Glassine paper having good heat sealability and water barrier property and a method for manufacturing the same
By coating the surface of cellophane with a specific ratio of emulsion, the problems of insufficient heat-sealing performance and high water vapor permeability of cellophane are solved, achieving good heat-sealing and water-blocking properties, making it suitable for food packaging and supporting resource recycling.
Patent Information
- Application Number
- CN202311200985.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-18
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-18
AI Technical Summary
Existing cellophane has shortcomings in heat-sealing performance, which cannot meet the needs of food packaging. At the same time, its high water vapor permeability makes it unable to effectively prevent moisture loss.
By coating the cellophane surface with a specific ratio of coating emulsion, including a mixture of EAA emulsion, carbamate wax emulsion, carboxymethyl cellulose, vinyl silane coupling agent, bactericide and defoamer, chemical bonding is formed to improve heat sealability and water resistance, and the coating thickness is controlled at 5-8 μm.
It achieves excellent heat-sealing performance and low water vapor permeability of cellophane at high temperatures, meeting the requirements of food packaging. Furthermore, the coating has good stability, is not easy to peel off, and supports resource recycling.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically relating to a cellophane with good heat-sealing and water-blocking properties and its manufacturing method. Background Technology
[0002] In recent years, due to the excessive use of plastic bags and inadequate recycling, serious resource waste and environmental pollution have gradually occurred. In particular, some ultra-thin plastic shopping bags are easily damaged and are mostly discarded carelessly after use, making non-degradable plastic bags a major source of "white pollution." More and more countries and regions have restricted or stopped the production, sale, and use of plastic shopping bags. Cellophane is an environmentally friendly, biodegradable cellulose film. With the continuous expansion of cellophane product applications in the market, in the food packaging industry, cellophane with water vapor barrier properties and high heat-sealing strength can prevent water vapor in the air and food from absorbing moisture, thereby reducing moisture loss and extending food shelf life. Chinese patent CN200980139574.4 discloses a polysiloxane composition that can be used to coat cellophane. Its coating can form a cross-linked coating on cellophane with improved water resistance, mechanical strength, and reactivity, but the heat-sealing performance on cellophane is not improved. Summary of the Invention
[0003] In view of this, the present invention provides a cellophane with good heat-sealing and water-blocking properties and a method for manufacturing the same. The cellophane has good heat-sealing performance at a certain temperature, while the water vapor permeability can meet the packaging standards for use in the food industry.
[0004] A type of cellophane with good heat-sealing and water-resistant properties is made by coating cellophane with a coating emulsion formulated from raw materials comprising the following mass percentages: 60-70% EAA emulsion, 10-17% carnauba wax emulsion, 0.4-0.8% carboxymethyl cellulose, 0.6-0.9% vinyl silane coupling agent, 1.7-3% bactericide, 0.3-1% defoamer, and 16-20% soft water.
[0005] Preferably, the degree of substitution of the carboxymethyl cellulose is 0.3 to 0.9, and the pH value is 6.5 to 8.
[0006] Preferably, the solid content of the EAA emulsion is 30-35%; and the solid content of the carnauba wax emulsion is 20-25%.
[0007] Preferably, the thickness of the cellophane is 70–90 μm; the coating thickness is 5–8 μm.
[0008] Preferably, the vinylsilane coupling agent is PU116 or PU118.
[0009] Preferably, the bactericide is an MBS series bactericide; the defoamer is an organosilicon defoamer.
[0010] A method for manufacturing cellophane with good heat-sealing and water-blocking properties includes the following steps: (1) Adding carboxymethyl cellulose to soft water and stirring at a temperature of 75-80°C and a stirring speed of 400-500 r / min until no precipitate is obtained, thus obtaining solution A; (2) After solution A is cooled to room temperature, EAA emulsion is added to solution A and stirred for 15 min at a stirring speed of 500-600 r / min, then carnauba wax emulsion is added and stirred for 10 min, and then vinyl silane coupling agent and bactericide are added and stirred for 5 min at a stirring speed of 400-450 r / min, then defoamer is added, and stirring is continued for 5 min before discharging, thus obtaining the coating emulsion; (3) Coating the coating emulsion onto the surface of cellophane using a coating machine and drying it at 100-110°C for 5-7 s, thus obtaining cellophane with good heat-sealing and water-blocking properties.
