A method for preparing a MEMS micromirror array

By combining bonding structures and processes, the problems of bonding adhesion failure and suspension film rupture in the manufacturing process of MEMS micromirror arrays were solved, achieving high-yield MEMS micromirror array fabrication, which is suitable for large-scale, highly integrated MEMS ultrathin devices.

CN117326521BActive Publication Date: 2026-11-24NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311120416.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2026-11-24
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

In the fabrication of MEMS micromirror arrays, there are problems such as bonding failure and suspension film rupture. In particular, during wafer bonding, the application of temperature, pressure and voltage may cause the bonding failure between the cavity structure formed by etching and the underlying substrate, and structural rupture may occur during the thinning process.

Method used

By employing a hybrid bonding structure and process, including metal thin film deposition, patterning, bonding adhesive spin coating and patterning, MEMS etching, and thinning, the hybrid bonding process solves the problems of bonding adhesion failure and suspended film rupture, and achieves submicron gap control between the torsion fulcrum and the underlying substrate.

Benefits of technology

High-yield fabrication of MEMS micromirror arrays has been achieved, which is suitable for large-scale, highly integrated MEMS ultrathin devices and promotes their widespread application in practical systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117326521B_ABST
    Figure CN117326521B_ABST
Patent Text Reader

Abstract

The application relates to a novel MEMS micromirror array processing method, which comprises the following steps: depositing a metal thin film on a first substrate surface; preparing a first addressing electrode and a second addressing electrode; selecting a second substrate, removing dust and organic residue existing on the surface; preparing an anchor point and a torsion fulcrum on the second substrate; continuing to etch the torsion fulcrum so that the surface of the torsion fulcrum is lower than the anchor point, thereby forming a height difference between the anchor point and the torsion fulcrum; bonding the first substrate and the second substrate; forming a metal reflecting layer on the thinned second substrate; completing the preparation of a micromirror structure; removing the adhesive bonding layer below the torsion fulcrum to complete the structure release of a discrete mirror surface; and the application solves the process problems of bonding adhesion failure of the torsion fulcrum and the substrate below the torsion fulcrum and rupture of a suspended thin film under the action of thinning external force in the preparation process of the MEMS micromirror array, and realizes the accurate control of the submicron gap between the torsion fulcrum and the substrate below the torsion fulcrum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of micro-opto-electro-mechanical systems (MEMS) technology, and in particular to a method for fabricating MEMS micromirror arrays. Background Technology

[0002] Spatial light modulator chips fabricated using Microelectromechanical Systems (MEMS) technology possess advantages such as small size, low power consumption, and strong integration and customization capabilities, and are now widely used in defense and civilian fields such as optical communication, spectral imaging, and projection displays. In particular, with the successful application of digital micromirror devices (DMDs) from Texas Instruments (TI) in commercial fields such as digital projectors, micromirrors have gradually become a research hotspot in the MEMS field.

[0003] One of the most critical challenges in micromirror fabrication is achieving a stress-free, smooth surface. In surface micromachining processes, both thin film deposition and sacrificial layer removal introduce residual stress, causing deformation of the fabricated micromirror. Even planarization before sacrificial layer removal has limited effectiveness. Furthermore, to release the sacrificial layer, "release holes" are typically created on the structural layer, negatively impacting the mirror's optical performance. Fabricating smooth micromirrors and elastic beams using single-crystal silicon and bulk micromachining offers significant advantages. Bulk micromachining micromirrors can be made from various materials, including single-crystal silicon and metals. Generally, single-crystal silicon exhibits significantly better stress and surface finish than polycrystalline silicon or metals. Micromirror structures are typically fabricated using a combination of deep silicon etching and wafer bonding. However, during wafer bonding, the applied temperature, pressure, and voltage can cause the etched cavity structure to fail bond to the underlying substrate. Even without these failures, structural areas not bonded to the substrate during the thinning of the single-crystal silicon structure can crack under external forces or internal residual stress. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a novel MEMS micromirror array fabrication method, which aims to solve the problems of bonding adhesion failure and suspension film rupture that occur in the manufacturing process of MEMS micromirror array chips by hybrid bonding structure and process, and at the same time provide a high-yield fabrication method for large-scale, highly integrated MEMS suspended ultrathin devices.

