Process for preparing a multi-anion synergistically modified metal layered hydroxide and use thereof
The preparation of multi-anion synergistically modified metal layered hydroxides by a one-step hydrothermal method solves the problem of complex and time-consuming modification methods in the prior art, and achieves a high-efficiency improvement in the catalytic performance of oxygen evolution reaction.
Patent Information
- Application Number
- CN202311256474.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-27
AI Technical Summary
Existing methods for modifying non-precious metal layered hydroxide catalysts are complex, time-consuming, and energy-intensive. The synergistic effect of multiple anions has not been reported, which affects their catalytic performance in the oxygen evolution reaction (OER).
A one-step hydrothermal method was used to synthesize multi-anion synergistic modified metal layered hydroxides. By introducing MoS₄²⁻ anions, SO₄²⁻ and MoO₄S₄-x²⁻ groups were generated under high temperature and high pressure, thus preparing materials with multiple anion co-modification.
In 1M KOH medium, the material exhibits excellent OER performance, with low overpotential and small Tafel slope. The overpotential is only 228 and 270 mV at current densities of 10 and 100 mA cm⁻², respectively, which significantly improves the catalytic activity.
Smart Images

Figure CN117305894B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing and applying a non-precious metal layered hydroxide, and more particularly to a method for preparing and applying a multi-anion synergistically modified metal layered hydroxide. Background Technology
[0002] Electrochemical water splitting is a promising technology for converting renewable electricity into environmentally friendly hydrogen energy. A bottleneck hindering its development lies in the sluggish oxygen evolution reaction (OER) at the cathode, prompting researchers to develop efficient and stable electrocatalysts to accelerate the OER reaction rate. Binary nickel-iron (oxygen) hydroxides are widely considered non-noble metal benchmark catalysts due to their superior catalytic activity and cost-effectiveness, serving as an alternative to noble metal catalysts such as Ru and Ir-based compounds. Furthermore, nickel-iron oxyhydrides (NiFeOOH) formed through in-situ electrochemical self-reconstruction on the catalyst surface have been identified as truly active species. Currently, researchers have proposed numerous methods to enhance the OER activity of nickel-iron (oxygen) hydroxides, such as morphology manipulation, metal cation (Ce, W, Ru) doping, defect fabrication, and induced spin state transitions.
[0003] Recent studies have shown that the intercalation and / or adsorption of oxyanions can enhance the electrocatalytic activity of catalysts by optimizing the energy between the catalyst and OER intermediates through electronic interactions. For example, Liu et al. used a co-precipitation method to intercalate molybdate ions (MoO4) into OER intermediates. 2- Intercalation into nickel-iron layered bimetallic hydroxide nanosheets exhibited excellent OER activity, 100 mA / cm². -2 The overpotential at the current density was only 292 mV. Hu et al. synthesized a p-NiFeMo / NF catalyst using a plasma etching-electrochemical doping strategy at 100 mA / cm². -2 The overpotential at current density was further reduced to 274 mV. They claimed that MoO4 2- Intercalation can prevent excessive oxidation of active β-NiOOH. Researchers also found that adding SO4... 2- Modification in nickel-iron (oxygen) hydroxide, CoFeO x The electronic structure of active sites on Co3O4 and NiFe2O4 can be altered, and intermediates can be stabilized by forming hydrogen bonds, thereby optimizing the adsorption capacity of oxygen-containing intermediates and breaking the adsorption energy ratio of OER.
[0004] However, the aforementioned work mainly investigated the effects of modifying nickel-iron hydroxides with a single type of oxyanion on the catalytic performance of OER, while the synergistic effects of multiple anionic groups have not been reported. Furthermore, existing methods for modifying non-noble metal layered hydroxide (LDH) catalysts typically involve multiple steps, are time-consuming and energy-intensive. Therefore, in the pursuit of a green economy, finding simple and environmentally friendly material synthesis methods is also crucial. Summary of the Invention
[0005] Purpose of the invention: The purpose of this invention is to provide a method for preparing metal layered hydroxides that can achieve multi-anion synergistic modification in one step;
[0006] A second objective of this invention is to provide the application of the metal layered hydroxide prepared by the above method in the OER process.
[0007] Technical solution: The preparation method of the multi-anion synergistic modified metal layered hydroxide of the present invention includes the following steps:
[0008] (1) Prepare a precursor solution by dissolving the metal salt, precipitant, ammonium fluoride and thiomolybdate;
[0009] (2) The precursor solution is mixed with the self-supporting conductive substrate and subjected to a hydrothermal reaction. After the reaction is completed, the self-supporting conductive substrate is removed, cleaned and dried to obtain the multi-anion synergistic modified metal layered hydroxide.
