A multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, its preparation method and application

By growing a core-shell structured Re-Ni@Ni(OH)₂/CC electrocatalyst in situ on carbon cloth, the problems of high cost of precious metal catalysts and low efficiency of non-precious metal catalysts were solved, and highly efficient electrocatalytic water splitting to produce hydrogen and furfural oxidation reaction were achieved across the entire pH range, generating high-value-added chemicals.

CN117305887BActive Publication Date: 2026-11-24ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311158814.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-08
Publication Date
2026-11-24
Estimated Expiration
2043-09-08

AI Technical Summary

Technical Problem

In existing water electrolysis technologies, precious metal catalysts are expensive, non-precious metal catalysts are inefficient over a wide pH range, slow OER kinetics lead to large energy losses, and the electrocatalytic process is significantly affected by proton or hydroxide concentrations, making it difficult to achieve multifunctional and efficient electrocatalysis.

Method used

A multifunctional electrocatalyst with a core-shell structure, Re-Ni@Ni(OH)₂/CC, was grown in situ using carbon cloth as a substrate. By forming a nickel hydroxide shell around the nickel core and using perrhenate to regulate the nickel core, a core-shell catalyst was formed, which improved the electrocatalytic activity and stability.

Benefits of technology

The cathode HER kinetics of electrocatalytic water splitting for hydrogen production are improved across the entire pH range, replacing OER, increasing electron utilization, and generating high-value-added chemicals, exhibiting excellent electrocatalytic activity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117305887B_ABST
    Figure CN117305887B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of electrocatalysis technology and discloses a multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, its preparation method, and its application. The catalyst uses carbon cloth as a substrate, on which nanospheres are grown in situ. The nanospheres have a core-shell structure, with the core being a rhenium-controlled nickel core and the shell being nickel hydroxide. The preparation steps are as follows: (1) Commercial carbon cloth is cut, acid-washed, and dried for later use; (2) Perrhenate, nickel salt, hydrazine hydrate, and water are stirred evenly together, and the mixed solution is transferred to a hydrothermal reactor; (3) The carbon cloth obtained in step (1) is placed in the hydrothermal reactor, the reactor lid is tightened, and the hydrothermal reactor is reacted at 100-250 °C for 300-1000 min. After cooling to room temperature, the carbon cloth is removed and dried to obtain the target catalyst. The catalyst prepared by this invention has the advantages of simple process, economy and practicality, high stability, and excellent electrocatalytic hydrogen production and furfural oxidation activity at all pH.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalysis technology, specifically relating to a multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, its preparation method, and its application. Background Technology

[0002] With the continuous depletion of fossil fuels and the persistent severity of environmental pollution, replacing fossil resources with renewable hydrogen (H2) energy is an effective approach. Electrochemical water splitting is recognized as the cleanest hydrogen production technology. However, the catalysts for the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode are generally precious metals such as platinum / ruthenium / iridium. To reduce costs, researchers have extensively studied abundant transition metal materials. For example, cobalt, nickel, and iron-based catalysts exhibit OER performance comparable to ruthenium oxide, while the HER performance of most non-precious metals is far inferior to that of precious metals. Moreover, considering the inevitable influence of proton or hydroxide concentrations during electrocatalysis, developing a non-precious metal electrocatalyst that can operate effectively over a wide pH range is noteworthy. Most importantly, the slow OER kinetics during water electrolysis lead to significant energy loss. Considering the use of biomass organic reactions (furfural oxidation, FOR) to replace OER can not only improve electron utilization but also generate high-value-added chemicals. Therefore, exploring a multifunctional electrocatalyst is extremely challenging. Summary of the Invention

[0003] The purpose of this invention is to provide a multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, its preparation method, and its application.

[0004] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A multifunctional electrocatalyst, Re-Ni@Ni(OH)2 / CC, is based on carbon cloth, on which nanospheres are grown in situ. The nanospheres have a core-shell structure, with the core being a rhenium-regulated nickel core and the shell being nickel hydroxide.