[0005] The technical solution adopted in this invention is a novel MEMS micromirror array fabrication method, which includes the following steps:

[0006] Step 1: Remove dust and organic matter from the surface of the first substrate by a cleaning process, and deposit a metal thin film on the surface of the first substrate using a metal thin film deposition process;

[0007] Step 2: Pattern the metal thin film using a metal etching process to complete the fabrication of the first addressing electrode and the second addressing electrode;

[0008] Step 3: Spin-coat bonding adhesive onto the surface of the first substrate and pattern it to form an adhesive bonding layer;

[0009] Step 4: Select a second substrate and remove dust and organic residues from its surface through a cleaning process;

[0010] Step 5: Use MEMS etching technology to fabricate anchor points and torsion fulcrums on the second substrate;

[0011] Step 6: Continue etching the torsion fulcrum using MEMS etching technology, making its surface lower than the anchor point, thus forming a height difference between the anchor point and the torsion fulcrum;

[0012] Step 7: Bond the first substrate and the second substrate using MEMS bonding technology;

[0013] Step 8: According to the preset requirements of micromirror driving, the second substrate is thinned using MEMS thinning technology;

[0014] Step 9: Deposit and pattern the metal on the thinned second substrate to form a metal reflective layer;

[0015] Step 10: Using the metal reflective layer described in Step 9 as a mask, pattern the remaining mirror structure using MEMS etching technology to complete the fabrication of the micromirror structure.

[0016] Step 11: Use MEMS polymer etching process to remove the adhesive bonding layer below the torsion fulcrum, and finally complete the structural release of the discrete mirror.

[0017] The beneficial effects of this invention are as follows: The MEMS micromirror array fabrication method proposed in this invention solves the technological challenges of bonding failure between the torsion fulcrum and the underlying substrate, and the rupture of the suspended film under thinning forces during the fabrication of MEMS micromirror arrays, by employing a hybrid bonding structure and process. This achieves precise control of the submicron gap between the torsion fulcrum and the underlying substrate. Furthermore, the fabrication method proposed in this invention is also applicable to other large-scale, highly integrated MEMS ultrathin devices, providing a novel high-yield fabrication method. This invention will promote the widespread application of MEMS ultrathin devices in practical systems.

[0018] Furthermore, the metal thin film mentioned in step 1 is divided into a bottom metal thin film and an upper metal thin film. The main function of the bottom metal thin film is to increase the adhesion between the upper metal thin film and the first substrate. Cr thin film, Ti thin film, or other thin films are selected. The upper metal thin film is selected from Au thin film, Al thin film, Cu thin film, or other materials with good conductivity. The metal thin film deposition process is selected from electron beam evaporation, magnetron sputtering, atomic layer deposition, etc.

[0019] Furthermore, the metal etching process described in step 2 is either a wet etching process or a plasma dry etching process.

[0020] Furthermore, the bonding adhesive mentioned in step 3 is selected from photosensitive bonding adhesives PMGI-SF11, BCB, PI, or SU8.

[0021] Furthermore, step 5 also includes depositing a bonding film on the surface of the anchor point, which is then patterned to form a second bonding layer;

[0022] The bonding film is selected from Ge film, Sn film, or other films that can be used for bonding.

[0023] Furthermore, the MEMS etching processes described in steps 5, 6, and 10 may include plasma dry etching, wet etching, or surface laser processing.

