50–180°C.

[0050] In some embodiments, preferably, in step (c), the drying temperature is 60–230°C. More preferably, the thickness of the composite proton exchange membrane is 8–50 μm, more preferably 8–20 μm.

[0051] Example 1

[0052] (1) Add 0.1 part of cerium nitrate powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of cerium nitrate added is 0.1 wt% of the polytetrafluoroethylene resin).

[0053] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 5:1, wherein 500g of resin and 100g of auxiliary oil are placed in a mixing drum and cured in an oven at 60℃ for 24 hours. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.2 mm and a width of about 100 mm using a precision calender;

[0054] (3) The roll material is passed through a high-temperature degreasing oven to remove the auxiliary oil, and then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.15 mm.

[0055] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain the polytetrafluoroethylene microporous membrane F-ePTFE1.

[0056] Example 2

[0057] (1) Add 0.1 part of cerium nitrate powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of cerium nitrate added is 0.1 wt% of the polytetrafluoroethylene resin).

[0058] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 5:1, wherein 500g of resin and 100g of auxiliary oil are placed in a mixing drum and cured in an oven at 60℃ for 24 hours. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.2 mm and a width of about 100 mm using a precision calender;

[0059] (3) The roll material is passed through a high-temperature degreasing oven to remove the auxiliary oil, and then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.15 mm.

[0060] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain a polytetrafluoroethylene microporous membrane.

[0061] (5) The polytetrafluoroethylene microporous membrane is unwound through the secondary sintering zone at a speed of 5 m / min. The temperature in the secondary sintering zone is heated to 340°C by roller heating and held for 120 s. Finally, after cooling, the microporous membrane FH-ePTFE2 is obtained.

[0062] Example 3

[0063] (1) Add 0.8 parts of manganese nitrate powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of manganese nitrate added is 0.8 wt% of the polytetrafluoroethylene resin).

[0064] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 3:2, wherein 600g of resin and 400g of auxiliary oil are placed in a mixing drum and cured in an oven at 60℃ for 24 hours. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.25 mm and a width of about 120 mm using a precision calender.

[0065] (3) After passing the roll material through a high-temperature degreasing oven to remove the auxiliary oil, it is then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.15 mm.

[0066] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain the polytetrafluoroethylene microporous membrane F-ePTFE3.

[0067] Example 4

[0068] The preparation method of the polytetrafluoroethylene microporous membrane in this embodiment is the same as that in Example 3. The only difference is that the polytetrafluoroethylene microporous membrane is passed through a secondary sintering zone, unwound at a speed of 5 m / min, the temperature of the secondary sintering zone is set to 340°C, the holding time is 60 s, and finally, after cooling, it is wound up to obtain the microporous membrane FH-ePTFE4.

[0069] Example 5

[0070] (1) Add 1 part of cerium chloride powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of cerium chloride added is 1 wt% of the polytetrafluoroethylene resin).

[0071] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 3:2, wherein 600g of resin and 400g of auxiliary oil are placed in a mixing drum and cured in an oven at 70℃ for 20h. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.25 mm and a width of about 120 mm using a precision calender.

[0072] (3) After passing the roll material through a high-temperature degreasing oven to remove the auxiliary oil, it is then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.17 mm.

[0073] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain a polytetrafluoroethylene microporous membrane.

[0074] (5) The polytetrafluoroethylene microporous membrane is unwound through the secondary sintering zone at a speed of 5 m / min. The temperature in the secondary sintering zone is heated to 330°C by hot air circulation heating and held for 120 s. Finally, after cooling, the microporous membrane FH-ePTFE5 is obtained.

[0075] Example 6

[0076] (1) Add 5 parts of manganese acetate powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of manganese acetate added is 5 wt% of the polytetrafluoroethylene resin).

[0077] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 5:1, wherein 500g of resin and 100g of auxiliary oil are placed in a mixing drum and cured in an oven at 70℃ for 24 hours. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.3 mm and a width of about 130 mm using a precision calender.

[0078] (3) After passing the roll material through a high-temperature degreasing oven to remove the additive oil, it is then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.2 mm.

[0079] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain a polytetrafluoroethylene microporous membrane.

[0080] (5) The polytetrafluoroethylene microporous membrane is unwound through the secondary sintering zone at a speed of 5 m / min. The temperature in the secondary sintering zone is heated to 330°C by infrared radiation heating and held for 120 s. Finally, after cooling, the membrane is wound up to obtain the microporous membrane FH-ePTFE6.

[0081] Example 7

[0082] (1) Add 3 parts of manganese nitrate powder to a polytetrafluoroethylene emulsion (solid content 60%) containing 100 parts of solid PTFE material (10 kg) and mix thoroughly. After drying, the mixture F-PTFE is obtained (i.e., the amount of manganese nitrate added is 3 wt% of the polytetrafluoroethylene resin).

