Semiconductor device
By introducing a buffer layer with a specific impurity concentration distribution into the semiconductor substrate of the IGBT, the oscillation problem of the IGBT at cutoff time is solved, improving productivity and withstand voltage performance.
Patent Information
- Application Number
- CN202310741424.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-27
- Filing Date
- 2023-06-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-21
AI Technical Summary
Existing technologies struggle to effectively suppress oscillations in IGBTs during cutoff, especially those caused by electric field concentration at the boundary between the proton layer and the drift layer.
A first buffer layer with a specific impurity concentration distribution, including a first region, a second region, and a third region, is introduced into the semiconductor substrate of the IGBT. A gentle impurity concentration gradient is formed by proton injection, which ensures that the extension of the depletion layer stops slowly in time and space, preventing carrier retention.
It effectively prevents IGBT oscillations at cutoff, improves productivity, reduces product costs, and enhances voltage resistance.
Smart Images

Figure CN117316996B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to semiconductor devices, and more particularly to semiconductor devices containing protons as impurities. Background Technology
[0002] For example, the Insulated Gate Bipolar Transistor (IGBT):
[0003] For vertical semiconductor devices such as IGBTs, the switching from an on-state to a non-on-state is performed by stopping the extension of the depletion layer at a predetermined depth. This switching is called the cutoff operation. Surge voltages may occur during the cutoff operation. Furthermore, oscillations may occur due to these surge voltages. As a technique for successfully suppressing surge voltages or oscillations, proton implantation into silicon (Si) wafers has been proposed. It is widely known that proton implantation into silicon and subsequent heat treatment can generate donors beneficial to n-type conductivity.
[0004] According to Japanese Patent Application Publication No. 2016-009868 (Patent Document 1), from the viewpoint of suppressing on / off oscillations, a vertical variation in the doping distribution of the drift layer is beneficial. Therefore, the use of radiation-induced donors is considered. Specifically, the wafer is irradiated with high-energy particles, such as protons, and donors are generated corresponding to the implanted damage concentration distribution through subsequent heat treatment.
[0005] According to Japanese Patent Application Publication No. 2013-138172 (Patent Document 2), a vertical semiconductor device comprises: an n-type drift layer; an n-type or p-type semiconductor region formed on the back side of the drift layer; an n-type field-stop layer formed at a deeper location from the back side of the semiconductor substrate compared to the semiconductor region, having a higher impurity concentration than the drift layer; a p-type region formed on the surface side of the drift layer; an upper electrode formed on the surface side of the drift layer and in contact with the p-type region; and a lower electrode formed on the back side of the drift layer and in contact with the semiconductor region. The field-stop layer comprises a phosphorus / arsenic layer doped with phosphorus or arsenic and a proton-doped proton layer. The phosphorus / arsenic layer is formed at a predetermined depth from the back side of the semiconductor substrate. The proton layer has a concentration peak within the phosphorus / arsenic layer, is formed deeper than the phosphorus / arsenic layer, and is formed with a concentration distribution that slowly decreases in impurity concentration at locations deeper than the phosphorus / arsenic layer.
[0006] According to the claims in the aforementioned literature, firstly, the field cutoff layer is composed of a phosphorus / arsenic layer and a proton layer, and the impurity concentration in the proton layer decreases slowly. Therefore, compared to the case where the field cutoff layer is composed solely of protons, the impurity concentration in the proton layer can be reduced. Thus, compared to the case where the field cutoff layer is constructed by injecting only protons, productivity can be improved, and product cost deterioration can be prevented. Secondly, at a depth deeper than the phosphorus / arsenic layer, the concentration distribution of n-type impurities in the proton layer continuously and slowly decreases, thus reducing the difference in n-type impurity concentration at the boundary between the proton layer and the drift layer. Therefore, electric field concentration can be mitigated, withstand voltage can be ensured, and switching surges can be suppressed.
[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-009868
[0008] Patent Document 2: Japanese Patent Application Publication No. 2013-138172
[0009] The technology disclosed in Japanese Patent Application Publication No. 2013-138172 claims that the difference in n-type impurity concentration at the boundary between the proton layer and the drift layer is reduced, thereby suppressing on / off surges. However, in this technology, the concentration of the proton layer has a peak within the phosphorus / arsenic layer, and then slowly decreases towards the drift layer from that position. Therefore, this technology does not ideally result in a structure where the peak of the proton concentration is formed at a deeper location in the substrate. In such a structure, according to the inventors' research based on the present invention, it is difficult to sufficiently suppress oscillations. Summary of the Invention
[0010] The present invention was proposed to solve the above-mentioned problems, and its purpose is to provide a semiconductor device that can effectively prevent oscillations during cutoff.
[0011] One aspect of the present invention relates to a semiconductor device comprising: a first electrode layer; a second electrode layer separated from the first electrode layer in a thickness direction; and a semiconductor substrate having a first main surface and a second main surface opposite to the first main surface in the thickness direction, the first main surface contacting the first electrode layer and the second main surface contacting the second electrode layer. The semiconductor substrate comprises: an n-shaped drift layer; and a first buffer layer, also n-shaped, disposed between the first main surface and the drift layer. The first buffer layer comprises: a first region containing protons, the first region having an impurity concentration higher than that of the drift layer, and contacting the drift layer; a second region containing protons, the second region having an impurity concentration higher than that of the drift layer, disposed between the first region and the first main surface, and contacting the first region; and a third region disposed between the second region of the first buffer layer and the first main surface of the semiconductor substrate. The first buffer layer has an impurity concentration distribution that depends on the depth distance measured from the first main surface along the thickness direction. The impurity concentration distribution has: a maximum value in the second region, which is the maximum value of the impurity concentration distribution in the first buffer layer; a bend at the boundary point between the first and second regions where the decrease from the maximum value is mitigated or stopped; and a value greater than or equal to 80% of the maximum value.