[0024] Furthermore, the MEMS bonding process described in step 7 is a hybrid bonding process, and the corresponding structure is a hybrid bonding structure, that is, the bonding region is divided into two parts, namely the anchor point and the first substrate, and the torsion fulcrum and the adhesive bonding layer. The two bonding regions use different bonding process types. Adhesive bonding is used between the torsion fulcrum and the adhesive bonding layer; the bonding process between the anchor point and the first substrate can be any one of anodic bonding, melt bonding, or eutectic bonding.

[0025] Furthermore, the hybrid bonding process is mainly divided into two stages: the first stage is adhesive bonding, and the second stage is any one of anodic bonding, melt bonding, and eutectic bonding.

[0026] Furthermore, the thinning process described in step 8 is any one of wet etching, chemical mechanical polishing, or plasma dry etching.

[0027] Furthermore, the metal deposited in step 9 may be selected from other metal films such as Au thin film, Al thin film, etc.

[0028] Furthermore, the MEMS polymer etching process described in step 11 is either oxygen plasma dry etching or wet etching. Attached Figure Description

[0029] Figure 1 This is a schematic diagram of the three-dimensional structure of the MEMS micromirror array described in this invention;

[0030] Figure 2 This is a schematic diagram of the MEMS micromirror array fabrication process provided in Embodiment 1 of the present invention;

[0031] Figure 3 This is a schematic diagram of the MEMS micromirror array fabrication process provided in Embodiment 2 of the present invention;

[0032] Figure 4 This is a schematic diagram of the MEMS micromirror array fabrication process provided in Embodiment 3 of the present invention.

[0033] As shown in the figure: 1. First substrate; 2. Bottom metal film; 3. Upper metal film; 4. First addressing electrode; 5. Second addressing electrode; 6. Bonding adhesive; 7. Adhesive bonding layer; 8. Second substrate; 9. Anchor point; 10. Torsion fulcrum; 11. Metal reflective layer; 12. Mirror; 13. Support beam; 14. First bonding layer; 15. Second bonding layer. Detailed Implementation

[0034] The invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can implement it based on the description. The scope of protection of the invention is not limited to these specific embodiments.

[0035] Those skilled in the art should understand that, in the disclosure of this invention, the terms "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, the above terms should not be construed as limiting this invention.

[0036] Furthermore, the terms "first," "second," and "third" are used only to distinguish descriptions and should not be interpreted as indicating or implying relative importance.

[0037] In the description of the embodiments of this application, it should also be noted that, unless otherwise expressly specified and limited, the terms "set," "install," "connect," and "link" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0038] The MEMS micromirror array involved in this invention is composed of multiple groups of equally spaced micromirror units. Each group of micromirror units mainly includes a first addressing electrode 4, a second addressing electrode 5, an anchor point 9, a torsion fulcrum 10, and a mirror surface 12. The first addressing electrode 4 and the second addressing electrode 5 are fabricated on a first substrate 1, while the anchor point 9, support beam 13, torsion fulcrum 10, and mirror surface 12 are fabricated on a second substrate 8. The mirror surface 12 is suspended above the first substrate 1 by the support beams 13 at both ends.

[0039] The first substrate 1 can be a glass sheet, a silicon wafer, or other substrate materials. The second substrate 8 is used to process anchor points and mirrors, and needs to be made of materials suitable for wafer-level MEMS bulk micromachining processes, and can be a regular silicon wafer, an SOI silicon wafer, or other materials.

[0040] Example 1:

[0041] The MEMS micromirror array in this embodiment consists of 1×60 micromirror units, with a spacing of 1 μm between the micromirror units. Each micromirror unit mainly includes a first addressing electrode 4, a second addressing electrode 5, an anchor point 9, a torsion fulcrum 10, a mirror surface 12, and a support beam 13. The first addressing electrode 4 and the second addressing electrode 5 are fabricated on a first substrate 1, while the anchor point 9, the torsion fulcrum 10, and the mirror surface 12 are fabricated on a second substrate 8. The mirror surface 12 is suspended above the first substrate 1 by the support beams 13 at both ends.