[0011] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0012] The carnauba wax emulsion of this invention is a good oily wax emulsion with excellent water-blocking properties, while the EAA emulsion is a watery emulsion with heat-sealing properties. After the two are miscible under stirring, oil-water separation occurs after a period of standing. The added carboxymethyl cellulose reduces the surface tension between water and oil, slows down the rate of oil phase aggregation, and prevents fat droplets from agglomerating and floating, thus ensuring the oil remains stable in water and improving the stability of the coating emulsion. The added vinyl silane coupling agent first undergoes a hydrolysis reaction in the coating emulsion to form silanol. After the coating emulsion is applied to cellophane, the silanol reacts with the hydroxyl groups on the cellophane surface to form hydrogen bonds, and then dehydrates during the drying and curing process to form silicon-oxygen bonds. The chemical bonding force formed between the coating and the cellophane improves the adhesion of the coating to the cellophane, ensuring the coating does not peel off and fully utilizing its heat-sealing and water-blocking properties. Furthermore, vinyl groups are cationic hydrophobic groups; the addition of the vinyl silane coupling agent further enhances the water-blocking properties of the coating.
[0013] The preferred coating thickness during coating in this invention is 5–8 μm. A coating that is too thin will result in insufficient heat-sealing strength and excessive water vapor permeability; a coating that is too thick will result in excessive heat-sealing strength, making the heat-sealed opening prone to tearing and causing paper fibers to fall out, which does not meet food packaging requirements. This invention can be used to prepare food packaging bags, which can be recycled for papermaking after use. The coating on the cellophane can be used as a filler for the cellophane, achieving resource recycling. Detailed Implementation
[0014] To better understand the technical content of this invention, specific embodiments will be provided below to further illustrate the invention.
[0015] Example 1
[0016] A cellophane with good heat-sealing and water-resistant properties is made by coating cellophane with a coating emulsion formulated from raw materials comprising the following mass percentages: 60% EAA emulsion, 17% carnauba wax emulsion, 0.8% carboxymethyl cellulose, 0.6% vinyl silane coupling agent, 3% bactericide, 0.6% defoamer, and 18% soft water. Further, the degree of substitution of carboxymethyl cellulose is 0.8, and the pH value is 6.5; the solid content of the EAA emulsion is 30%, and the solid content of the carnauba wax emulsion is 25%; the vinyl silane coupling agent is PU118; the bactericide is an MBS series bactericide; and the defoamer is an organosilicone defoamer.
[0017] A method for manufacturing cellophane with good heat-sealing and water-resistant properties includes the following steps: (1) adding 0.8% carboxymethyl cellulose to 18% soft water and stirring at 75°C and 400 r / min until no precipitate is obtained, to obtain solution A; (2) after solution A has cooled to room temperature, adding 60% carboxymethyl cellulose to solution A at a stirring speed of 500 r / min. Stir the EAA emulsion for 15 minutes, then add 17% carnauba wax emulsion and stir for 10 minutes. Then, under the condition of stirring speed of 400 r / min, add 0.6% vinyl silane coupling agent and 3% bactericide and stir for 5 minutes. Then add 0.6% defoamer and continue stirring for 5 minutes before discharging. The coating emulsion is obtained and does not separate when left to stand. (3) Coat the coating emulsion onto the surface of cellophane using a coating machine. The thickness of the cellophane is 70 μm and the coating thickness is 5 μm. Dry it at 100°C for 6 seconds to obtain cellophane with good heat-sealing and water-resistant properties.
[0018] Example 2
[0019] A cellophane with good heat-sealing and water-resistant properties is made by coating cellophane with a coating emulsion formulated from raw materials comprising the following mass percentages: 65% EAA emulsion, 11% carnauba wax emulsion, 0.4% carboxymethyl cellulose, 0.9% vinyl silane coupling agent, 1.7% bactericide, 1% defoamer, and 20% soft water. Further, the degree of substitution of carboxymethyl cellulose is 0.3, and the pH value is 7; the solid content of the EAA emulsion is 30%, and the solid content of the carnauba wax emulsion is 25%; the vinyl silane coupling agent is PU116; the bactericide is an MBS series bactericide; and the defoamer is an organosilicon defoamer.
[0020] A method for manufacturing cellophane with good heat-sealing and water-resistant properties includes the following steps: (1) adding 0.4% carboxymethyl cellulose to 20% soft water and stirring at 80°C and 400 r / min until no precipitate is obtained, to obtain solution A; (2) after solution A has cooled to room temperature, adding 65% EAA emulsion to solution A and stirring for 15 min at a stirring speed of 600 r / min, and then adding 11% carnauba wax emulsion and stirring for 10 min. min, and then under the condition of stirring speed of 400r / min, add 0.9% vinyl silane coupling agent and 1.7% bactericide and stir for 5min, then add 1% defoamer and continue stirring for 5min to discharge the material, and the coating emulsion is obtained. The coating emulsion does not separate when left to stand; (3) The coating emulsion is coated on the surface of cellophane by a coating machine. The thickness of the cellophane is 90μm and the coating thickness is 7μm. It is dried at 110℃ for 5s to obtain cellophane with good heat sealing and water resistance.