[0012] The value at the boundary point is % of the value at the boundary point; and the value in the third region, within a range greater than or equal to 5 μm, is lower than the value at the boundary point and less than or equal to 5.0 × 10⁻⁶. 14 / cm 3 The distribution of impurity concentrations.
[0013] The effects of the invention
[0014] According to one aspect of the present invention, a semiconductor device is capable of effectively preventing oscillations during cutoff. Attached Figure Description
[0015] Figure 1 This is a cross-sectional view that schematically illustrates the structure of the semiconductor device according to Embodiment 1.
[0016] Figure 2 It means Figure 1 A graph showing an example of the impurity concentration distribution near the back side of a semiconductor substrate.
[0017] Figure 3 It is a cross-sectional view that roughly shows the structure of a comparative semiconductor device.
[0018] Figure 4 It means Figure 3A graph showing an example of the impurity concentration distribution near the back side of a semiconductor substrate.
[0019] Figure 5 This is a graph representing an example of a cutoff waveform obtained through simulation of a comparative semiconductor device.
[0020] Figure 6 This is a graph showing an example of a cutoff waveform obtained by simulation of the semiconductor device according to Embodiment 1.
[0021] Figure 7 This is a cross-sectional view that schematically shows the structure of the semiconductor device involved in the first variation of Embodiment 1.
[0022] Figure 8 It means Figure 7 A graph showing an example of the impurity concentration distribution near the back side of a semiconductor substrate.
[0023] Figure 9 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0024] Figure 10 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0025] Figure 11 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0026] Figure 12 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0027] Figure 13 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0028] Figure 14 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0029] Figure 15 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0030] Figure 16 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0031] Figure 17 It is shown in general terms. Figure 7 A cross-sectional view of one step in the manufacturing process of a semiconductor device.
[0032] Figure 18 This is a graph showing the impurity concentration distribution of a semiconductor device obtained by a manufacturing method involving two proton implantation processes into a semiconductor substrate, measured using resistance measurement. The semiconductor substrate has a higher density than... Figure 19 The situation is a low oxygen concentration.
[0033] Figure 19 This is a graph showing the impurity concentration distribution of a semiconductor device obtained by a manufacturing method involving two proton implantation processes into a semiconductor substrate, measured using resistance measurement. The semiconductor substrate has a higher density than... Figure 18 High oxygen concentration.
[0034] Figure 20 It is a graph showing the measurement results of the relationship between the oxygen concentration of the semiconductor substrate before wafer processing and the peak value of the Gaussian approximation of the first region of the first buffer layer.
[0035] Figure 21 It is a graph showing the relationship between the oxygen concentration on the surface of the semiconductor substrate after wafer processing and the gate withstand voltage.
[0036] Figure 22 This is a cross-sectional view that schematically illustrates the structure of the semiconductor device involved in the second variation of Embodiment 1.
[0037] Figure 23 It means Figure 22 A graph showing an example of the impurity concentration distribution near the back side of a semiconductor substrate.
[0038] Figure 24 This is a cross-sectional view that schematically illustrates the structure of the semiconductor device involved in Embodiment 2. Detailed Implementation
[0039] The embodiments will now be described based on the accompanying drawings. Furthermore, in the following drawings, the same or corresponding parts will be labeled with the same reference numerals, and their descriptions will not be repeated. In this specification, unless otherwise specified, the impurity concentration of the semiconductor substrate refers to the effective impurity concentration. In the n-type region, the effective impurity concentration is the concentration obtained by subtracting the effective acceptor concentration from the effective donor concentration; in the p-type region, it is the concentration obtained by subtracting the effective donor concentration from the effective acceptor concentration. In the case of non-proton impurities (impurities other than protons), the effective concentration is the concentration of activated impurities; in the case of protons, it is the concentration of donors generated by protons.
[0040] <Implementation Method 1>
[0041] Figure 1 This is a cross-sectional view that schematically shows the structure of the IGBT 901 (semiconductor device) according to Embodiment 1. Figure 2 It means Figure 1 A graph showing an example of the impurity concentration distribution near the back surface MS1 (first main surface) of wafer 101 (semiconductor substrate).
[0042] IGBT 901 has: a collector electrode layer 201 (first electrode layer); and an emitter electrode layer 202 (second electrode layer), which, in the thickness direction ( Figure 1 Separated from the collector electrode layer 201 in the longitudinal direction; and a wafer 101 (semiconductor substrate) having a back surface MS1 (first main surface) in contact with the collector electrode layer 201, and an upper surface MS2 in contact with the emitter electrode layer 202 and opposite to the back surface MS1 in the thickness direction.
[0043] (Second main surface). Furthermore, the IGBT 901 has a gate structure, specifically, it has a gate electrode 203, a gate oxide film 301 (gate insulating film) and an interlayer insulating film 302.
[0044] The wafer 101 may be a silicon wafer. The wafer 101 includes an n-shaped drift layer 190 and an n-shaped first buffer layer 110. In this embodiment, the wafer 101 also includes an n-shaped second buffer layer 120.
[0045] Furthermore, when the semiconductor device is an IGBT, as a desired structure, the wafer 101 includes: a p-type p-base layer 141; n + Emitter layer 151 is n-type and has a higher impurity concentration than drift layer 190; p + A p-type contact layer 152 has a higher impurity concentration than the p-type base layer 141; and a p-type collector layer 131. The collector layer 131 is disposed on the back surface MS1 and functions as a carrier injection layer. In summary, the collector layer 131, the second buffer layer 120, the first buffer layer 110, the drift layer 190, and the p-type base layer 141 are sequentially stacked from the back surface MS1 toward the upper surface MS2. Additionally, an n-type contact layer is disposed on the upper surface MS2. + Emitter layer 151 and p + Contact layer 152.