[0010] In step (1), the molar ratio of the metal salt, precipitant, ammonium fluoride and thiomolybdate is 0.4-4:2-20:1-10:0.01-0.5.
[0011] In step (1), the metal salt is one, two, or more; the metal salt is at least one of Ni salt, Fe salt, Co salt, Cu salt, Mn salt, Zn salt, Cr salt, Mg salt, or Al salt. The metal salt includes nickel salt and iron salt, the precipitant is urea or hexamethylenetetramine, and the molar ratio of nickel salt, iron salt, urea, ammonium fluoride or hexamethylenetetramine, and tetrathiomolybdate is 0.3-3:0.1-1:2-20:1-10:0.01-0.5.
[0012] The nickel salt is nickel chloride and / or nickel nitrate; the iron salt is ferric chloride and / or ferric nitrate.
[0013] In step (1), the metal salt, precipitant, ammonium fluoride and thiomolybdate are dissolved in water to prepare a precursor solution.
[0014] In step (2), the temperature of the hydrothermal reaction is 100-180℃ and the time is 8-12h.
[0015] In step (2), the self-supporting conductive substrate is at least one of nickel foam, copper foam, carbon nanofiber, carbon cloth or carbon paper; the self-supporting conductive substrate is used after cleaning; preferably, it is used after ultrasonic cleaning in hydrochloric acid, ethanol and distilled water respectively.
[0016] Application of the multi-anion synergistic modified metal layered hydroxides prepared by the above method in OER catalyst materials.
[0017] Specifically, it is applied to the oxygen evolution process in the fields of water electrolysis for hydrogen production, metal-air batteries, and fuel cells.
[0018] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects: The present invention uses a one-step hydrothermal method to prepare a variety of anion-modified self-supporting nickel-iron hydroxide materials, by introducing MoS4 during the synthesis process. 2- Anions, under high temperature and high pressure hydrothermal reaction conditions, promote the production of most MoS4. 2- The anions degrade to form SO4. 2- and MoO x S 4-x 2- The groups were combined to ultimately obtain a metal layered hydroxide material modified with multiple anionic groups. In 1M KOH medium, the optimized sample exhibited excellent OER performance at current densities of 10 and 100 mA / cm². -2 At that time, its overpotential was only 228 and 270 mV, and it had a dec of 35.5 mV. -1 The low Tafel slope. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the preparation process of the present invention;
[0020] Figure 2 Morphology characterization of the NiFe LDH-MoS4-0.1 / NF sample in Example 2 of this invention;
[0021] Figure 3 Wide-angle (a) and low-angle (b) XRD spectra, (c) FTIR spectra, and (d) Raman spectra of NiFe LDH / NF and NiFe LDH-MoS4-0.1 / NF samples, respectively, are shown for the NiFe LDH / NF sample of Comparative Example 1, the NiFe LDH-MoS4-0.05 / NF sample of Example 1, the NiFe LDH-MoS4-0.1 / NF sample of Example 2, and the NiFe LDH-MoS4-0.2 / NF sample of Example 3.
[0022] Figure 4High-resolution XPS spectra of the samples obtained in Examples 1-3 and Comparative Example 1;
[0023] Figure 5 The graph shows the OER performance test results of the samples obtained in Examples 1-3 and Comparative Example 1;
[0024] Figure 6 The LSV polarization curves of the NiFe LDH-MoO4-0.1 / NF sample in Comparative Example 2 are shown.
[0025] Figure 7 The LSV polarization curves are for the NiFe LDH-SO4-0.1 / NF sample of Comparative Example 3. Detailed Implementation
[0026] The present invention will now be described in further detail.
[0027] Example 1
[0028] Dissolve 3 mmol nickel chloride hexahydrate, 1 mmol ferric nitrate nonahydrate, 20 mmol urea, and 10 mmol ammonium fluoride in 21 mL of water. Then, add 0.05 mmol ammonium tetrathiomolybdate. Finally, mix the mixture with four clean 1×2 cm tablets. 2 The nickel foam was transferred to a 30 mL Teflon-lined reactor, which was then sealed and placed in an oven at 120°C for 8 hours. After the reaction was complete, it was allowed to cool naturally to room temperature. The nickel foam was removed, rinsed three times with water, and dried at 60°C. The resulting sample was labeled NiFe LDH-MoS4-0.05 / NF. Here, LDH represents non-noble metal layered hydroxide, NF represents nickel foam, and 0.05 represents the molar amount of tetrathiomolybdate.