[0042] In this embodiment, the first substrate 1 is made of BF33 glass. The second substrate 8 is made of SOI silicon wafer, wherein the SOI silicon wafer 8 is composed of a device layer 8.1, an oxide layer 8.2, and a substrate layer 8.3.

[0043] See Figure 2 The MEMS micromirror array fabrication method proposed in this embodiment includes the following basic steps:

[0044] Step 1: Refer to Figure 2 (a) The dust and organic matter on the surface of BF33 glass plate 1 are removed by a cleaning process, and a 10nm Cr thin film 2 and a 100nm Au thin film 3 are deposited by electron beam evaporation.

[0045] Step 2: Refer to Figure 2 (b) The Au / Cr thin film is patterned using a gold-chromium wet etching process to form the first addressing electrode 4 and the second addressing electrode 5.

[0046] Step 3: Refer to Figure 2 (c)(d) A bonding adhesive 6, model PMGI-SF11, is spin-coated onto the surface of BF33 glass slide 1 at a spin speed of 2000 rpm and a spin coating thickness of 1.2 micrometers. After patterning, an adhesive bonding layer 7 is formed.

[0047] Step 4: Refer to Figure 2 (e) SOI silicon wafer 8 is selected as the second substrate according to the processing requirements (device layer 8.1 is 15μm; oxide layer 8.2 is 1μm; substrate layer 8.3 is 300μm), and dust and organic residues on the surface are removed by cleaning process;

[0048] Step 5: Refer to Figure 2 (f) Anchor point 9 and torsion fulcrum 10 were fabricated on the device layer of SOI silicon wafer 8 using plasma dry etching process, with an etching height of 10 μm.

[0049] Step 6: Refer to Figure 2 (g) The torsion fulcrum 10 is further etched using plasma dry etching process to a depth of 500 nm, so that its surface is lower than the anchor point 9, and the height difference between the anchor point 9 and the torsion fulcrum 10 is 500 nm.

[0050] Step 7: Refer to Figure 2 (h) The BF33 glass sheet 1 and the SOI silicon wafer 8 are hybrid bonded. The anchor point 9 and the BF33 glass sheet 1 are bonded by silicon-glass anodic bonding, and the torsion fulcrum 10 and the BF33 glass sheet 1 are bonded by adhesive bonding. The hybrid bonding process is mainly divided into two stages. The first stage is adhesive bonding, with the process conditions of 270℃ and 1800N. The second stage is anodic bonding, with the process conditions of 270℃, 5000N, and 1000V. The two stages are carried out continuously.

[0051] Step 8: Refer to Figure 2 (i) According to the preset requirements of micromirror driving, the 300μm substrate layer 8.3 and the 1μm oxide layer 8.2 of SOI silicon wafer 8 are removed by plasma dry etching process;

[0052] Step 9: Refer to Figure 2 (j) A 200 nm Au film is deposited and patterned on the surface of the thinned SOI silicon wafer device layer 8.1 to form a metal reflective layer 11;

[0053] Step 10: Refer to Figure 2 (k) Using the metal reflective layer 11 in step 9 as a mask, the remaining 5μm thick device layer 8.1 is etched using a plasma dry etching process to finally form a discrete mirror 12.

[0054] Step 11: Refer to Figure 2 (l) The adhesive bonding layer 7 below the torsion fulcrum is removed by using oxygen plasma dry etching process, and finally the structure of the discrete mirror 12 is released.

[0055] Example 2:

[0056] The micromirror array in this embodiment consists of 1×50 micromirror units, with a spacing of 2 μm between the micromirror units. Each micromirror unit mainly includes a first addressing electrode 4, a second addressing electrode 5, an anchor point 9, a torsion fulcrum 10, a mirror surface 12, and a support beam 13. The first addressing electrode 4 and the second addressing electrode 5 are fabricated on a first substrate 1, while the anchor point 9, the torsion fulcrum 10, the mirror surface 12, and other structures are fabricated on a second substrate 8. The mirror surface 12 is suspended above the first substrate 1 by the support beams 13 at both ends.