[0005] The preparation method of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC includes the following steps: (1) Commercial carbon cloth is cut, acid-washed and dried for later use; (2) Stir perrhenate, nickel salt, hydrazine hydrate and water together until homogeneous, and transfer the mixed solution to a hydrothermal reactor; (3) Place the carbon cloth obtained in step (1) into a hydrothermal reactor, tighten the reactor lid, react the hydrothermal reactor at 100~250 ℃ for 300-1000 min, cool to room temperature, take out the carbon cloth, dry it, and the target catalyst is obtained. The perrhenate is calculated based on the rhenium element provided, and the nickel salt is calculated based on the nickel element provided. The ratio of raw materials used is perrhenate: nickel salt: hydrazine hydrate: water = (0.1-2) mmol: (0.1-2) mmol: (1-3) mL: (10-30) mL, and the total number of moles of perrhenate and nickel salt is 2 mmol. The area of ​​the carbon cloth in step (3) is 2-5 cm². 2 / 2 mmol (perrhenate + nickel salt).

[0006] Preferably, the nickel salt is nickel nitrate, nickel chloride, or nickel sulfate.

[0007] Preferably, the perrhenate is ammonium perrhenate, potassium perrhenate, or sodium perrhenate.

[0008] Application of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC in electrocatalytic water splitting for hydrogen production across the entire pH range or in furfural oxidation.

[0009] In this invention, the addition of a small amount of hydrazine hydrate serves two purposes: first, to reduce some of the high-valence nickel to nickel elemental nuclei; and second, to provide an alkaline environment for the synthesis process, allowing a nickel hydroxide shell to grow on the outside of the nickel nuclei, thereby forming a core-shell catalyst.

[0010] Beneficial effects: The catalyst prepared by this invention has the advantages of simple process, economic and practicality, and high stability. It can not only improve the cathode HER kinetics of electrocatalytic water splitting to produce hydrogen, but also replace OER with FOR at the anode to improve electron utilization and generate high value-added chemicals. It exhibits excellent electrocatalytic hydrogen production at all pH and furfural oxidation activity. Attached Figure Description

[0011] Figure 1 XRD patterns of the Re-Ni@Ni(OH)2 / CC catalyst prepared in Example 2 of this invention and the Ni@Ni(OH)2 / CC catalyst prepared in Comparative Example 1.

[0012] Figure 2 TEM image of the Re-Ni@Ni(OH)2 / CC catalyst prepared in Example 2 of this invention.

[0013] Figure 3 EDX elemental mapping diagram of the Re-Ni@Ni(OH)2 / CC catalyst prepared in Example 2 of this invention.

[0014] Figure 4 XRD patterns of the Re-Cu / CC and Re-Ni / CC catalysts prepared in Comparative Examples 2 and 3 of this invention.

[0015] Figure 5Electrocatalytic hydrogen production at all pH values ​​for the Re-Ni@Ni(OH)2 / CC catalysts prepared in Examples 1-4 of this invention and the Ni@Ni(OH)2 / CC catalyst prepared in Comparative Example 1.

[0016] Figure 6 Hydrogen production diagrams of the Re-Cu / CC and Re-Ni / CC catalysts prepared in Comparative Examples 2 and 3 of this invention.

[0017] Figure 7 Furfural oxidation diagrams of the Re-Ni@Ni(OH)2 / CC and Ni@Ni(OH)2 / CC catalysts prepared in Example 2 and Comparative Example 1 of this invention.

[0018] Figure 8 Stability diagram of the Re-Ni@Ni(OH)2 / CC catalyst prepared in Example 2 of this invention. Detailed Implementation

[0019] To make the present invention clearer and more explicit, the present invention will be further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0020] Example 1

[0021] A method for preparing a multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, the preparation steps are as follows: (1) Commercial carbon cloth (CC) is cut, acid washed and dried for later use; (2) Mix 0.1 mmol ammonium perrhenate, 1.9 mmol nickel chloride, and 20 mL water together until homogeneous; (3) Quickly add 2 mL of hydrazine hydrate to the mixed salt solution and stir for 5 min; (4) Transfer the mixed solution to a hydrothermal reactor, and at the same time place a piece of material with an area of ​​2.5 cm². 2 Place the carbon cloth in the hydrothermal reactor, tighten the lid, and transfer the hydrothermal reactor to the oven; (5) Set the oven heating temperature to 170 ℃ and the heating time to 720 min; (6) After the oven is cooled to room temperature, the carbon cloth is taken out and dried to obtain the target catalyst, which is labeled as Re-Ni@Ni(OH)2 / CC-0.1∶1.9.