[0046] Gate electrode 203 in n + The emitter layer 151 and the drift layer 190 are separated by a gate oxide film 301 and face the p base layer 141. Figure 1The IGBT 901 shown has a trench-type gate structure, whereby the wafer 101 has a trench extending from the upper surface MS2 to the drift layer 190. A gate electrode 203 is buried within this trench, separated by a gate oxide film 301. An emitter electrode layer 202 is disposed on the upper surface MS2, adjacent to n... + Emitter layer 151 and p + Contact layer 152 makes contact. Interlayer insulating film 302 insulates the emitter electrode layer 202 from the gate electrode 203. The impurity concentration of the p-base layer 141 can be determined by the threshold voltage of the on / off state achieved by the gate configuration; for example, at approximately 6V, the peak impurity concentration can be greater than or equal to 8 × 10⁻⁶. 16 / cm 3 And less than or equal to 5×10 17 / cm 3 .
[0047] A first buffer layer 110 is disposed between the back surface MS1 and the drift layer 190. The first buffer layer 110 has, sequentially from the upper surface MS2 towards the back surface MS1, a first region 111, a second region 112, and a third region 113. The first region 111 is in contact with the drift layer 190. The first region 111 contains protons for donor generation and has a higher impurity concentration than the impurity concentration of the drift layer 190. The impurity concentration of the first region 111 can be less than or equal to 1 × 10⁻⁶. 15 / cm 3 A second region 112 is disposed between the first region 111 and the back surface MS1, and is in contact with the first region 111. The second region 112 contains protons for generating donors and has an impurity concentration higher than that of the drift layer 190. A third region 113 is disposed between the second region 112 and the back surface MS1 of the wafer 101. The third region 113 may contain protons for generating donors and may have an impurity concentration higher than that of the drift layer 190.
[0048] The first buffer layer 110 has an impurity concentration distribution that depends on the depth distance measured from the back side MS1 along the thickness direction. Figure 2 The impurity concentration distribution of the first buffer layer 110 has the following characteristics.
[0049] First: The impurity concentration distribution of the first buffer layer 110 has a maximum value in the second region 112, which is the maximum value of the impurity concentration distribution of the first buffer layer 110. In other words, the location of the maximum value of the impurity concentration distribution of the first buffer layer 110 is located within the second region 112. The distance from the back surface MS1 to this location can be greater than or equal to 10 μm. Figure 2 In the example shown, the value is greater than or equal to 20 μm.
[0050] Second: The impurity concentration distribution of the first buffer layer 110 has a bend at the boundary point KN between the first region 111 and the second region 112, where the decrease from the aforementioned maximum value is mitigated or stopped. In other words, the decrease from the aforementioned maximum value is mitigated or stopped by the bend at the boundary point KN between the first region 111 and the second region 112. Figure 2 In the example shown, as the distance from the back side, as shown by the horizontal axis of the curve, increases, the impurity concentration decreases from its maximum value, and at the boundary point KN, this decrease roughly stops, then decreases again. The decrease in impurity concentration from its maximum value does not necessarily have to stop at the boundary point KN, as long as it is at least mitigated. Furthermore, it is not necessary for the decrease to transition to an increase at the boundary point KN.
[0051] Here, in Figure 2 In the graph, the impurity concentration represented by the vertical axis is denoted as N, and the distance from the back side represented by the horizontal axis is denoted as Z. Imagine a function f that satisfies N = f(Z). Furthermore, the position on the horizontal axis corresponding to the aforementioned maximum value is denoted as Z. MAX Let Z corresponding to the boundary point KN be represented as Z. KN Let Z be the position where the drift layer 190 reaches the first region 111. drft Under these definitions, Z satisfies MAX <Z KN <Z drft Furthermore, in Z=Z KN When, the second differential d 2 N / dZ 2 It can have a positive maximum value.
[0052] Third: The impurity concentration distribution of the first buffer layer 110 has a boundary point KN value that is greater than or equal to 80% of the aforementioned maximum value. In other words, the value at the boundary point KN of the impurity concentration distribution of the first buffer layer 110 is greater than or equal to 80% of the aforementioned maximum value. Therefore, the increase in the half-width at half-maximum (WHM) of the first buffer layer 110 caused by the bend at the boundary point KN is sufficiently obtained. The value at the boundary point KN of the impurity concentration distribution of the first buffer layer 110 can be less than or equal to 1 × 10⁻⁶. 15 / cm 3 .
[0053] Fourth: The impurity concentration distribution of the first buffer layer 110, which is the third region 113, shows a value lower than that at the boundary point KN and less than or equal to 5.0 × 10⁻⁶ within a range greater than or equal to 5 μm. 14 / cm 3 The distribution of impurity concentrations is as follows.
[0054] Furthermore, the impurity concentrations in regions 111 and 112 are approximated by the sum of Gaussian distributions GS1 and GS2. The peak position of Gaussian distribution GS2 roughly corresponds to the position of the maximum value in region 112. The peak position of Gaussian distribution GS1 lies between the peak position of Gaussian distribution GS2 and the drift layer 190. The peak value of Gaussian distribution GS1 is smaller than the peak value of Gaussian distribution GS2. Figure 2 The intersection of the Gaussian distribution GS2 and Gaussian distribution GS1 on the horizontal axis of the curve roughly corresponds to the position of the boundary point KN. The impurity concentration at this intersection point can be greater than or equal to 80% of the peak value of the Gaussian distribution GS2.
[0055] The distribution of impurity concentration in the third region 113 can be maintained within 20% of the representative value. In this case, the impurity concentration in the third region 113 is a roughly flat region. The representative value can be a value near the center of the third region 113, for example, the value at the midpoint between the position of the maximum impurity concentration in the second region 112 and the peak position of the impurity concentration in the fourth region 121 (described later). If the fourth region 121 is omitted, the peak position of the impurity concentration in the fourth region 121 can be used instead of the peak position of the collector layer 131.