[0029] like Figure 1 As shown, this invention uses a one-step hydrothermal method to prepare SO4. 2- and MoO x S 4-x 2- Self-supporting nickel-iron hydroxide materials modified by multiple anionic groups can be used to accelerate the oxygen evolution reaction.
[0030] Example 2
[0031] Dissolve 3 mmol nickel chloride hexahydrate, 1 mmol ferric nitrate nonahydrate, 20 mmol urea, and 10 mmol ammonium fluoride in 21 mL of water. Then, add 0.1 mmol ammonium tetrathiomolybdate. Finally, mix the mixture with four clean 1×2 cm tablets. 2The nickel foam was transferred to a 30 mL Teflon-lined reactor, which was then sealed and placed in an oven at 120°C for 8 hours. After the reaction was complete, the reactor was allowed to cool naturally to room temperature. The nickel sheet was then removed, rinsed three times with water, and dried at 60°C. The resulting sample was labeled as NiFeLDH-MoS4-0.1 / NF.
[0032] like Figure 2 As shown in Figure a, the scanning electron microscope image of the NiFe LDH-MoS4-0.1 / NF sample reveals numerous densely packed nanosheets vertically grown on the NF framework. Figure 2 As shown in b in the image, the nanosheet structure is clearly visible in the TEM image, with a thickness of approximately 15 nm. Figure 2 As shown in c in the figure, the bright spots in the SAED electron diffraction pattern demonstrate the high crystallinity of the material. Figure 2 As shown in d, the high-resolution TEM (HRTEM) image shows that the lattice spacings of 0.156 nm and 0.152 nm correspond to the (110) and (113) crystal planes of NiFe LDH. Figure 2 As shown in Figure e, the elemental mapping diagrams obtained by high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) and energy-dispersive X-ray analysis (EDS) show that Ni, Fe, O, Mo, and S are uniformly distributed in the nanosheets.
[0033] Example 3
[0034] Dissolve 3 mmol nickel chloride hexahydrate, 1 mmol ferric nitrate nonahydrate, 20 mmol urea, and 10 mmol ammonium fluoride in 21 mL of water. Then, add 0.2 mmol ammonium tetrathiomolybdate. Finally, mix the mixture with four clean 1×2 cm tablets. 2 The nickel foam was transferred to a 30 mL Teflon-lined reactor, which was then sealed and placed in an oven at 120 °C for 8 hours. After the reaction was complete, it was allowed to cool naturally to room temperature. The nickel foam was then removed, rinsed three times with water, and dried at 60 °C. The resulting sample was labeled as NiFe LDH-MoS4-0.2 / NF.
[0035] Example 4
[0036] Dissolve 0.3 mmol nickel nitrate, 0.1 mmol ferric chloride, 2 mmol urea, and 1 mmol ammonium fluoride in 21 mL of water. Then, add 0.01 mmol ammonium tetrathiomolybdate. Finally, mix the mixture with four clean 1×2 cm tablets. 2The nickel foam was transferred to a 30 mL Teflon-lined reactor, which was then sealed and placed in an oven at 100°C for 12 hours. After the reaction was complete, it was allowed to cool naturally to room temperature. The nickel foam was then removed, rinsed three times with water, and dried at 60°C. The resulting sample was labeled as NiFeLDH-MoS4-0.01 / NF.
[0037] Example 5
[0038] Dissolve 3 mmol cobalt nitrate, 1 mmol ferric chloride, 20 mmol urea, and 10 mmol ammonium fluoride in 21 mL of water. Then, add 0.5 mmol ammonium tetrathiomolybdate. Finally, mix the mixture with four clean 1×2 cm tablets. 2 The nickel foam was transferred to a 30 mL Teflon-lined reactor, which was then sealed and placed in an oven at 180°C for 8 hours. After the reaction was complete, it was allowed to cool naturally to room temperature. The nickel foam was then removed, rinsed three times with water, and dried at 60°C. The resulting sample was labeled CoFe-LDH-MoS4-0.5 / NF.
[0039] Comparative Example 1
[0040] Based on Example 2, the difference is that (NH4)2MoS4 was not added during the synthesis process, and the resulting sample was denoted as NiFe LDH / NF.
[0041] Comparative Example 2
[0042] Based on Example 2, the difference is that 0.1 mmol of (NH4)2MoO4 was used instead of (NH4)2MoO4. 4) The resulting sample was denoted as NiFe LDH-MoO4-0.1 / NF.
[0043] Comparative Example 3
[0044] Based on Example 2, the difference is that 0.1 mmol of Na2SO4 was used instead of (NH4+). 4)2 The resulting sample was named NiFe LDH-SO4-0.1 / NF.