[0022] Example 2

[0023] The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0.3 mmol and the amount of nickel chloride is changed to 1.7 mmol; everything else is the same as in Example 1, and the resulting catalyst is labeled as Re-Ni@Ni(OH)2 / CC-0.3∶1.7.

[0024] Example 3

[0025] The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0.5 mmol and the amount of nickel chloride is changed to 1.5 mmol; everything else is the same as in Example 1, and the resulting catalyst is labeled as Re-Ni@Ni(OH)2 / CC-0.5∶1.5.

[0026] Example 4

[0027] The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 1.5 mmol and the amount of nickel chloride is changed to 0.5 mmol; everything else is the same as in Example 1, and the resulting catalyst is labeled as Re-Ni@Ni(OH)2 / CC-1.5∶0.5.

[0028] Compare with Example 1 The difference from Example 1 is that in step (2), the amount of ammonium perrhenate is changed to 0 and the amount of nickel chloride is changed to 2 mmol; everything else is the same as in Example 1, and the resulting catalyst is labeled as Ni@Ni(OH)2 / CC.

[0029] Compare with Example 2 The difference from Example 2 is that in step (2), nickel chloride is replaced with an equimolar amount of copper chloride; everything else is the same as in Example 2, and the resulting catalyst is labeled Re-Cu / CC.

[0030] Compare with Example 3 The difference from Example 2 is that in step (3), the amount of hydrazine hydrate is changed to 0.5 mL; everything else is the same as in Example 2, and the resulting catalyst is labeled Re-Ni / CC.

[0031] Catalyst characterization Figure 1 XRD patterns of the Re-Ni@Ni(OH)2 / CC-0.3∶1.7 catalyst prepared in Example 2 and the Ni@Ni(OH)2 / CC catalyst prepared in Control Example 1. Figure 1 It can be seen that the catalysts prepared in Example 2 and Comparative Example 1 of this invention both showed characteristic peaks of CC and Ni. Ni(OH)2 was not detected in XRD because of its poor crystal form.

[0032] Figure 2 TEM image of the Re-Ni@Ni(OH)2 / CC-0.3∶1.7 catalyst prepared in Example 2. Figure 2 It can be seen that the prepared catalyst is based on carbon cloth, on which nanospheres are grown in situ. The nanospheres have a core-shell structure, with the core being a Ni core (lattice spacing of 0.206 nm) and the shell being Ni(OH)2 (lattice spacing of 0.233 nm).

[0033] Figure 3 The image shows the EDX elemental mapping of the Re-Ni@Ni(OH)2 / CC-0.3∶1.7 catalyst prepared in Example 2. Figure 3 It can be seen that the catalyst prepared by this invention contains Re, indicating that Re has been successfully introduced into the present invention. Moreover, compared with the distribution of Ni, Re is mainly distributed in the middle of the selected region, while there is almost no Re distribution around the region, indicating that Re is mainly located in the Ni core.

[0034] Combination Figure 1-3 It can be seen that, after comparison with the standard card, the product prepared in Example 2 of the present invention is Re-Ni@Ni(OH)2 / CC, and the product prepared in Comparative Example 1 is Ni@Ni(OH)2 / CC.

[0035] Figure 4 XRD patterns of the Re-Cu / CC and Re-Ni / CC catalysts prepared in Comparative Examples 2 and 3 are shown. Figure 4 It can be seen that, after comparison with the standard card, the products prepared in Comparative Examples 2 and 3 are Re-Cu / CC and Re-Ni / CC, respectively, and no corresponding hydroxides are generated. This indicates that changing the type of metal or the amount of hydrazine hydrate will directly affect the composition of the product.