[0083] (2) F-PTFE resin and auxiliary oil are mixed evenly at a mass ratio of 3:2, wherein 600g of resin and 400g of auxiliary oil are placed in a mixing drum and cured in an oven at 70℃ for 22h. The cured resin is then extruded through a casting and extrusion process to obtain... The rod-shaped material is then pressed into a roll material with a thickness of about 0.3 mm and a width of about 130 mm using a precision calender.

[0084] (3) After passing the roll material through a high-temperature degreasing oven to remove the additive oil, it is then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.2 mm.

[0085] (4) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain a polytetrafluoroethylene microporous membrane.

[0086] (5) The polytetrafluoroethylene microporous membrane is unwound through the secondary sintering zone at a speed of 5 m / min. The temperature in the secondary sintering zone is heated to 340°C by roller heating and held for 120 s. Finally, after cooling, the microporous membrane FH-ePTFE7 is obtained.

[0087] Comparative Example 1

[0088] The preparation method of this comparative example is the same as that of Example 1, except that step (1) is omitted, that is, the material for preparing the microporous membrane is untreated PTFE resin, and the microporous membrane ePTFE8 is obtained.

[0089] Comparative Example 2

[0090] The method is the same as in Example 7, except that step (1) is omitted and cerium nitrate is not added, as follows:

[0091] (1) Untreated PTFE resin and auxiliary oil were mixed evenly at a mass ratio of 3:2, with 600g of resin and 400g of auxiliary oil. The mixture was placed in a mixing drum and cured in an oven at 70℃ for 22 hours. The cured resin was then extruded through a casting and extrusion process to obtain the desired product. The rod-shaped material is then pressed into a roll material with a thickness of about 0.3 mm and a width of about 130 mm using a precision calender.

[0092] (2) The roll material is passed through a high-temperature degreasing oven to remove the auxiliary oil, and then passed through a longitudinal stretching oven to obtain a polytetrafluoroethylene film material with a thickness of about 0.2 mm.

[0093] (3) The polytetrafluoroethylene film material is stretched horizontally and unwound at a speed of 5 m / min. The temperature in the preheating zone is set to 120℃, the temperature in the stretching zone is set to 200℃, the temperature in the heat setting zone is set to 370℃, and finally, after cooling, it is wound up to obtain a polytetrafluoroethylene microporous membrane.

[0094] (4) The polytetrafluoroethylene microporous membrane is unwound through the secondary sintering zone at a speed of 5 m / min. The temperature in the secondary sintering zone is heated to 340°C by hot air circulation heating and held for 120 s. Finally, after cooling, the microporous membrane H-ePTFE9 is obtained.

[0095] Performance testing

[0096] The relevant testing methods are as follows:

[0097] Membrane thickness test: The test equipment is a contact flat-head thickness gauge. Three microporous membrane sheets are cut out with a cutter as test samples. During the thickness measurement, points are taken at equal intervals along the MD (longitudinal) and TD (transverse) directions of the sample to perform matrix testing, and the average value of each point is calculated as the average thickness of the membrane.

[0098] Free radical resistance: The proton exchange membrane was immersed in Fenton's reagent at 80℃ for 8 hours, and the mass loss before and after treatment with different immersion times was compared. Preparation of Fenton's reagent: 0.1 mL of 0.01 mol / L Fe was added dropwise to 50 mL of 3% (w / w) H₂O₂ solution. 2+ The solution, i.e., the prepared Fenton reagent, should be prepared fresh for immediate use. A smaller percentage of mass loss indicates better free radical resistance.

[0099] The test methods for electrical conductivity and tensile strength are as described in "Proton Exchange Membrane Fuel Cells Part 3: Test Methods for Proton Exchange Membranes". The test conditions for electrical conductivity are a temperature of 80°C and a relative humidity of 30%.

[0100] (1) The properties of the polytetrafluoroethylene microporous membranes prepared in Examples 1-7 and Comparative Examples 1-2 were tested, and the results are shown in Table 1:

[0101] Table 1

[0102]

[0103] As can be seen from the data in Table 1, secondary sintering of polytetrafluoroethylene (PTFE) microporous membranes can significantly increase their mechanical strength (e.g., compared to Example 1, Example 2, and Example 3). However, as the content of active material increases, the mechanical strength of PTFE microporous membranes shows a trend of first increasing and then decreasing (e.g., Comparative Example 2, Example 2, and Examples 4-7). This is because an appropriate amount of active material can improve the mechanical strength of the membrane material, but when the content is too high, the agglomeration of inorganic materials and the incompatibility between inorganic and organic materials lead to the destruction of the structure of organic fibers, which in turn causes the mechanical strength of the membrane to decrease rapidly.

[0104] (2) The polytetrafluoroethylene microporous membranes prepared in Examples 1, 2, and 2 were characterized by scanning electron microscopy, and the results are as follows: Figure 1 , Figure 2 and Figure 3 As shown:

[0105] As can be seen from the figures, the polytetrafluoroethylene (PTFE) membranes in Examples 2 and 2, after secondary sintering, exhibit larger nodes, coarser fibers, and larger pore sizes compared to the membrane material in Example 1 without secondary sintering. This is because secondary sintering at higher temperatures causes the fine fibers to fuse and shrink, forming coarser fibers. Simultaneously, the fibers near the nodes shrink to form larger nodes, thereby increasing mechanical strength. Furthermore, the microstructure of the PTFE microporous membrane obtained in Example 2 differs significantly from that in Comparative Example 2. Both the nodes and fibers of the membrane are coated with functional particles. Coating the nodes and fibers with an appropriate amount of functional material enhances the mechanical strength of the PTFE microporous membrane.

