Surface treatment method for dental implants
By using laser processing and etching to treat the surface of dental implants, a regular macroscopic and microscopic groove structure is formed, which solves the problem of insufficient osseointegration characteristics in existing technologies and achieves excellent osseointegration characteristics and short-term healing effect.
Patent Information
- Application Number
- CN202280033541.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-19
- Filing Date
- 2022-07-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-07-13
AI Technical Summary
Existing dental implant surface treatment methods cannot fully realize osseointegration characteristics, resulting in the inability to form complete osseointegration between the implant and the bone, which may prolong the operation period or lead to surgical failure.
The surface of the dental implant is treated with laser processing and etching to form a regular and uniform macroscopic and microscopic groove structure, including a first groove and a second groove. The groove depth and width at the upper end of the outer peripheral surface are greater than those at the lower end. Titanium-based materials are used in combination with etching solution treatment.
By forming a regular groove structure, the osseointegration properties of dental implants are significantly improved, the surgical healing time is shortened, and bacterial proliferation is inhibited.
Smart Images

Figure CN117320663B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a surface treatment method for dental implants. Background Technology
[0002] Osteointegration refers to the formation of a permanent bond between the implant and bone within a short treatment period after initial stability is achieved by fixing the implant to the bone.
[0003] As mentioned above, to improve osseointegration properties, the implant surface can be appropriately treated and endowed. Surface treatment methods include chemical roughening, such as sandblasting, anodizing, or etching. Other methods include surface treatment via coating or impregnation with materials possessing excellent biocompatibility. Implants treated with the aforementioned surface treatment methods can shorten postoperative healing time.
[0004] In particular, as an example of existing surface treatment methods, a method has been proposed to improve osseointegration properties by sandblasting and etching the surface of the implant to impart surface roughness. However, implants treated using these existing methods have surface roughness in an irregular shape, thus failing to fully achieve osseointegration properties. As mentioned above, when an implant with insufficiently achieved osseointegration properties is implanted into the human body, complete osseointegration cannot be formed between the implant and the bone, which may excessively prolong the operation or lead to surgical failure.
[0005] As mentioned above, various surface treatment methods have been proposed as ways to improve the osseointegration properties of existing implants, and further research and development of surface treatment methods for further improving osseointegration properties are needed. Summary of the Invention
[0006] Technical issues
[0007] To address the aforementioned problems in the prior art, a surface treatment method is provided for dental implants that exhibit excellent osseointegration properties by having a surface roughness achieved in a constant and uniform manner.
[0008] Solution to the problem
[0009] According to one aspect, a surface treatment method for a dental implant is provided, comprising: step (a) laser processing of the implant surface; step (b) etching of the laser-processed implant surface; and step (c) cleaning of the etched implant; wherein step (a) forms a macroscopic surface including one or more first grooves on the implant surface, and step (b) forms a microscopic surface including one or more second grooves on the implant surface, wherein the outer peripheral surface of the implant is composed of an upper end and a lower end, and at the upper end of the outer peripheral surface of the implant, at least one of the average width and average depth of the first groove is formed to be greater than that of the lower end of the outer peripheral surface of the implant.
[0010] In one embodiment, one or more of the second grooves may be formed inside the first groove.
[0011] In one embodiment, the average width of the first groove can be from 5 μm to 100 μm, and the average depth can be from 5 μm to 50 μm.
[0012] In one embodiment, the average width and average depth of the second groove can be from 1 μm to 10 μm, respectively.
[0013] In one embodiment, step (a) may include: step i) laser processing of the upper end of the outer peripheral surface of the implant; and step ii) laser processing of the lower end of the outer peripheral surface of the implant.
[0014] In one embodiment, the lower end of the outer peripheral surface of the implant may be composed of a first lower end and a second lower end. Step (a) may include: step i), laser processing of the upper end of the outer peripheral surface of the implant; step ii), laser processing of the first lower end of the outer peripheral surface of the implant; and step iii), laser processing of the second lower end of the outer peripheral surface of the implant.