[0056] The back surface MS1 of wafer 101 has a first oxygen concentration, and the top surface MS2 of wafer 101 has a second oxygen concentration. The first oxygen concentration can be higher than the second oxygen concentration. The first oxygen concentration can be greater than or equal to 4.5 × 10⁻⁶. 17 / cm 3 The second oxygen concentration can be less than or equal to 1.8 × 10⁻⁶. 17 / cm 3 The first oxygen concentration can be less than or equal to 2.0 × 10⁻⁶. 18 / cm 3 The second oxygen concentration can be greater than or equal to 1.0 × 10⁻⁶. 16 / cm 3 .
[0057] A second buffer layer 120 is disposed between the back surface MS1 and the first buffer layer 110. The second buffer layer 120 has a higher impurity concentration than the third region 113 of the first buffer layer 110. In this embodiment 1, the second buffer layer 120 is composed of a fourth region 121. The fourth region 121 contains protons for generating donors. The impurity concentration distribution in the fourth region 121 can have a maximum value in the thickness direction. At the location of this maximum value, the fourth region 121 has protons at an effective concentration higher than the effective concentration of non-proton impurities. In other words, the donors in the fourth region 121 are mainly generated by protons.
[0058] IGBT 901 is used for high voltage applications, for example, IGBTs with a withstand voltage of 1200V. In this case, the resistivity of the drift layer 190 can be greater than or equal to 50 Ω·cm and less than or equal to 67 Ω·cm. Additionally, the total thickness of the drift layer 190, the first buffer layer 110, and the second buffer layer 120 can, for example, be greater than or equal to 100 μm and less than or equal to 130 μm.
[0059] Figure 3 This is a cross-sectional view that schematically shows the structure of a comparative IGBT 901C (semiconductor device). Figure 4 It means Figure 3 A graph showing an example of the impurity concentration distribution near MS1 on the back side of wafer 101C (semiconductor substrate). Wafer 101C ( Figure 3 The first buffer layer 110C and the chip 101 Figure 1 Unlike the first buffer layer 110 in embodiment 1), it does not have a first region 111. Therefore, the first buffer layer 110C ( Figure 4 The situation is similar to that of the first buffer layer 110. Figure 2 Compared to the case where the maximum value is located in region 2 112, the decrease in impurity concentration distribution towards drift layer 190 becomes more abrupt near the location of the maximum value.
[0060] Figure 5 This is a graph representing an example of the cutoff waveform obtained by simulating a semiconductor device with a voltage rating of 1200V. Figure 6 This is a graph showing an example of the cutoff waveform of the semiconductor device according to Embodiment 1, obtained through simulation assuming a withstand voltage of 1200V. In each graph, the horizontal axis represents time, and the vertical axis on the left represents the collector-emitter voltage V. CE The vertical axis on the right represents the collector current I. C These simulation results show that, compared to the comparative example, this embodiment prevents oscillations at the cutoff point.
[0061] <First variation of Implementation Method 1>
[0062] Figure 7 This is a cross-sectional view that schematically shows the structure of the IGBT 902 (semiconductor device) according to the first variation of Embodiment 1. Figure 8 It means Figure 7 A graph showing an example of the impurity concentration distribution near MS1 on the back side of wafer 101.
[0063] In the case of IGBT 902, the second buffer layer 120 includes a fifth region 122. The fifth region 122 has an aprotic impurity at an effective concentration higher than the effective concentration of protons. The aprotic impurity may also include phosphorus.
[0064] Furthermore, regarding the IGBT 902, the impurity concentration distribution of the second buffer layer 120 has multiple maxima. These maxima are located at position 1 in the thickness direction (…). Figure 8 The first maximum value at the right position in the middle and the second maximum value at the thickness direction (position 1) and the second maximum value at the right position in the middle. Figure 8 The second maximum value is located at the left position in the middle, which is located between the first position and the back surface MS1 in the thickness direction. The second buffer layer 120 has protons at the first position with an effective concentration higher than the effective concentration of aprotic impurities (specifically phosphorus), and has aprotic impurities at the second position with an effective concentration higher than the effective concentration of protons.
[0065] Figures 9-17 This is a rough representation of the IGBT 902 ( Figure 7 A cross-sectional view of the manufacturing process of ).
[0066] Reference Figure 9 Prepare the bare wafer (the wafer before the grinding and surface treatments described later). Perform a surface treatment on the bare wafer to form the structure on the upper surface MS2 side of the IGBT 902. This process can be performed using conventional semiconductor manufacturing techniques, and therefore its detailed description is omitted. The thickness of the wafer 101 after the surface treatment is completed is approximately the same as the thickness of the bare wafer, for example, about 700 μm. Next, grind the back surface MS0 using, for example, a grinder or wet etching. Thus, as Figure 10 As shown, the back side MS1 is formed.
[0067] Reference Figure 11 The fourth region 121 (using a proton implanter) is used to form the first buffer layer 110 and the second buffer layer 120. Figure 7 and Figure 8 Proton (H) implantation. To form the fourth region 121 of the first buffer layer 110 and the second buffer layer 120, at least two implantation processes with different accelerating voltages are performed. To form the first buffer layer 110 having two regions, the second region 112 and the first region 111... Figure 7 and Figure 8The process can involve two implantation steps with different accelerating voltages, or a single implantation step using the method described later. In the former case, a total of three implantation steps are performed, while in the latter case, a total of two implantation steps are performed. Furthermore, in either case, further proton implantation can be performed to adjust the shape of the impurity concentration distribution. After proton implantation, a heat treatment such as furnace annealing at a temperature greater than or equal to 300°C and less than or equal to approximately 500°C is performed. This achieves donor generation by protons. The result is as follows: Figure 12 As shown, the fourth region 121 and the first buffer layer 110 form the second buffer layer 120.
[0068] Furthermore, the mechanism of proton-induced donor generation is believed to be as follows: Through proton injection, as hydrogen is introduced into the wafer, silicon atoms located at lattice sites are expelled, generating lattice defects such as vacancies. These lattice defects react with light element impurities such as oxygen or carbon contained in the silicon substrate to form complexes. Subsequent heat treatment allows hydrogen to combine with these complexes, thereby generating donors. The mechanism of donor generation is believed to be as described above.