[0106] (3) Proton exchange membranes were prepared using the polytetrafluoroethylene microporous membranes obtained in Examples 1-7 and Comparative Examples 1-2, and the performance of the proton exchange membranes was tested. The results are shown in Table 2.

[0107] The preparation method of the proton exchange membrane is as follows:

[0108] (a) 3M 725 ion exchange resin (EW≈725g / mol) was dispersed in tetrahydrofuran to obtain an ion exchange resin dispersion;

[0109] (b) A certain thickness of 3M725 ion exchange membrane resin dispersion is coated on the PET base film. Then, the polytetrafluoroethylene microporous membrane is fully stretched and covered on the wet film surface. Then, it is placed in an oven at 80°C to dry, and a composite membrane is obtained.

[0110] (c) A certain thickness of 3M725 ion exchange membrane resin dispersion is coated again on the other side of the polytetrafluoroethylene microporous membrane that is opposite to the wet membrane in the composite membrane, and dried at 160°C to obtain a composite proton exchange membrane.

[0111] Table 2

[0112]

[0113] As can be seen from the data in the table above, the composite proton exchange membranes prepared using the polytetrafluoroethylene microporous membranes obtained in Examples 1-7 exhibit better free radical resistance, and the free radical resistance gradually increases with the increase of active material content. After secondary sintering and shaping treatment, the mechanical properties of the composite proton exchange membrane are improved, and the free radical resistance is also slightly improved (as compared with Examples 1 and 2, and with Examples 3 and 4). This is because the better the mechanical properties of the polytetrafluoroethylene microporous membrane, the better the dimensional stability and mechanical stability of the proton exchange membrane, the less likely it is to form defects such as pores and cracks, and the smaller the contact area with hydroxyl free radicals, thus improving the free radical resistance.

[0114] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0115] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.

Claims

1. A method for preparing a polytetrafluoroethylene microporous membrane, characterized in that, Includes the following steps: (1) The active material and polytetrafluoroethylene resin are mixed to obtain a mixture F-PTFE, wherein the active material includes at least one of cerium nitrate, cerium acetate, cerium chloride, cerium sulfate, manganese sulfate, manganese nitrate, and manganese acetate; the amount of the active material added is 0.1~0.8 wt% of the polytetrafluoroethylene resin; (2) The F-PTFE obtained in step (1) is mixed with the additive oil and then subjected to aging treatment. Then, it is processed through casting and extrusion processes to obtain rod-shaped material, and then the rod-shaped material is pressed into rolls. (3) After degreasing the roll material obtained in step (2), longitudinal stretching is performed to obtain polytetrafluoroethylene film material; (4) The polytetrafluoroethylene film material obtained in step (3) is stretched laterally, cooled and then wound up to obtain a polytetrafluoroethylene microporous membrane; in the lateral stretching, the temperature of the preheating zone of the lateral stretching equipment is 100~250℃, the temperature of the stretching zone is 180℃~280℃, and the temperature of the heat setting zone is 330~380℃. (5) The polytetrafluoroethylene microporous membrane obtained in step (4) is subjected to a secondary sintering and shaping treatment. The temperature of the secondary sintering and shaping is 330~340℃ and the time of the secondary sintering and shaping is 60~180s.

2. The method for preparing the polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (2), the mass ratio of F-PTFE to additive oil is 5:1 to 3:

2.

3. The method for preparing the polytetrafluoroethylene microporous membrane according to claim 1 or 2, characterized in that, In step (2), the curing temperature is 60~70℃ and the curing time is 20~24h; and / or, the diameter of the rod-shaped material is 14~20 mm; the thickness of the roll material is 0.2~0.4mm and the width is 100~130mm.

4. The method for preparing the polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (3), the thickness of the polytetrafluoroethylene film material is 0.15mm~0.2mm.

5. The method for preparing the polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (4), the final stretching ratio of the polytetrafluoroethylene microporous membrane is 24 to 40 times.

6. The method for preparing the polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (5), the heating method for the secondary sintering and shaping includes at least one of roller heating, hot air circulation heating, and infrared radiation heating.

7. A polytetrafluoroethylene microporous membrane, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 6.

8. A proton exchange membrane, characterized in that, This includes the polytetrafluoroethylene microporous membrane prepared by the preparation method according to any one of claims 1 to 6, or the polytetrafluoroethylene microporous membrane according to claim 7.

Citation Information

Patent Citations

  • Free radical quenching agent, preparation method thereof and application of free radical quenching agent in membrane electrode

    CN113690450A

  • Proton exchange membrane and preparation method and application thereof

    CN114665134A