[0015] According to another aspect, a dental implant is provided, which is a surface-treated dental implant, at least a portion of the implant surface including a macroscopic surface having one or more first grooves and a microscopic surface having one or more second grooves, the outer peripheral surface of the implant being formed by an upper end and a lower end, wherein at the upper end of the outer peripheral surface of the implant, at least one of the average width and average depth of the first groove is formed to be greater than the lower end of the outer peripheral surface of the implant.
[0016] In one embodiment, the lower end of the outer peripheral surface of the implant may be composed of a first lower end and a second lower end.
[0017] Invention Effects
[0018] On one hand, a macroscopic surface can be formed, including one or more grooves formed in a regular shape. On the other hand, the surface area can be increased by forming a microscopic surface with one or more grooves inside the aforementioned grooves, while imparting a surface roughness suitable for osseointegration, thereby improving the osseointegration properties of the dental implant.
[0019] The effects of this specification are not limited to those described above, and it should be understood that the effects of this specification include all effects that can be inferred from the configuration of the invention described in the detailed description or claims of this specification. Attached Figure Description
[0020] Figure 1 This is a schematic diagram illustrating a surface treatment method for dental implants using sandblasting and etching.
[0021] Figure 2 This is a schematic diagram illustrating a surface treatment method for a dental implant according to an embodiment of this specification.
[0022] Figure 3 SEM images of the surface of a dental implant according to an embodiment of this specification are shown.
[0023] Figure 4 SEM images of the upper and lower ends of the peripheral surface of the dental implant of Example 3 of this specification are shown.
[0024] Figure 5 SEM images of the upper end, first lower end, and second lower end of the peripheral surface of the dental implant of Embodiment 4 of this specification are shown.
[0025] Figure 6 The graph shows the results of bone interface bonding force measurements for dental implants according to the embodiments and comparative examples in this specification. Detailed Implementation
[0026] One aspect of this specification will now be described with reference to the accompanying drawings. However, the matters described in this specification can be implemented in many different forms and should not be construed as limited to the embodiments set forth herein. Furthermore, in the drawings, portions irrelevant to the description are omitted for clarity, and the same reference numerals consistently indicate the same components.
[0027] Throughout the specification, when it is stated that a part is "connected" to other parts, this includes not only "direct connections" but also "indirect connections" where other components are placed in between. Furthermore, when it is stated that a part "includes" a structural element, unless otherwise stated otherwise, this means that other structural elements are not excluded, but rather may be included.
[0028] In this specification, when describing a range of numerical values, unless otherwise specifically stated, these values have the precision of significant figures provided in accordance with the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, while the number 10.0 includes a range of 9.50 to 10.49.
[0029] An embodiment of this specification will now be described in detail with reference to the accompanying drawings.
[0030] Surface treatment methods for dental implants
[0031] According to one aspect, a surface treatment method for a dental implant is provided, comprising: step (a) laser processing of the implant surface; step (b) etching of the laser-processed implant surface; and step (c) cleaning of the etched implant; wherein step (a) forms a macroscopic surface including one or more first grooves on the implant surface, and step (b) forms a microscopic surface including one or more second grooves on the implant surface, wherein the outer peripheral surface of the implant is composed of an upper end and a lower end, and at the upper end of the outer peripheral surface of the implant, at least one of the average width and average depth of the first groove is formed to be greater than that of the lower end of the outer peripheral surface of the implant.
[0032] In dental implant surgery, osseointegration is the most crucial factor. Excellent osseointegration allows for a strong bond to form between the implant and the gingival bone within a short time after placement. Generally, the degree of osseointegration varies depending on the surface treatment method. Surface treatments for implants include sandblasting, anodizing, and etching. Appropriate application of these methods imparts surface roughness to the implant, thereby improving osseointegration. However, among surface treatments, sandblasting creates an irregularly shaped macroscopic surface, which may result in relatively insufficient improvement in osseointegration.