[0069] Reference Figure 13 Phosphorus (P) is injected into the back side MS1 at a shallow depth. Then, a heat treatment such as laser annealing is performed. Thus, as... Figure 14 As shown, the fifth region 122 forms the second buffer layer 120. Furthermore, by omitting this step, it is possible to manufacture the IGBT 901 (…). Figure 1 and Figure 2 Implementation method 1) instead of IGBT 902 ( Figure 7 and Figure 8 ).
[0070] Reference Figure 15 Boron (B) is implanted into the back side MS1 at a shallow depth. Then, a heat treatment such as laser annealing is performed. Thus, as... Figure 16 As shown, a collector layer 131 is formed.
[0071] Furthermore, as long as in-furnace annealing is performed after proton implantation and laser annealing is performed after phosphorus implantation and boron implantation, the order of proton implantation, in-furnace annealing, phosphorus implantation, boron implantation and laser annealing can be appropriately changed for manufacturing convenience.
[0072] Reference Figure 17 For example, the collector electrode layer 201 is formed by sputtering. The material of the collector electrode layer 201 can be, for example, a multilayer material such as Al / Ti / Ni / Au or AlSi / Ti / Ni / Au. Next, a heat treatment is performed to reduce the contact resistance between the collector electrode layer 201 and the wafer 101.
[0073] Therefore, IGBT 902 ( Figure 7 ).
[0074] Next, the following discussion focuses on the use of the aforementioned proton injection ( Figure 11 and Figure 12 This section explains the donor generation technique.
[0075] Figure 18 and Figure 19 This is a graph showing the impurity concentration distribution of an IGBT obtained through a manufacturing method involving two proton implantation processes into the wafer, measured using spreading resistance (SR). Furthermore, in the SR measurement, the portion near zero distance from the back surface MS1 is not observed. Therefore, the collector layer 131 (…) was not observed. Figure 8 The intent of one of the two proton injections is to achieve an injection near the depth of the fourth region 121 forming the second buffer layer 120, and the intent of the other is to achieve an injection near the depth of the second region 112 forming the first buffer layer 110. Figure 18 and Figure 19 The difference between them is that, Figure 19 In the case of chips and Figure 18 Compared to wafers in this case, the oxygen concentration is higher.
[0076] As previously mentioned, the mechanism of proton-driven donor generation is considered to be related to the oxygen content in the silicon substrate. Therefore, the oxygen concentration within the wafer significantly influences the contribution of protons to the distribution of impurity concentration. Specifically, in areas with relatively low oxygen concentrations... Figure 18 In the case of 112 in region 2, the peak is formed in roughly isolated form, but in regions with higher oxygen concentrations... Figure 19 In this case, not only is the second region 112 formed, but also the adjacent first region 111 is formed. Regarding this mechanism, it is believed that a portion of the hydrogen accumulated by proton injection into the region forming the second region 112 diffuses into the region forming the first region 111 through post-injection heat treatment, and the first region 111 is formed by the action of this diffused hydrogen on the high oxygen concentration wafer.
[0077] Figure 20 This is a graph showing the measurement results of the relationship between the oxygen concentration of wafer 101 before wafer processing and the peak value of the Gaussian approximation of the first region 111 of the first buffer layer 110. Gaussian approximation and... Figure 2 Similarly, this was done using Gaussian distributions GS1 and GS2. Figure 20 The peak value of the vertical axis is the peak value of the Gaussian distribution GS1. Furthermore, the back surface MS1 of wafer 101 is located relative to the back surface MS0 of the bare wafer (…). Figure 9 Since the oxygen concentration is relatively deep, it is assumed that it will not be significantly affected by the reduction in oxygen concentration caused by oxygen diffusion during the wafer process. Therefore, it is considered that the oxygen concentration from the back side MS1 to the location where the first region 111 is formed during the proton implantation process can be regarded as almost the same as the oxygen concentration of the wafer 101 before the wafer process.
[0078] according to Figure 20 The results shown suggest that by increasing the oxygen concentration on the back side MS1, the first region 111 can be formed with a sufficient impurity concentration together with the second region 112. (Reference) Figure 20 The approximate curve (dashed line) preferably shows that the oxygen concentration of MS1 on the reverse side is greater than or equal to 4.5 × 10⁻⁶. 17 / cm 3 More preferably, greater than or equal to 5.0 × 10 17 / cm 3 Additionally, if the oxygen concentration of MS1 on the reverse side is greater than or equal to 5.2 × 10⁻⁶... 17 / cm 3 This more reliably increases the impurity concentration in the first region 111. Furthermore, when measuring the oxygen concentration at the back surface MS1, to avoid the influence of the surface oxide film formed on the back surface MS1, the measurement is performed at a position slightly recessed inward from the back surface MS1 (e.g., a few μm). Similarly, when measuring the oxygen concentration at the upper surface MS2 (described later), the measurement is performed at a position slightly recessed inward from the upper surface MS2 (e.g., a few μm).
[0079] Furthermore, the technique described above for forming both the first region 111 and the second region 112 using a wafer with a high oxygen concentration through a single ion implantation is also described. However, it is also possible to implant protons into the depth positions of the first region 111 and the second region 112 respectively through two proton implantations with different acceleration voltages, in which case the oxygen concentration of the back surface MS1 is not particularly limited. Alternatively, it is also possible to ensure a certain level of impurity concentration in the first region 111 by using a back surface MS1 with a certain degree of high oxygen concentration, and to compensate for any insufficient impurity concentration by proton implantation.