[0057] The first substrate 1 is made of BF33 glass. The second substrate 7 is made of ordinary silicon wafer.

[0058] See Figure 3 The MEMS micromirror array fabrication method proposed in this embodiment includes the following basic steps:

[0059] Step 1: Refer to Figure 3 (a) The dust and organic matter that may exist on the surface of BF33 glass plate 1 are removed by cleaning process, and a 15nm Ti thin film 2 and a 150nm Al thin film 3 are deposited by magnetron sputtering process.

[0060] Step 2: Refer to Figure 3 (b) The Al / Cr thin film is patterned using a wet etching process to form the first addressing electrode 4 and the second addressing electrode 5;

[0061] Step 3: Refer to Figure 3 (c)(d) A bonding adhesive 6 of model SU-8 was spin-coated onto the surface of BF33 glass slide 1 at a spin speed of 2500 rpm and a spin coating thickness of 2 μm. After patterning, an adhesive bonding layer 7 was formed.

[0062] Step 4: Refer to Figure 3 (e) According to the processing requirements, a 300μm ordinary silicon wafer is selected as the second substrate 8, and the dust and organic residue on the surface are removed by a cleaning process.

[0063] Step 5: Refer to Figure 3 (f) Anchor points and torsion fulcrum points 9 are fabricated on silicon wafer 8 using a wet etching process with an etching height of 8 μm;

[0064] Step 6: Refer to Figure 3 (g) The torsion fulcrum 10 is further etched using a wet etching process so that its surface is lower than that of the anchor point 9, with an etching depth of 1 μm and a height difference of 1 μm between the anchor point 9 and the torsion fulcrum 10.

[0065] Step 7: Refer to Figure 3(h) The BF33 glass sheet 1 and the silicon wafer 8 are hybrid bonded. The anchor point 9 and the BF33 glass sheet 1 are bonded by silicon-glass anodic bonding, and the torsion fulcrum 10 and the BF33 glass sheet 1 are bonded by adhesive bonding. The hybrid bonding process is mainly divided into two stages. The first stage is adhesive bonding, with the process conditions of 280℃ and 1800N. The second stage is anodic bonding, with the process conditions of 300℃, 3000N, and 1000V. The two stages are carried out continuously.

[0066] Step 8: Refer to Figure 3 (i) According to the preset requirements of micromirror driving, the silicon wafer 8 is thinned to 15 micrometers using chemical mechanical polishing process;

[0067] Step 9: Refer to Figure 3 (j) An Al film is deposited and patterned on the thinned silicon wafer 8 to form a metal reflective layer 11;

[0068] Step 10: Refer to Figure 3 (k) Using the metal reflective layer 11 in step 9 as a mask, the remaining 7μm thick silicon wafer is patterned using surface laser micromachining technology to form discrete mirror 12.

[0069] Step 11: Refer to Figure 3 (l) Select the appropriate solvent and use a wet etching process to remove the adhesive bonding layer 7 below the torsion fulcrum, thus completing the structural release of the discrete mirror 12.

[0070] Example 3:

[0071] The micromirror array in this embodiment consists of 1×70 micromirror units, with a spacing of 3 μm between the micromirror units. Each micromirror unit mainly includes a first addressing electrode 4, a second addressing electrode 5, an anchor point 9, a torsion fulcrum 10, a mirror surface 12, and a support beam 13. The first addressing electrode 4 and the second addressing electrode 5 are fabricated on a first substrate 1, while the anchor point 9, the torsion fulcrum 10, the mirror surface 12, and other structures are fabricated on a second substrate 8. The mirror surface 12 is suspended above the first substrate 1 by the support beams 13 at both ends.