[0033] In step (a) above, one or more first grooves are formed in a regular shape by laser processing of the implant surface, thereby imparting macroscopic surface properties. The laser can be a UV laser, for example, a UV laser beam having an ultraviolet wavelength of 200 nm to 400 nm. The ultraviolet wavelength of the UV laser beam can be, for example, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm, or a range between these values, but is not limited thereto. Since the intensity of the laser beam increases as the ultraviolet wavelength of the UV laser beam decreases, appropriate values can be selected from the above range, taking into account the width and depth of the first grooves to be formed on the implant surface in this specification.
[0034] In addition, the pulse width of the aforementioned laser can be from 1 ns to 200 ns (nanoseconds), for example, it can be 1 ns, 2 ns, 3 ns, 4 ns, 5 ns, 6 ns, 7 ns, 8 ns, 9 ns, 10 ns, 15 ns, 20 ns, 25 ns, 30 ns, 35 ns, 40 ns, 45 ns, 50 ns, 55 ns, 60 ns, 65 ns, 70 ns, 75 ns, 80 ns, 85 ns, 90 ns, 95 ns, 100 ns, 110 ns, 115 ns, 120 ns, 125 ns, 130 ns, 135 ns, 140 ns, 145 ns, 150 ns, 155 ns, 160 ns, 165 ns, 170 ns, 175 ns, 180 ns, 185 ns, 190 ns, 195 ns, 200 ns or a range between these two values, but is not limited to these. The pulse width of the laser mentioned above refers to the duration of the irradiated laser beam. If the pulse width of the laser mentioned above is greater than 200 ns, the width and depth of the first groove mentioned above may be excessively increased. If the pulse width of the laser mentioned above is less than 1 ns, sufficient surface roughness cannot be achieved, and therefore the osseointegration characteristics may deteriorate.
[0035] On the other hand, the average width of the first groove can be from 5 μm to 100 μm, and the average depth can be from 5 μm to 50 μm. The average width of the first groove can be, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, or a range between these values, but is not limited thereto. If the average width of the first groove is greater than 100 μm, the durability of the implant may deteriorate; if the average width of the first groove is less than 5 μm, the osseointegration properties of the implant may decrease.
[0036] In one example, the difference between the maximum and minimum width of the first groove is 50% or less, for example, it can be 50%, 45%, 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or a range between these two values. For example, if the difference between the maximum and minimum width is 50%, then when the maximum width in the first groove is 100 μm, this means the minimum width is 50 μm or greater. Further satisfying these characteristics can significantly improve osseointegration properties.
[0037] Furthermore, the average depth of the aforementioned first groove can be, for example, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, or a range between these values, but is not limited thereto. If the average depth of the aforementioned first groove is greater than 50μm, the durability of the aforementioned implant may deteriorate; if the average depth of the aforementioned first groove is less than 5μm, the osseointegration characteristics of the aforementioned implant may decrease.
[0038] In one example, the difference between the maximum and minimum depths of the first groove is 50% or less, for example, it can be 50%, 45%, 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or a range between these two values. If these characteristics are further satisfied, the second groove forming the micro-surface will be formed more uniformly, thereby addressing the problem of insufficient osseointegration in some areas.
[0039] In step (a) above, one or more first grooves are formed by laser processing to impart surface roughness at one time. Then, in step (b) above, the implant surface is etched to form one or more second grooves with a size smaller than the first grooves, thereby imparting microscopic surface properties.
[0040] Furthermore, the average width and average depth of the second groove can be from 1 μm to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or a range between these two values, but are not limited thereto. If the average width and average depth of the second groove are greater than 10 μm, the durability of the implant may deteriorate; if the average width and average depth of the second groove are less than 1 μm, the osseointegration properties of the implant may decrease.
[0041] In one example, one or more of the aforementioned second grooves may be formed within the aforementioned first groove in the implant. When a micro-surface is formed within the macro-surface of the implant, the integration between the implant and the bone is improved, which can shorten the postoperative healing period.
[0042] The length of the implant can be from 5 mm to 15 mm, for example, 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 9 mm, 9.5 mm, 10 mm, 10.5 mm, 11 mm, 11.5 mm, 12 mm, 12.5 mm, 13 mm, 13.5 mm, 14 mm, 14.5 mm, 15 mm, or a range between these two values. The implant can have a truncated cone structure with threads formed on its outer peripheral surface, the diameter of which is larger than the diameter of its upper end. The surface treatment method for the dental implant can involve forming macroscopic and microscopic surfaces on the threaded outer peripheral surface of the implant.