[0080] Figure 21This is a graph showing the measurement results of the relationship between the oxygen concentration on the upper surface MS2 of wafer 101 after wafer processing and the gate withstand voltage of IGBT 901. According to the results, if the oxygen concentration on the upper surface MS2 of wafer 101 is too high, the gate withstand voltage decreases. The reasoning is that, for wafer 101, if the oxygen concentration in the portion forming the gate oxide film 301 is too high, the quality of the gate oxide film 301 deteriorates. Around a crystal defect, namely a vacancy, a portion of the four bonding types of silicon atoms is not used. Such silicon atoms and oxygen atoms in wafer 101 form a complex, which sometimes forms an oxide film (the inner wall oxide film of the trench). This complex adversely affects the surface oxidation process performed to form the gate oxide film 301. Therefore, it is believed that if the oxygen concentration on the upper surface MS2 is too high, the quality of the gate oxide film 301 deteriorates, resulting in a decrease in the gate withstand voltage. (Reference) Figure 21 The approximate curve (solid line) is preferably such that the oxygen concentration on the upper surface MS2 is less than or equal to 1.8 × 10⁻⁶. 17 / cm 3 Additionally, if the oxygen concentration of MS2 on the upper surface is less than or equal to 1.7 × 10⁻⁶... 17 / cm 3 This will more reliably improve the gate withstand voltage.
[0081] In summary, from the viewpoint of improving gate breakdown voltage, it is preferable to reduce the oxygen concentration near the upper surface MS2 at least before forming the gate electrode 203. For this purpose, it is effective to perform an outward diffusion process of oxygen from the upper surface MS2 at a temperature of approximately 1100°C or higher. This is achieved through the wafer grinding process ( Figures 9 to 10 Before the process of (the process), an outward diffusion process is performed, so that even if the back side MS0 ( Figure 9 The decrease in oxygen concentration near the MS1 on the back side can also prevent the back side from being affected. Figure 10 The oxygen concentration decreases. Therefore, even after outward diffusion is implemented, it is possible to apply the technique of forming the first region 111 simultaneously with the second region 112 by utilizing the high oxygen concentration of the back side MS1.
[0082] <Second variation of Implementation Method 1>
[0083] Figure 22 This is a cross-sectional view that schematically shows the structure of the IGBT 903 (semiconductor device) according to the second variation of Embodiment 1. Figure 23 It means Figure 22 A graph illustrating an example of impurity concentration distribution near MS1 on the back side of wafer 101. (Regarding IGBT 903) Figure 22 and Figure 23 In this regard, chip 101 does not have a second buffer layer 120. Figure 1 and Figure 2 Implementation method 1). IGBT 903 ( Figure 22 ) can be achieved by using IGBT 902 ( Figure 7 and Figure 8 The second buffer layer 120 is obtained by omitting the forming process in the manufacturing method already described in detail. Furthermore, in... Figure 23 In the impurity concentration distribution shown, by adjusting the conditions related to the first buffer layer 110 in the above manufacturing method, the ratio of the boundary point KN value to the maximum value of the impurity concentration distribution in the first buffer layer 110 (specifically, the maximum value in the second region 112) can be adjusted. Therefore, compared with Embodiment 1 ( Figure 2 Similarly, the value at the boundary point KN can be adjusted to be greater than or equal to 80% of the above maximum value.
[0084] <Implementation Method 1 ( Figure 1 and Figure 2 The effect of ) >
[0085] According to the IGBT 901 described above, the first: the first region 111 and the second region 112 of the first buffer layer 110 contain protons. Protons are more easily implanted into the wafer 101 than other impurities, thus the first region 111 and the second region 112 of the first buffer layer 110 can be formed to a depth measured from the back surface MS1 of the wafer 101 by using protons. Secondly: the impurity concentration distribution of the first buffer layer 110 has a maximum value in the second region 112, and the decrease in impurity concentration from this position towards the drift layer 190 is moderated or stopped at the boundary point KN between the second region 112 and the first region 111, and the impurity concentration at the boundary point KN is greater than or equal to 80% of the maximum value. Therefore, the slope of the distribution from the maximum value towards the drift layer 190 becomes gentler near the maximum value position. Therefore, at cutoff, in wafer 101, the first buffer layer 110 can slowly stop the extension of the depletion layer from the drift layer 190 toward the first main surface MS1 in both time and space. Thirdly, the first buffer layer 110 has a third region 113 with a thickness greater than or equal to 5 μm between the second region 112, which has the aforementioned maximum impurity concentration, and the back surface MS1 of wafer 101. Therefore, at cutoff, carriers can be retained over a large area in the thickness direction between the depletion layer, which has been stopped as described above, and the back surface MS1 of wafer 101. In summary, oscillations at cutoff can be effectively prevented.
[0086] The distribution of the third region 113 in the impurity concentration distribution can be maintained within 20% of the representative value. Therefore, the function of the third region 113 at the cutoff point can be stably maintained.
[0087] The wafer 101 may also have a second buffer layer 120 between the back surface MS1 and the first buffer layer 110. The second buffer layer 120 is n-shaped and has a higher impurity concentration than the third region 113 of the first buffer layer 110. This allows for more effective prevention of oscillations during cutoff.
[0088] The first oxygen concentration on the back surface MS1 of wafer 101 can be higher than the second oxygen concentration on the upper surface MS2 of wafer 101. The relatively higher oxygen concentration near the back surface MS1 compared to the vicinity of the upper surface MS2 allows for the easy formation of the first region 111 of the first buffer layer 110 using protons. Conversely, the relatively lower oxygen concentration near the upper surface MS2 compared to the vicinity of the back surface MS1 improves the gate withstand voltage. In summary, it is possible to improve both the manufacturing efficiency of the process forming the first region 111 of the first buffer layer 110 and the gate withstand voltage.
[0089] <From the first variation ( Figure 7 and Figure 8 Additional effects achieved >
[0090] The second buffer layer 120 may include a region containing non-proton impurities as n-type impurities at an effective concentration higher than the effective concentration of protons. Compared to the first buffer layer 110, the second buffer layer 120 is located at a shallower depth from the back side MS1, so even non-proton impurities that are difficult to inject deeply compared to protons can sometimes be easily and adequately injected from the back side MS1.