[0072] The first substrate 1 is made of BF33 glass. The second substrate 7 is made of SOI silicon wafer.

[0073] See Figure 4 The micromirror array fabrication method proposed in this embodiment includes the following basic steps:

[0074] Step 1: Refer to Figure 4 (a) The dust and organic matter that may exist on the surface of BF33 glass plate 1 are removed by cleaning process, and a 20nm Cr thin film and a 200nm Au thin film 3 are deposited by magnetron sputtering process.

[0075] Step 2: Refer to Figure 4 (b) The Au / Cr thin film is patterned using a wet etching process to form the first addressing electrode 4, the second addressing electrode 5 and the first bonding layer 14;

[0076] Step 3: Refer to Figure 4 (c)(d) A bonding adhesive 6, model PMGI-SF11, was spin-coated onto the surface of BF33 glass slide 1 at a spin speed of 2500 rpm and a spin coating thickness of 1 μm. After patterning, an adhesive bonding layer 7 was formed.

[0077] Step 4: Refer to Figure 4 (e) According to the processing requirements, an SOI silicon wafer is selected as the second substrate 8 (the device layer 8.1 is 13μm; the oxide layer 8.2 is 1.5μm; and the substrate layer 8.3 is 400μm), and the dust and organic residues on the surface are removed by a cleaning process;

[0078] Step 5: Refer to Figure 4 (f)(g) A 200 nm Sn film is deposited on the surface of the SOI silicon wafer device layer, and after patterning, a second bonding layer 15 is formed. Anchor points 9 and torsion fulcrums 10 are fabricated on the SOI silicon wafer device layer 8.1 using surface laser micromachining technology, with an etching height of 8 μm.

[0079] Step 6: Refer to Figure 4 (h) The surface laser micromachining process is used to continue etching the torsion fulcrum 10 so that its surface is lower than the anchor point 9, forming a height difference of 400nm between the anchor point 9 and the torsion fulcrum 10.

[0080] Step 7: Refer to Figure 4 (i) BF33 glass sheet 1 and SOI silicon wafer 8 are hybrid bonded. Anchor point 9 and BF33 glass sheet 1 are bonded by gold-tin eutectic bonding, and torsion fulcrum 10 and BF33 glass sheet 1 are bonded by adhesive bonding. The hybrid bonding process is mainly divided into two stages. The first stage is adhesive bonding, with the process conditions being: temperature 290℃ and pressure 2000N; the second stage is anodic bonding, with the process conditions being: temperature 350℃, pressure 2000N, and voltage 800V. The two stages are carried out continuously.

[0081] Step 8: Refer to Figure 4 (g) According to the preset requirements of micromirror driving, the substrate layer 8.3 and oxide layer 8.2 of SOI silicon wafer 8 are removed by wet etching process;

[0082] Step 9: Refer to Figure 4 (k) A 200nm Au film is deposited and patterned on the surface of the thinned SOI silicon wafer 8 to form a metal reflective layer 11;

[0083] Step 10: Refer to Figure 4 (l) Using the metal reflective layer 11 in step 9 as a mask, the remaining 5μm device layer 8.1 is patterned using plasma dry etching process to form discrete mirror 12.

[0084] Step 11: Refer to Figure 4 (m), select the appropriate solvent and use wet etching process to remove the adhesive bonding layer 7 below the torsion fulcrum, thus completing the structural release of the discrete mirror 12.