[0043] In one example, at least one of the average width and average depth of the first groove at the upper end of the outer peripheral surface of the implant is formed to be greater than at least one of the average width and average depth of the first groove at the lower end of the outer peripheral surface of the implant. For example, the upper end of the outer peripheral surface may refer to a region of 0.5 mm to 2 mm, and the lower end of the outer peripheral surface may refer to the remaining region.
[0044] In one example, the upper end of the peripheral surface of the implant, which is in contact with the cortical bone, has a first groove with a depth of 1 μm to 15 μm and a width of 1 μm to 25 μm. The lower end of the peripheral surface of the implant, which is in contact with the cancellous bone, can have a first groove with a depth of 20 μm to 75 μm and a width of 30 μm to 125 μm. By forming a relatively small first groove at the upper end and a relatively large first groove at the lower end of the peripheral surface, bacterial proliferation can be inhibited, and osseointegration properties can be improved.
[0045] In one example, when the outer peripheral surface of the implant is composed of an upper end and a lower end, step (a) may include: step i), laser processing of the upper end of the outer peripheral surface of the implant; and step ii), laser processing of the lower end of the outer peripheral surface of the implant, thereby forming a first groove with an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm at the upper end of the outer peripheral surface of the implant, and forming a first groove with an average depth of 20 μm to 75 μm and an average width of 30 μm to 125 μm at the lower end of the outer peripheral surface of the implant. Figure 4 An example of the surface treatment images of the upper and lower ends is shown below.
[0046] In another example, the lower portion of the peripheral surface of the implant described above can be composed of a first lower portion with an average depth of 20 μm to 35 μm and an average width of 30 μm to 65 μm, and a second lower portion with an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm. By dividing the lower portion into two or more regions, bacterial proliferation inhibition and osseointegration properties can be improved in a balanced manner.
[0047] On the other hand, when the lower end of the outer peripheral surface of the implant is composed of a first lower end and a second lower end, step (a) may include: step i), laser processing of the upper end of the outer peripheral surface of the implant; step ii), laser processing of the first lower end of the outer peripheral surface of the implant; and step iii), laser processing of the second lower end of the outer peripheral surface of the implant, thereby forming a first groove with an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm at the upper end of the outer peripheral surface of the implant, forming a first groove with an average depth of 20 μm to 35 μm and an average width of 30 μm to 65 μm at the first lower end of the outer peripheral surface of the implant, and forming a first groove with an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm at the second lower end of the outer peripheral surface of the implant. Figure 5 The image shows the surface treatment of the upper end, the first lower end (middle section), and the second lower end.
[0048] On the other hand, the etching in step (b) above can be performed by treating an etching solution, which can be selected from the group consisting of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, hydrogen peroxide, and mixtures of two or more thereof, but is not limited thereto. For example, when the etching solution is a mixture of hydrochloric acid and sulfuric acid, the content of the hydrochloric acid can be from 50 vol% to 100 vol%, for example, it can be 50 vol%, 55 vol%, 60 vol%, 65 vol%, 70 vol%, 75 vol%, 80 vol%, 85 vol%, 90 vol%, 95 vol%, 100 vol%, or a range between these two values, but is not limited thereto.
[0049] As a non-limiting example, the etching described above can be performed from 10 seconds to 120 minutes, for example, for 10 seconds, 30 seconds, 60 seconds, 3 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, 75 minutes, 80 minutes, 85 minutes, 90 minutes, 95 minutes, 100 minutes, 105 minutes, 110 minutes, 115 minutes, 120 minutes, or a range between these two values. The etching time can vary depending on the type of etching solution, and typically, it can be performed from 10 minutes to 40 minutes, but is not limited to this.
[0050] In step (c) above, the etched implant can be cleaned to remove the etching solution remaining on the surface of the implant. Step (c) can be performed by immersing the etched implant in a solution selected from the group consisting of alcohol, purified water, and mixtures thereof, followed by stirring or ultrasonic treatment.