[0045] Figure 3 Wide-angle (a) and low-angle (b) XRD spectra of synthesized NiFe LDH / NF, NiFe LDH-MoS4-0.05 / NF, NiFe LDH-MoS4-0.1 / NF and NiFe LDH-MoS4-0.2 / NF, (c) FTIR spectra, and (d) Raman spectra of NiFe LDH / NF and NiFe LDH-MoS4-0.1 / NF.
[0046] The crystal structure of the prepared LDH material was characterized using XRD. For example... Figure 3 As shown in Figure a, three distinct diffraction peaks at 44.5°, 51.8°, and 76.4° belong to the Ni substrate, while the others mainly correspond to NiFe LDH (PDF No. 40-0215). The weaker diffraction peak intensities of the NiFe LDH-MoS4 / NF sample indicate a decrease in crystallinity compared to the original NiFe LDH / NF. Figure 3 In the low-angle XRD patterns (b), it can be observed that compared with NiFe LDH / NF, the diffraction peaks of the (003) plane in NiFe LDH-MoS4-0.05 / NF, NiFe LDH-MoS4-0.1 / NF, and NiFe LDH-MoS4-0.2 / NF shift to lower angles, indicating that the lattice distance of NiFe LDH in the c direction is increased. This may be due to the insertion of anionic groups. The increased lattice distance is beneficial to electrolyte permeation and exposure of active sites. It is worth noting that MoS4 was introduced during the synthesis process. 2- After anionization, a new small peak appeared at 18.3° in the sample, which belongs to the β-NiOOH phase (PDF No. 06-0141). Figure 3 The Fourier transform infrared (FTIR) spectra of the c-axis in the image show that all NiFe LDH-MoS4 / NF samples show a peak density at 457 cm⁻¹. -1 There is a typical peak at 1018 cm⁻¹, corresponding to the Mo-S vibration peak; the other three are located at 1018, 1111, and 1247 cm⁻¹, respectively. -1 Characteristic peaks attributable to sulfate ions. In contrast, the original NiFe LDH does not exhibit these peaks. Figure 3 As shown in d, the Raman spectra of both NiFeLDH / NF and NiFe LDH-MoS4-0.1 / NF show two characteristic peaks located at 458 and 538 cm⁻¹. -1 , respectively corresponding to Ni 2+ The bending vibration (δ(Ni-O)) and stretching vibration (ν(Ni-O)) of Ni-O are located at 290–300 cm⁻¹. -1 The Raman peak can be attributed to the Fe-O vibrational mode. Furthermore, in NiFe LDH-MoS4-0.1 / NF, a peak appears at 803 cm⁻¹. -1 The Raman peak can be attributed to MoO4. 2- The Mo-O stretching vibration mode was observed. Several small peaks were also observed at 420, 606, and 965 cm⁻¹. -1 It can be classified as SO4. 2- The OSO bending vibration and SO stretching vibration modes are observed. Another mode is located at 378 cm⁻¹. -1The new peak may originate from the coordination vibration of Ni / Fe-S.
[0047] X-ray photoelectron spectroscopy (XPS) was used to analyze the surface elemental composition and electronic structure of the samples. Figure 4 a and Figure 4 As can be observed in b, compared with the original NiFe LDH / NF, the Ni and Fe 2p XPS peaks of the NiFe LDH-MoS4 / NF sample show higher binding energies. This change in binding energy indicates the introduction of MoS4 during the synthesis process. 2- This results in the presence of more Ni and Fe in higher valence states in the sample. By fitting the high-resolution Ni 2p peak, it was found that Ni... 3+ The proportion of MoS4 2- The concentration increases with increasing concentration. The metal components in the catalyst are oxidized to higher valence states, which donate more 3d electron orbitals than lower valence states, resulting in higher electron accepting capacity. This is beneficial for improving the electrochemical activity of the OER process. Figure 4 In c, the Mo 3d5 / 2 fitting curve of the NiFeLDH-MoS4 / NF sample can be fitted as Mo 4+ and Mo 6+ Two peaks. The observed increase in the valence states of Ni and Fe, accompanied by a decrease in the valence state of Mo, indicates a charge transfer process from Ni / Fe to Mo, suggesting a strong electronic interaction between NiFe LDH and the inserted anionic groups in the composite material. From Figure 4 As can be seen from d, the high-resolution S2p spectrum can be fitted with three peaks. The two peaks at lower binding energies correspond to MoS4 and MoO. x S 4-x S in the group 2- The high binding energy main peak at 168.6 eV belongs to SO4. 2- Based on this, it can be inferred that most of the thiomolybdate anions are oxidized during the synthesis process, generating thiomolybdate oxide and sulfate anions. These anionic groups insert into and / or adsorb onto the LDH material, potentially further promoting the OER activity of the LDH material. Electrochemical testing:
[0048] Electrochemical measurements were performed using an electrochemical workstation (CHI 760e, Shanghai Chenhua) equipped with a standard three-electrode system. In this setup, a graphite rod and a Hg / HgO (1M KOH) electrode served as the counter and reference electrodes, respectively. The prepared sample (area: 1 × 1 cm²) was... 2 It was used directly as the working electrode. Linear sweep voltammetry (LSV) was used in oxygen-saturated 1M KOH medium at a rate of 5 mV / s. -1The OER polarization curve was obtained by scanning at a certain rate. The AC impedance (EIS) was measured using an AC amplitude of 5 mV over a frequency range of 100 kHz to 0.1 Hz.