[0036] Catalyst Application (I) Electrocatalytic hydrogen production at all pH levels A single electrolytic cell was used to prepare the catalyst, with a carbon cloth area of ​​1.3 cm². 2 The catalyst, silver chloride, and carbon rod were cut and then used as the working electrode, reference electrode, and counter electrode, respectively. They were placed together in an electrolytic cell, and 30 mL of electrolyte was added to the cell. The electrolyte consisted of 1 M potassium hydroxide solution, 0.5 M H2SO4, and 1 M PBS electrolyte.

[0037] Figure 5 Electrocatalytic hydrogen production at all pH values ​​for the catalysts prepared in Examples 1-4 and Comparative Example 1. Figure 5 It can be seen that the catalyst Re-Ni@Ni(OH)2 / CC-0.3∶1.7 prepared in this invention exhibits good HER activity across the entire pH range, and at a current density of 10 mA cm⁻¹ -2The overpotentials in 1 M KOH, 0.5 M H2SO4, and 1 M PBS were 65, 38, and 71 mV, respectively, which were much lower than those of Re-Ni@Ni(OH)2 / CC-0.1∶1.9 (162, 86, 163 mV), Re-Ni@Ni(OH)2 / CC-0.5∶1.5 (78, 54, 118 mV), Re-Ni@Ni(OH)2 / CC-1.5∶0.5 (199, 151, 228 mV), and Ni@Ni(OH)2 / CC (269, 212, 345 mV). These data indicate that, compared with Control Example 1, the present invention, after introducing an appropriate amount of Re, helps to improve the HER activity of electrocatalytic hydrogen production at all pH, and the optimal Re∶Ni molar ratio is 0.3∶1.7.

[0038] Figure 6 The graph shows the electrocatalytic hydrogen production of the catalysts prepared in Comparative Examples 2 and 3 in 1 M KOH electrolyte. Figure 6 It can be seen that at a current density of 10 mA cm⁻¹ -2 At that time, the overpotential of Re-Cu / CC was 113 mV, and the overpotential of Re-Ni / CC was 155 mV. (This is in conjunction with...) Figure 5 a. It can be seen that: in 1 M KOH, when the proportion of Re is consistent, the HER activity of Re-Ni@Ni(OH)2 / CC-0.3∶1.7 prepared in this invention is significantly better than that of the catalysts prepared in Control Examples 2 and 3.

[0039] (II) Furfural oxidation reaction An H-type electrolytic cell was used, which consisted of two cells, A and B. Cell A contained the working electrode and the reference electrode, while cell B contained the counter electrode. The prepared catalyst was placed on a carbon cloth with a surface area of ​​1.8 cm². 2 The catalyst was cut and then placed in electrolytic cell A as the working electrode and silver chloride as the reference electrode. The carbon rod was placed in electrolytic cell B as the counter electrode. 20 mL of 1 M potassium hydroxide solution containing 50 mM furfural (FF) was added to electrolytic cell A, and 20 mL of 1 M potassium hydroxide solution was added to electrolytic cell B.

[0040] Table 1 shows the furfural conversion rate and furoic acid selectivity obtained after reacting at 1.4 V for 60 min. As shown in Table 1, compared to Control Example 1, the introduction of an appropriate amount of Re in Examples 1-4 of this invention helps improve the furfural oxidation performance, and the optimal Re:Ni molar ratio is 0.3:1.7. When the Re ratio is consistent, the furfural oxidation performance of the catalyst prepared in Example 2 of this invention is significantly better than that of the catalysts prepared in Control Examples 2-3.

[0041]

[0042] Figure 7 The diagram shows the furfural oxidation of the catalysts prepared in Example 2 and Comparative Example 1. Figure 7 It can be seen that, compared with the Ni@Ni(OH)2 / CC prepared in Comparative Example 1, the catalyst Re-Ni@Ni(OH)2 / CC-0.3∶1.7 prepared in Example 2 of this invention exhibits better FOR activity, at a current density of 100 mA cm⁻¹. -2 At that time, the overpotential was 200 mV in 1 M KOH and 50 mM FF, which is much lower than that of Ni@Ni(OH)2 / CC (310 mV).