[0051] According to another aspect, a dental implant is provided, which is manufactured by a surface treatment method for a dental implant including the following steps: step (a), laser processing of the surface of the implant; step (b), etching of the laser-processed surface of the implant; and step (c), cleaning of the etched implant.
[0052] At least a portion of the surface of the aforementioned dental implant may include a macroscopic surface having one or more first grooves and a microscopic surface having one or more second grooves. The outer peripheral surface of the implant may be composed of an upper end and a lower end. At least one of the average width and average depth of the first groove at the upper end of the outer peripheral surface of the implant may be formed to be greater than at least one of the average width and average depth of the first groove at the lower end of the outer peripheral surface of the implant.
[0053] In one example, the first groove described above can be formed by laser processing in the surface treatment method of the implant, thereby achieving a macroscopic surface including one or more first grooves. The macroscopic surface can be achieved in a regular and uniform shape by the laser processing. The microscopic surface can be achieved by forming one or more second grooves within the first groove.
[0054] In another example, the lower end of the outer peripheral surface of the implant described above may be composed of a first lower end and a second lower end.
[0055] Furthermore, the average width and average length of the first and second grooves, the implementation conditions of laser processing as a surface treatment method, the implementation conditions of etching processing, and the resulting effects are the same as described above.
[0056] On the other hand, the aforementioned dental implants can be made of titanium-based materials. These titanium-based materials refer to materials formed from pure titanium or alloys of titanium with other metals in the periodic table. The titanium alloys may be, for example, at least one selected from the group consisting of titanium (Ti), aluminum (Al), silicon (Si), vanadium (V), niobium (Nb), zirconium (Zr), molybdenum (Mo), chromium (Cr), tin (Sn), tantalum (Ta), and palladium (Pd), but are not limited thereto.
[0057] As a non-limiting example, the dental implant described above may also include a central portion, which includes one selected from the group consisting of polymers, ceramics, metals, and combinations thereof. For example, the central portion may be existing titanium or its alloys, ceramics such as zirconium oxide, or polymers such as general-purpose plastics, engineering plastics, super engineering plastics, or combinations thereof, but is not limited thereto.
[0058] The aforementioned surface and the aforementioned central portion can be manufactured as separate components and then combined to form a dental implant. If necessary, they can be machined from a single prototype and then laser-processed and / or etched to form a dental implant in which the aforementioned surface and the aforementioned central portion are integrated, but are not limited thereto.
[0059] The embodiments of this specification will now be described in more detail. However, the experimental results described below are only representative of the experimental results described in the above embodiments and should not be construed as narrowing or limiting the scope and content of this specification due to the embodiments. Each effect in the various embodiments of this specification not explicitly shown below will be specifically described in the corresponding section.
[0060] Figure 1 This diagram illustrates an example of an existing surface treatment method, specifically a dental implant surface treatment method employing sandblasting and etching. (Refer to...) Figure 1 It can be confirmed that the surface of implants treated with existing sandblasting-etching is given surface roughness to have an irregular shape, especially the macroscopic surface with an irregular shape formed by sandblasting.
[0061] Figure 2 This is a schematic diagram illustrating a surface treatment method for a dental implant according to an embodiment of this specification. (Refer to...) Figure 2 This manual describes a method for surface preparation of dental implants that, for the first time, can be performed using laser processing of the implant surface. Specifically, a single laser treatment can process the surface of an implant that has not yet been individually roughened. Figure 2As shown, a macroscopic surface with a uniform shape can be achieved by regularly forming one or more first grooves on the surface of the implant using laser processing. When the macroscopic surface with one or more first grooves is etched to form a microscopic surface including one or more second grooves, the surface area of the implant increases. As a result, the bone-interfacial bonding force is increased through the unevenness effect, which may make the cellular response more active after implantation.
[0062] Example 1
[0063] Prepare a Cp-Ti (Titanium Grade 4) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Irradiate the surface of the sample with a 355 nm UV laser beam for 80 ns to form a macroscopic surface on the sample surface including a first groove with an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm.