[0049] Figure 5 The electrocatalytic OER performance of the sample of this invention in 1M KOH electrolyte. (a) LSV polarization curves; (b) 10, 50 and 100 mA cm⁻¹ -2 Comparison of overpotentials at current densities; (c) Tafel slope; (d) Double-layer capacitance (C dl (e) Comparison of TOF values at 1.5V; (f) Stability test of NiFe LDH-MoS4-0.1 / NF catalyst at 1.458V. Figure 5 It can be seen that among all catalysts, NiFe LDH-MoS4-0.1 / NF has the best performance at 10, 50, and 100 mA cm⁻¹. -2 The overpotentials at which the OER activity was achieved were 228, 253, and 270 mV, respectively, exhibiting the best OER activity. NiFeLDH-MoS4-0.05 / NF showed slightly worse performance, but was superior to NiFe LDH-MoS4-0.2 / NF. In contrast, NiFe LDH / NF required maximum overpotentials of 257, 356, and 456 mV to achieve 10, 50, and 100 mA / cm², respectively. -2 The current density. Under the same conditions, the NiFe LDH-MoO4-0.1 / NF control sample required overpotentials of 250, 325, and 370 mV to obtain 10, 50, and 100 mA cm⁻¹. -2 The current density, such as Figure 6 As shown. On the other hand, to obtain the same current density, NiFe LDH-SO4-0.1 / NF requires overpotentials of 235, 286, and 319 mV, respectively, as... Figure 7 As shown.
[0050] These results indicate that the introduction of a certain oxyanion, such as MoO4, is related to... 2- or SO4 2- Compared to other modified materials, the metal layered hydroxide material modified with multiple anions of this invention exhibits better OER performance.
Claims
1. A method for preparing a multi-anion synergistically modified metal layered hydroxide, characterized in that, Includes the following steps: (1) Prepare a precursor solution by dissolving the metal salt, precipitant, ammonium fluoride and tetrathiomolybdate; (2) The precursor solution is mixed with the self-supporting conductive substrate and subjected to a hydrothermal reaction. After the reaction is completed, the self-supporting conductive substrate is removed, cleaned and dried to obtain the multi-anion synergistic modified metal layered hydroxide.
2. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 1, characterized in that, The molar ratio of the metal salt, precipitant, ammonium fluoride and tetrathiomolybdate is 0.4~4:2~20:1~10:0.01~0.
5.
3. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 1, characterized in that, In step (2), the temperature of the hydrothermal reaction is 100~180℃ and the time is 8~12 h.
4. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 1, characterized in that, In step (1), the metal salt is a nickel salt and an iron salt, or a cobalt salt and an iron salt.
5. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 1, characterized in that, In step (1), the metal salt includes nickel salt and iron salt, the precipitant is urea or hexamethylenetetramine, and the molar ratio of nickel salt, iron salt, urea or hexamethylenetetramine, ammonium fluoride and tetrathiomolybdate is 0.3~3:0.1~1:2~20:1~10:0.01~0.
5.
6. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 5, characterized in that, The nickel salt is nickel chloride and / or nickel nitrate; the iron salt is ferric chloride and / or ferric nitrate.
7. The method for preparing multi-anion synergistically modified layered metal hydroxides according to claim 1, characterized in that, In step (2), the self-supporting conductive substrate is at least one of nickel foam, copper foam, carbon nanofibers, carbon cloth, or carbon paper.
8. The application of a multi-anion synergistically modified metal layered hydroxide prepared by the method of claim 1 in OER catalyst materials.
9. The application of the multi-anion synergistic modified metal layered hydroxide according to claim 8 in OER catalyst materials, characterized in that, Oxygen evolution process used in water electrolysis for hydrogen production, metal-air batteries, and fuel cells.