[0091] Non-proton impurities can include phosphorus. This ensures a higher activation rate of impurities during the formation of the second buffer layer 120. Specifically, with appropriate heating, the activation rate of phosphorus is 70-100%, while the proportion of proton-generating donors is approximately 0.5-2%. Therefore, the amount of phosphorus required to ensure a certain impurity concentration is significantly less than that required for protons. Thus, using phosphorus (or other non-proton impurities) instead of protons as the implanted species for donor generation at a shallow position measured from the back side MS1 reduces the workload of the implantation process.
[0092] The impurity concentration of the second buffer layer 120 can have multiple maxima. This allows for more effective prevention of oscillations during cutoff.
[0093] The multiple maxima include a first maximum located at a first position in the thickness direction and a second maximum located at a second position in the thickness direction, which is situated between the first position and the back surface MS1. The second buffer layer 120 may have protons at the first position at an effective concentration higher than the effective concentration of aprotic impurities, and may have aprotic impurities at the second position at an effective concentration higher than the effective concentration of protons. Therefore, protons can be used for doping in a relatively deep region from the back surface MS1, and aprotic impurities can be used for doping in a relatively shallow region from the back surface MS1. This improves the manufacturing efficiency of the process for forming the second buffer layer 120 having multiple maxima.
[0094] <From the second variation ( Figure 22 and Figure 23 Additional effects achieved >
[0095] It is possible to omit the second buffer layer 120 ( Figure 1 and Figure 2 The manufacturing method is simplified by simplifying the formation process of implementation method 1).
[0096] <Implementation Method 2>
[0097] Figure 24 This is a schematic cross-sectional view showing the structure of the diode 911 (semiconductor device) according to Embodiment 2. The diode 911 has a wafer 102 replacing the wafer 101. Figure 1 The wafer 102, from its back surface MS1 towards its upper surface MS2, sequentially comprises an n-type cathode layer 131D, a second buffer layer 120, a first buffer layer 110, a drift layer 190, and a p-type anode layer 141D. The cathode layer 131D is disposed on the back surface MS1, not the collector layer 131, and functions as a carrier injection layer. Furthermore, a cathode electrode layer 201D and an anode electrode layer 202D are disposed as the first and second electrodes, respectively, replacing the collector electrode layer 201 and the emitter electrode layer 202. Figure 1 ).
[0098] Chip 102 is also related to chip 101 ( Figure 1 Similarly, the structure including the drift layer 190, the first buffer layer 110, and the second buffer layer 120 can be formed using the process described in Embodiment 1. Furthermore, the other structures are the same as those of a typical diode. Therefore, the description of the manufacturing method of the diode 911 is omitted.
[0099] Furthermore, variations of the same as those in Embodiment 1 can be applied to this Embodiment 2. Specifically, in this Embodiment 2, the second buffer layer 120 can also be modified or omitted in the same way as in the variations of Embodiment 1.
[0100] Additionally, by using the collector layer 131 in Embodiment 1 or its variations ( Figure 1 A portion of the cathode layer 131D (etc.) was replaced with a portion of the cathode layer 131D. Figure 24 Thus, the collector layer 131 and the cathode layer 131D are configured as the carrier injection layer on the back side MS1. This allows for the generation of a reverse-conducting IGBT (RC-IGBT).
[0101] Furthermore, it is possible to freely combine the various implementation methods, or to appropriately modify or omit the various implementation methods.
[0102] Hereinafter, the various aspects of the present invention will be summarized as appendices.
[0103] (Postscript 1)
[0104] A semiconductor device having:
[0105] First electrode layer;
[0106] A second electrode layer, which is separated from the first electrode layer in the thickness direction; and
[0107] A semiconductor substrate having a first main surface and a second main surface opposite to the first main surface in the thickness direction, the first main surface being in contact with a first electrode layer and the second main surface being in contact with a second electrode layer.
[0108] The semiconductor substrate has:
[0109] An n-shaped drift layer; and
[0110] The first buffer layer, which is n-shaped, is disposed between the first main surface and the drift layer.
[0111] The first buffer layer has:
[0112] A first region containing protons, having an impurity concentration higher than that of the drift layer, is in contact with the drift layer;
[0113] A second region, containing protons, having a higher impurity concentration than the drift layer, is disposed between the first region and the first main surface, and in contact with the first region; and
[0114] The third region is disposed between the second region of the first buffer layer and the first main surface of the semiconductor substrate.
[0115] The first buffer layer has an impurity concentration distribution that depends on the depth distance measured from the first main surface along the thickness direction.
[0116] The impurity concentration distribution has the following characteristics:
[0117] The maximum value in the second region is the maximum value of the impurity concentration distribution in the first buffer layer;
[0118] The decrease from the maximum value results in a bend at the boundary point between the first region and the second region that is either eased or stopped;
[0119] The value at the boundary point that is greater than or equal to 80% of the maximum value; and
[0120] The value of the third region, within a range greater than or equal to 5 μm, is lower than that at the boundary point and less than or equal to 5.0 × 10⁻⁶. 14 / cm 3 The distribution of impurity concentrations.
[0121] (Postscript 2)
[0122] According to the semiconductor device described in Appendix 1, wherein,
[0123] The distribution in the third region of the impurity concentration distribution remains within 20% of the representative value.
[0124] (Note 3)
[0125] According to the semiconductor device described in Appendix 1 or 2, wherein,
[0126] The semiconductor substrate further comprises a second buffer layer between the first main surface and the first buffer layer. The second buffer layer is n-shaped and has a higher impurity concentration than the third region of the first buffer layer.
[0127] (Postscript 4)
[0128] According to the semiconductor device described in Appendix 3, wherein,
[0129] The second buffer layer includes regions containing non-proton impurities at an effective concentration higher than the effective concentration of protons.