[0064] After laser processing, the sample is immersed in a high-temperature (approximately 50°C) etching solution containing a mixture of hydrochloric acid and sulfuric acid for 10 minutes to form a microscopic surface on the sample containing a second groove with an average width of 3 μm and an average depth of 4 μm.
[0065] After etching, the above sample is immersed in pure water for 30 seconds, then immersed in 90% ethanol, ultrasonically treated for 5 minutes, and completely dried. Then, a dental implant with macroscopic and microscopic surfaces is manufactured.
[0066] Example 2
[0067] Prepare a Cp-Ti (Titanium Grade 4) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Irradiate the surface of the sample with a 355 nm UV laser beam for 100 ns to form a macroscopic surface on the sample surface including a first groove with an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm.
[0068] After laser processing, the sample is immersed in a high-temperature (approximately 50°C) etching solution containing a mixture of hydrochloric acid and sulfuric acid for 10 minutes to form a microscopic surface on the sample containing a second groove with an average width of 3 μm and an average depth of 4 μm.
[0069] After etching, the above sample is immersed in pure water for 30 seconds, then immersed in 90% ethanol, ultrasonically treated for 5 minutes, and completely dried. Then, a dental implant with macroscopic and microscopic surfaces is manufactured.
[0070] Example 3
[0071] Prepare a Cp-Ti (Titanium Grade 4) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Irradiate the surface of the sample with a 355 nm UV laser beam for 130 ns to form a macroscopic surface on the sample with a first groove at the upper end of a region corresponding to 1 mm, including an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm, and a first groove at the lower end corresponding to the remaining region, including an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm.
[0072] After laser processing, the sample is immersed in a high-temperature (approximately 50°C) etching solution containing a mixture of hydrochloric acid and sulfuric acid for 10 minutes to form a microscopic surface on the sample containing a second groove with an average width of 5 μm and an average depth of 5 μm.
[0073] After etching, the above sample is immersed in pure water for 30 seconds, then immersed in 90% ethanol, ultrasonically treated for 5 minutes, and completely dried. Then, a dental implant with macroscopic and microscopic surfaces is manufactured.
[0074] Example 4
[0075] Prepare a Cp-Ti (Titanium Grade 4) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Irradiate the surface of the sample with a 355 nm UV laser beam for 150 ns to form a macroscopic surface on the surface of the sample. The macroscopic surface consists of a first groove with an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm at the upper end of a 1 mm region, a first groove with an average depth of 20 μm to 35 μm and an average width of 30 μm to 65 μm at the lower end of a 4.5 mm region from the upper end, and a second groove with an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm at the lower end of the remaining region.
[0076] After laser processing, the sample is immersed in a high-temperature (approximately 50°C) etching solution containing a mixture of hydrochloric acid and sulfuric acid for 10 minutes to form a microscopic surface on the sample containing a second groove with an average width of 5 μm and an average depth of 5 μm.
[0077] After etching, the above sample is immersed in pure water for 30 seconds, then immersed in 90% ethanol, ultrasonically treated for 5 minutes, and completely dried. Then, a dental implant with macroscopic and microscopic surfaces is manufactured.
[0078] Comparative Example 1
[0079] Prepare Cp-Ti (Ti4 grade) samples in the form of discs (cylinders) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm, and prepare dental implants without any surface treatment.
[0080] Comparative Example 2
[0081] Prepare a Cp-Ti (Ti4 grade) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Spray alumina (Al2O3) powder with an average length of 250 μm to 500 μm at a pressure of 2.0 MPa for 1 minute to form a micro-surface containing a first groove with an average depth greater than 80 μm and an average width greater than 150 μm on the surface of the sample.
[0082] The subsequent etching and cleaning steps were performed in the same manner as in Example 3, and the dental implant with macroscopic and microscopic surfaces was manufactured using existing sandblasting and etching methods.