[0021] Example 3
[0022] A cellophane with good heat-sealing and water-resistant properties is made by coating cellophane with a coating emulsion formulated from raw materials comprising the following mass percentages: 70% EAA emulsion, 10% carnauba wax emulsion, 0.6% carboxymethyl cellulose, 0.7% vinyl silane coupling agent, 2.4% bactericide, 0.3% defoamer, and 16% soft water. Further, the degree of substitution of carboxymethyl cellulose is 0.9, and the pH value is 8; the solid content of the EAA emulsion is 35%, and the solid content of the carnauba wax emulsion is 20%; the vinyl silane coupling agent is PU116; the bactericide is an MBS series bactericide; and the defoamer is an organosilicon defoamer.
[0023] A method for manufacturing cellophane with good heat-sealing and water-resistant properties includes the following steps: (1) adding 0.6% carboxymethyl cellulose to 16% soft water and stirring at 80°C and 500 r / min until no precipitate is obtained, to obtain solution A; (2) after solution A has cooled to room temperature, adding 70% EAA emulsion to solution A and stirring for 15 min at a stirring speed of 600 r / min, and then adding 10% carnauba wax emulsion and stirring for 10 min. In, then under the condition of stirring speed of 450r / min, add 0.7% vinyl silane coupling agent and 2.4% bactericide and stir for 5min, then add 0.3% defoamer and continue stirring for 5min to discharge the material, and the coating emulsion is obtained. The coating emulsion does not separate when left to stand; (3) Coat the coating emulsion onto the surface of cellophane using a coating machine. The thickness of the cellophane is 80μm and the coating thickness is 8μm. Dry it at 105℃ for 7s to obtain cellophane with good heat sealing and water resistance.
[0024] Comparative Example 1
[0025] In Example 2, carboxymethyl cellulose was replaced with sodium alginate, while other raw materials and manufacturing methods remained the same as in Example 2. The resulting coating emulsion was allowed to stand for 30 minutes to separate into layers.
[0026] Comparative Example 2
[0027] The vinyl silane coupling agent in Example 2 was replaced with an amino silane coupling agent, while other raw materials and manufacturing methods remained the same as in Example 2. The resulting coating emulsion did not separate upon standing.
[0028] Comparative Example 3
[0029] The carnauba wax emulsion in Example 2 was replaced with McMen 180 wax emulsion, while other raw materials and manufacturing methods remained the same as in Example 2. The resulting coating emulsion did not separate upon standing.
[0030] The cellophane prepared in Examples 1-3 and Comparative Examples 1-3, as well as cellophane without emulsion coating, were subjected to performance testing. The results are shown in the table below:
[0031]
[0032] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A type of cellophane with good heat-sealing and water-resistant properties, characterized in that: The coating is prepared by coating cellophane with a coating emulsion containing the following raw materials in the indicated mass percentages: 60-70% EAA emulsion, 10-17% carnauba wax emulsion, 0.4-0.8% carboxymethyl cellulose, 0.6-0.9% silane coupling agent, 1.7-3% bactericide, 0.3-1% defoamer, and 16-20% soft water; the degree of substitution of the carboxymethyl cellulose is 0.3-0.9, and the pH value is 6.5-8; the solid content of the EAA emulsion is 30-35%; the solid content of the carnauba wax emulsion is 20-25%; the silane coupling agent is PU118; and the coating thickness during coating is 5-8 μm.
2. The cellophane with good heat-sealing and water-resistant properties according to claim 1, characterized in that: The thickness of the cellophane is 70~90μm.
3. The cellophane with good heat-sealing and water-blocking properties according to claim 1, characterized in that: The bactericide is an MBS series bactericide; the defoamer is an organosilicon defoamer.
4. The method for manufacturing cellophane with good heat-sealing and water-resistant properties according to claim 1, characterized in that: Includes the following steps: (1) Add carboxymethyl cellulose to soft water and stir at a temperature of 75~80℃ and a stirring speed of 400~500r / min until no precipitate is obtained to obtain solution A; (2) After solution A cools to room temperature, add EAA emulsion to solution A and stir for 15 minutes at a stirring speed of 500~600 r / min, then add carnauba wax emulsion and stir for 10 minutes. Then add silane coupling agent and bactericide at a stirring speed of 400~450 r / min and stir for 5 minutes. Then add defoamer and continue stirring for 5 minutes before discharging to obtain the coating emulsion. (3) Coat the coating emulsion onto the surface of cellophane using a coating machine and dry it at 100~110℃ for 5~7 seconds to obtain cellophane with good heat-sealing and water-resistant properties.
Citation Information
Patent Citations
Polysiloxane compositions for coating flexible supports forming crosslinked coatings with improved adhesion, mechanical strength and reactivity
CN102482532B
Acrylate barrier emulsion capable of reducing surface tension of paper-based material and preparation method thereof
CN116199816A
Coating and method for forming the same
US20180346611A1
Water-resistant oil-resistant heat seal paper
WO2022024845A1