[0130] (Note 5)
[0131] According to the semiconductor device described in Appendix 4, wherein,
[0132] The aprotic impurity contains phosphorus.
[0133] (Note 6)
[0134] According to the semiconductor device described in Appendix 3, wherein,
[0135] The impurity concentration of the second buffer layer has multiple maxima.
[0136] (Note 7)
[0137] According to the semiconductor device described in Appendix 6, wherein,
[0138] The plurality of maxima includes a first maxima located at a first position in the thickness direction and a second maxima located at a second position in the thickness direction, the second position being located between the first position and the first main surface in the thickness direction.
[0139] The second buffer layer has protons at the first position at an effective concentration higher than the effective concentration of non-proton impurities, and has non-proton impurities at the second position at an effective concentration higher than the effective concentration of protons.
[0140] (Postscript 8)
[0141] According to any one of the appendices 1 to 7, the semiconductor device wherein,
[0142] The first main surface of the semiconductor substrate has a first oxygen concentration, and the second main surface of the semiconductor substrate has a second oxygen concentration, wherein the first oxygen concentration is higher than the second oxygen concentration.
[0143] (Note 9)
[0144] According to the semiconductor device described in Appendix 8, wherein,
[0145] The first oxygen concentration is greater than or equal to 4.5 × 10⁻⁶. 17 / cm 3 The second oxygen concentration is less than or equal to 1.8 × 10⁻⁶. 17 / cm 3 .
[0146] (Postscript 10)
[0147] According to any one of the appendices 1 to 9, the semiconductor device wherein,
[0148] The value at the boundary point of the impurity concentration distribution is less than or equal to 1 × 10⁻⁶. 15 / cm 3 .
[0149] Explanation of the label
[0150] 101, 102 wafers (semiconductor substrates), 110 first buffer layer, 111 first region, 112 second region, 113 third region, 120 second buffer layer, 121 fourth region, 122 fifth region, 131 collector layer, 131D cathode layer, 141p base layer, 141D anode layer, 190 drift layer, 201 collector electrode layer (first electrode layer), 201D cathode electrode layer (first electrode layer), 202 emitter electrode layer (second electrode layer), 202D anode electrode layer (second electrode layer), 203 gate electrode, 301 gate oxide film, 901~903 IGBTs (semiconductor devices), 911 diodes (semiconductor devices), KN boundary point, MS1 back surface (first main surface), MS2 top surface (second main surface).
Claims
1. A semiconductor device comprising: First electrode layer; The second electrode layer is separated from the first electrode layer in the thickness direction; as well as A semiconductor substrate having a first main surface and a second main surface opposite to the first main surface in the thickness direction, the first main surface being in contact with a first electrode layer and the second main surface being in contact with a second electrode layer. The semiconductor substrate has: An n-shaped drift layer; and The first buffer layer, which is n-shaped, is disposed between the first main surface and the drift layer. The first buffer layer has: A first region containing protons, having an impurity concentration higher than that of the drift layer, is in contact with the drift layer; A second region, which contains protons and has a higher impurity concentration than the drift layer, is disposed between the first region and the first main surface and is in contact with the first region; as well as The third region is disposed between the second region of the first buffer layer and the first main surface of the semiconductor substrate. The first buffer layer has an impurity concentration distribution that depends on the depth distance measured from the first main surface along the thickness direction. The impurity concentration distribution has the following characteristics: The maximum value in the second region is the maximum value of the impurity concentration distribution in the first buffer layer; The decrease from the maximum value results in a bend at the boundary point between the first region and the second region that is either eased or stopped; The value at the boundary point that is greater than or equal to 80% of the maximum value; as well as The value of the third region, within a range greater than or equal to 5 μm, is lower than that at the boundary point and less than or equal to 5.0 × 10⁻⁶. 14 / cm 3 The distribution of impurity concentrations.
2. The semiconductor device according to claim 1, wherein, The distribution in the third region of the impurity concentration distribution remains within 20% of the representative value.
3. The semiconductor device according to claim 1 or 2, wherein, The semiconductor substrate further comprises a second buffer layer between the first main surface and the first buffer layer. The second buffer layer is n-shaped and has a higher impurity concentration than the third region of the first buffer layer.
4. The semiconductor device according to claim 3, wherein, The second buffer layer includes regions containing non-proton impurities at an effective concentration higher than the effective concentration of protons.
5. The semiconductor device according to claim 4, wherein, The aprotic impurity contains phosphorus.
6. The semiconductor device according to claim 3, wherein, The impurity concentration distribution of the second buffer layer has multiple maxima.
7. The semiconductor device according to claim 6, wherein, The plurality of maxima includes a first maxima located at a first position in the thickness direction and a second maxima located at a second position in the thickness direction, the second position being located between the first position and the first main surface in the thickness direction. The second buffer layer has protons at the first position at an effective concentration higher than the effective concentration of non-proton impurities, and has non-proton impurities at the second position at an effective concentration higher than the effective concentration of protons.
8. The semiconductor device according to any one of claims 1 to 7, wherein, The first main surface of the semiconductor substrate has a first oxygen concentration, and the second main surface of the semiconductor substrate has a second oxygen concentration, wherein the first oxygen concentration is higher than the second oxygen concentration.
9. The semiconductor device according to claim 8, wherein, The first oxygen concentration is greater than or equal to 4.5 × 10⁻⁶. 17 / cm 3 The second oxygen concentration is less than or equal to 1.8 × 10⁻⁶. 17 / cm 3 .
10. The semiconductor device according to any one of claims 1 to 9, wherein, The value at the boundary point of the impurity concentration distribution is less than or equal to 1 × 10⁻⁶. 15 / cm 3 .
Citation Information
Patent Citations
Semiconductor device
JP2013138172A
Method for processing semiconductor wafer
JP2016009868A
Semiconductor device
CN103959473A
Semiconductor device and method for manufacturing same
CN104620391A