[0083] Comparative Example 3
[0084] Prepare a Cp-Ti (Ti4 grade) sample in the form of a disc (cylinder) with a diameter of 6 mm, a thickness of 2 mm, and a length of 10 mm. Spray alumina (Al2O3) powder with an average length of 250 μm to 500 μm at a pressure of 2.0 MPa for 1 minute to form a macroscopic surface on the surface of the sample. The upper part of the sample has a first groove with an average depth of 1 μm to 15 μm and an average width of 1 μm to 25 μm, and the lower part of the sample has a first groove with an average depth of 40 μm to 75 μm and an average width of 70 μm to 125 μm. The subsequent etching and cleaning steps are performed in the same manner as in Comparative Example 2 to manufacture a dental implant.
[0085] Experimental Example 1: Surface Characteristics of Dental Implants
[0086] Figure 3 SEM images of the surfaces of dental implants manufactured according to Examples 1 to 4 of this specification are shown. (Refer to...) Figure 3 It can be confirmed that the surface of the implants in Examples 1 to 4 has a first groove regularly formed by laser processing, thus achieving a regular and uniform macroscopic surface. Furthermore, a second groove is uniformly formed within the first groove, which is expected to improve the surface roughness and surface area of the implants, resulting in excellent osseointegration characteristics.
[0087] Experimental Example 2: Bone-to-skin bonding force of dental implants
[0088] Twenty dental implants, manufactured according to the examples and comparative examples, were implanted into the rabbit tibias by applying a torque of 1 N·m. Subsequently, the torque required to remove each implant from the tibia of each rabbit was measured at 2 weeks (14 days) and 4 weeks (28 days), and the average value was calculated. The results are as follows: Figure 6 As shown. (Refer to...) Figure 6 Compared to the implants of Examples 2 to 4, Example 1 showed slightly insufficient bone-interface bonding strength, while the implants of Examples 2 and 4 showed excellent bone-interface bonding strength, especially the implant of Example 4. On the other hand, compared to the examples, Comparative Examples 1 to 3 showed insufficient bone-interface bonding strength, especially the implant of Comparative Example 1 without surface treatment, which showed the worst bone-interface bonding strength. However, in the case of Comparative Example 3, a macroscopic surface with gradually increasing first groove values according to the upper and lower ends was formed, but because only a conventional sandblasting process was used, a uniform macroscopic surface was not formed, resulting in poor bone-interface bonding strength compared to the examples. Therefore, it can be confirmed that compared to the implants of the comparative examples that did not undergo surface treatment or whose macroscopic surfaces were formed by conventional sandblasting processes, the implants of the examples, by forming a regular and uniform macroscopic surface through laser processing, have improved osseointegration characteristics.
[0089] Experiment Example 3: Bacterial Proliferation Experiment of Dental Implants
[0090] To evaluate bacterial proliferation in the dental implants manufactured according to the examples and comparative examples, Streptococcus variant IFO 13955 was used. 100 μl of the Streptococcus variant was mixed with 10 μl of BHI solution and then incubated at 37°C and 5% CO2 for 12 hours. The cultured bacteria were diluted 10-fold 5 to 7 times with Brain Heart Infusion (BHI) solution to achieve a 10-10 6 CFU / ml up to 10 7 The concentration of CFU / ml was determined. The implants were then immersed in the bacterial solution, removed after 4 hours, rinsed with purified water, and the degree of bacterial proliferation on the surface of each implant was evaluated. The results are shown in Table 1 below. The relative evaluation of bone interface bonding force in Experiment 2 is also shown in Table 1.
[0091] Table 1
[0092]
[0093] Referring to Table 1, it can be confirmed that the bacterial proliferation in Examples 3 and 4 was excellent, and therefore, compared with Examples 1 and 2, and Comparative Examples 1, 2, and 3, almost no bacterial proliferation occurred. In the case of Example 1, bacterial proliferation was low, but the bone-interface bonding strength was slightly poor. In the case of Example 2, the bone-interface bonding strength was excellent, but bacterial proliferation was slightly high. Therefore, it can be confirmed that, as shown in Examples 3 and 4, by gradually increasing the value of the first groove based on the upper and lower ends or the upper end, the first lower end, and the second lower end, the bone-interface bonding strength characteristics can be improved, while bacterial proliferation can be suppressed. On the other hand, in the cases of Comparative Examples 1 and 2, which had first grooves with depth and width exceeding the required level through conventional sandblasting-etching treatment without surface treatment, the bone-interface bonding strength was poor compared with the examples, and bacterial proliferation was active. However, in the case of Comparative Example 3, the value of the first groove based on the upper and lower ends was gradually increased, so bacterial proliferation was suppressed to a certain extent compared with Comparative Examples 1 and 2, and the bone-interface bonding strength was slightly better, but relatively insufficient compared with Examples 3 and 4.