[0043] (III) Stability Test An H-type electrolytic cell was used, which consisted of two cells, A and B. Cell A contained the working electrode and the reference electrode, while cell B contained the counter electrode. The catalyst prepared in Example 2 was used with a carbon cloth area of ​​1.8 cm². 2 The catalyst was cut and then placed in electrolytic cell A as the working electrode and silver chloride as the reference electrode. A carbon rod was placed in electrolytic cell B as the counter electrode. 20 mL of a 1 M potassium hydroxide solution containing 50 mM furfural (FF) was added to electrolytic cell A, and 20 mL of a 1 M potassium hydroxide solution was added to electrolytic cell B. The voltage was set to 1.4 V, and a constant current test was performed. The electrolyte was replaced with a new one every 60 minutes, and the test was repeated 5 times.

[0044] Figure 8 The results show the furfural conversion rate and furoic acid selectivity obtained from 5 cycles of testing. Figure 8 It can be seen that after 5 cycles of testing, the furfural conversion rate and furoic acid selectivity did not change much, indicating that the catalyst prepared in Example 2 exhibits good stability in furfural oxidation.

Claims

1. A multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC, characterized in that: The catalyst uses carbon cloth as a substrate, on which nanospheres are grown in situ. The nanospheres have a core-shell structure, with the core being a rhenium-regulated nickel core and the shell being nickel hydroxide. The preparation steps of the catalyst are as follows: (1) Commercial carbon cloth is cut, acid-washed and dried for later use; (2) Stir perrhenate, nickel salt, hydrazine hydrate and water together until homogeneous, and transfer the mixed solution to a hydrothermal reactor; (3) Place the carbon cloth obtained in step (1) into a hydrothermal reactor, tighten the reactor lid, react the hydrothermal reactor at 100-250 °C for 300-1000 min, cool to room temperature, remove the carbon cloth, dry it, and the target catalyst is obtained. The ratio of raw materials used in perrhenate (based on the amount of rhenium provided) to nickel salt (based on the amount of nickel provided) is: perrhenate : nickel salt : hydrazine hydrate : water = (0.1-2) mmol : (0.1-2) mmol : (1-3) mL : (10-30) mL. The total number of moles of perrhenate and nickel salt is 2 mmol. The area of ​​the carbon cloth in step (3) is 2-5 cm² for every 2 mmol of perrhenate and nickel salt. 2 .

2. A method for preparing the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC as described in claim 1, characterized in that, The preparation steps are as follows: (1) Commercial carbon cloth is cut, acid-washed and dried for later use; (2) Stir perrhenate, nickel salt, hydrazine hydrate and water together until homogeneous, and transfer the mixed solution to a hydrothermal reactor; (3) Place the carbon cloth obtained in step (1) into a hydrothermal reactor, tighten the reactor lid, react the hydrothermal reactor at 100-250 °C for 300-1000 min, cool to room temperature, remove the carbon cloth, dry it, and the target catalyst is obtained. The ratio of raw materials used in perrhenate (based on the amount of rhenium provided) to nickel salt (based on the amount of nickel provided) is: perrhenate : nickel salt : hydrazine hydrate : water = (0.1-2) mmol : (0.1-2) mmol : (1-3) mL : (10-30) mL. The total number of moles of perrhenate and nickel salt is 2 mmol. The area of ​​the carbon cloth in step (3) is 2-5 cm² for every 2 mmol of perrhenate and nickel salt. 2 .

3. The preparation method of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC as described in claim 2, characterized in that: The nickel salt is nickel nitrate, nickel chloride, or nickel sulfate.

4. The preparation method of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC as described in claim 2, characterized in that: The perrhenate is ammonium perrhenate, potassium perrhenate, or sodium perrhenate.

5. The application of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC as described in claim 1 in the electrocatalytic water splitting for hydrogen production across the entire pH range.

6. The application of the multifunctional electrocatalyst Re-Ni@Ni(OH)2 / CC as described in claim 1 in the furfural oxidation reaction.

Citation Information

Patent Citations

  • Electrochemical preparation method for nickel / nickel hydroxide energy storage electrode material

    CN105244185A

  • Nickel-tin alloy@nickel hydroxide core-shell structure composite material and preparation and application thereof

    CN114023568A