Claims

1. A method for fabricating a MEMS micromirror array, characterized in that: The method includes the following steps: Step 1: Remove dust and organic matter from the surface of the first substrate (1) by cleaning process, and deposit a metal film on the surface of the first substrate (1) using metal thin film deposition process; Step 2: Pattern the metal thin film using a metal etching process to complete the fabrication of the first addressing electrode (4) and the second addressing electrode (5); Step 3: Spin-coat bonding adhesive (6) onto the surface of the first substrate (1) and pattern it to form an adhesive bonding layer (7); Step 4: Select the second substrate (8) and remove dust and organic residues from the surface through a cleaning process; Step 5: Use MEMS etching technology to fabricate the anchor point (9) and torsion fulcrum (10) on the second substrate (8); Step 6: Continue etching the torsion fulcrum (10) using MEMS etching technology, so that its surface is lower than the anchor point (9), forming a height difference between the anchor point (9) and the torsion fulcrum (10); Step 7: Bond the first substrate (1) and the second substrate (8) using MEMS bonding technology; Step 8: According to the preset requirements of micromirror driving, the second substrate (8) is thinned using MEMS thinning process; Step 9: Deposit and pattern the metal on the thinned second substrate (8) to form a metal reflective layer (11); Step 10: Using the metal reflective layer (11) described in step 9 as a mask, pattern the remaining mirror structure using MEMS etching process to complete the fabrication of the micromirror structure; Step 11: Use MEMS polymer etching process to remove the adhesive bonding layer (7) below the torsion fulcrum (10) to complete the structural release of the discrete mirror (12).

2. The MEMS micromirror array fabrication method according to claim 1, characterized in that: The metal thin film mentioned in step 1 is divided into a bottom metal thin film (2) and an upper metal thin film (3). The bottom metal thin film (2) is selected as a Cr thin film or a Ti thin film, and the upper metal thin film (3) is selected as an Au thin film, an Al thin film or a Cu thin film. The metal thin film deposition process is selected as an electron beam evaporation process, a magnetron sputtering process or an atomic layer deposition process.

3. The MEMS micromirror array fabrication method according to claim 1, characterized in that: The metal etching process described in step 2 can be either wet etching or plasma dry etching.

4. The MEMS micromirror array fabrication method according to claim 1, characterized in that: The bonding adhesive (6) mentioned in step 3 is selected from photosensitive bonding adhesives (6) such as PMGI-SF11, BCB, PI or SU8.

5. The MEMS micromirror array fabrication method according to claim 1, characterized in that: Step 5 further includes depositing a bonding film on the surface of the anchor point (9), and forming a second bonding layer (15) after patterning; wherein the bonding film is selected as a Ge film or a Sn film.

6. The MEMS micromirror array fabrication method according to claim 1, characterized in that: The MEMS etching processes described in steps 5, 6, and 10 can be plasma dry etching, wet etching, or surface laser processing.

7. A method for fabricating a MEMS micromirror array according to claim 1, characterized in that: The MEMS bonding process described in step 7 is a hybrid bonding process, and the corresponding structure is a hybrid bonding structure. That is, the bonding region is divided into two parts: one part is the anchor point (9) and the first substrate (1), and the other part is the torsion fulcrum (10) and the adhesive bonding layer (7). The two bonding regions use different bonding process types. The torsion fulcrum (10) and the adhesive bonding layer (7) are bonded together by adhesive bonding. The bonding process between the anchor point (9) and the first substrate (1) is any one of anodic bonding, fusion bonding, and eutectic bonding. The hybrid bonding process is divided into two stages: the first stage is adhesive bonding, and the second stage is any one of anodic bonding, fusion bonding, and eutectic bonding.

8. The MEMS micromirror array fabrication method according to claim 1, characterized in that: The thinning process described in step 8 is any one of wet etching, chemical mechanical polishing, or plasma dry etching.

9. A method for fabricating a MEMS micromirror array according to claim 1, characterized in that: The metal deposited in step 9 is selected from Au thin films or Al thin films.

10. A method for fabricating a MEMS micromirror array according to claim 1, characterized in that: The MEMS polymer etching process described in step 11 uses either oxygen plasma dry etching or wet etching.

Citation Information

Patent Citations

  • Manufacturing method of wafer level glass microcavity used for packaging MEMS

    CN101734612A

  • Silicon nitride anodic bonding-based (111) silicon transfer process

    CN115215285A