[0094] The descriptions in this specification are merely illustrative. Anyone skilled in the art to which any aspect of this specification pertains will understand that other specific forms can be easily derived without altering the technical concepts or essential features described herein. Therefore, the embodiments described above are merely illustrative in various respects and are not limited thereto. For example, the structural components described as a single type can also be implemented separately, and similarly, the structural components described separately can also be implemented in a combined form.
[0095] The scope of this specification is indicated by the appended claims, and all variations or modifications derived from the meaning, scope and equivalent concepts of the claims shall be interpreted as being included within the scope of this specification.
Claims
1. A surface treatment method for dental implants, characterized in that, include: Step (a): Laser processing of the implant surface; Step (b) involves etching the surface of the laser-processed implant. and Step (c) involves cleaning the etched implant. Through the above step (a), a macroscopic surface including one or more first grooves is formed on the surface of the implant. Through step (b) above, a microscopic surface including one or more second grooves is formed on the surface of the implant. By etching the surface of the laser-processed implant in step (b), one or more of the second grooves are formed inside the first groove; The peripheral surface of the aforementioned implant consists of an upper portion that contacts the cortical bone and a lower portion that contacts the cancellous bone. At least one of the average width and average depth of the first groove at the lower end of the outer peripheral surface of the implant is formed to be greater than at least one of the average width and average depth of the first groove at the upper end of the outer peripheral surface of the implant.
2. The surface treatment method for dental implants according to claim 1, characterized in that, The average width of the first groove is 5µm to 100µm, and the average depth is 5µm to 50µm.
3. The surface treatment method for dental implants according to claim 1, characterized in that, The average width and average depth of the second groove are 1µm to 10µm, respectively.
4. The surface treatment method for dental implants according to claim 1, characterized in that, Step (a) above includes: Step i), laser processing of the upper end of the outer peripheral surface of the implant; and Step ii), laser processing of the lower end of the outer peripheral surface of the implant.
5. The surface treatment method for dental implants according to claim 1, characterized in that, The lower end of the outer peripheral surface of the aforementioned implant is composed of a first lower end and a second lower end. Step (a) above includes: Step i), laser processing of the upper end of the outer peripheral surface of the implant; and Step ii), laser processing of the first lower end of the outer peripheral surface of the implant; and Step iii), laser processing of the second lower end of the outer peripheral surface of the implant.
6. A dental implant, which is a surface-treated dental implant, characterized in that, At least a portion of the implant surface includes a macroscopic surface with one or more first grooves and a microscopic surface with one or more second grooves. The first groove is formed by laser processing, and one or more second grooves are formed inside the first groove by etching the surface of the implant after laser processing; The peripheral surface of the aforementioned implant consists of an upper portion that contacts the cortical bone and a lower portion that contacts the cancellous bone. At least one of the average width and average depth of the first groove at the lower end of the outer peripheral surface of the implant is formed to be greater than at least one of the average width and average depth of the first groove at the upper end of the outer peripheral surface of the implant. The average depth of the first groove formed at the upper end is 1 to 15 μm and the average width is 1 to 25 μm. The average depth of the first groove formed at the lower end is 20 to 75 μm and the average width is 30 to 125 μm.
7. The dental implant according to claim 6, characterized in that, The lower end of the outer peripheral surface of the implant is composed of a first lower end and a second lower end.
Citation Information
Patent Citations
Method for treating surface of dental implant and dental implant with surface treated by same
CN120435266A
Implant, and method and system for producing such an implant
US20050260540A1
Surface processing method for dental implant
WO2023003265A1