A polyglycolic acid-based degradable material suitable for low temperature wells and a method of making the same
By introducing polyethylene oxide segments into polyglycolic acid-based materials and copolymerizing them using a twin-screw extruder, the problems of slow degradation rate and insufficient mechanical properties in low-temperature wells were solved, achieving rapid degradation and effective plugging.
Patent Information
- Application Number
- CN202210736072.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-27
AI Technical Summary
Existing polyglycolic acid-based biodegradable materials have a slow degradation rate in low-temperature wells, which cannot meet the application requirements, and their mechanical properties are insufficient in low-temperature well environments.
By introducing hydrophilic segments of polyethylene oxide into polyglycolic acid-based materials and performing melt extrusion copolymerization using a twin-screw extruder, PEO-b-PGA or PGA-b-PEO-b-PGA block copolyesters can be prepared, thereby improving the hydrophilicity and mechanical properties of the materials.
Rapid degradation and effective plugging were achieved in a low-temperature well environment. After being kept in water for 3 days, the tensile strength of the material decreased by more than 50%, while the mechanical properties remained good, and the degradation rate was significantly improved.
Smart Images

Figure CN117327261B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials, specifically relating to a polyglycolic acid-based biodegradable material suitable for low-temperature wells and its preparation method. Background Technology
[0002] In oilfield applications, many low-permeability oil and gas reservoirs require fracturing to achieve stable production capacity, making temporary plugging materials widely used. Currently, many biodegradable temporary plugging materials are based on biodegradable metals. While these metals have high strength, their degradation conditions are demanding, requiring immersion in solvents for degradation. Biodegradable polymer materials, on the other hand, can degrade in an aqueous environment, avoiding secondary pollution to underground reservoirs, thus improving efficiency and saving costs.
[0003] Polyglycollide (PGA), also known as polyhydroxyacetic acid or polyglycolic acid, is a linear aliphatic polyester with the simplest chemical structure. It is a polymer material with good biocompatibility and unique biodegradability. Its high crystallinity gives it high strength, making it suitable for applications requiring high material strength, such as surgical sutures, orthopedic fixation, and tissue repair materials.
[0004] Polyethylene glycol (PEO), also known as ethylene glycol polyoxyethylene ether or polyethylene oxide, typically has hydroxyl or methoxy groups at its end groups. Its molecular weight ranges from 200,000 to 5,000,000. It possesses good water solubility, biocompatibility, and flexibility, and is non-toxic and non-irritating. Its properties vary depending on its relative molecular weight, ranging from a colorless, odorless, viscous liquid to a waxy solid, and it has a relatively low glass transition temperature and melting point.
[0005] Current research includes patents for PGA applications in oilfields, such as Chinese patents CN105189636A, CN108368572A, and CN106761546A. These patents primarily operate under high-temperature well conditions. However, the material still exhibits a slow degradation rate under low-temperature well conditions, failing to meet usage requirements and limiting its application scenarios. Therefore, it is necessary to develop a modified material that can be used in low-temperature wells to address these current technical challenges. Summary of the Invention
[0006] This invention provides a polyglycolic acid-based biodegradable material that is safe and maintains its shape for a long time in cryogenic well environments, achieving effective plugging and exhibiting rapid degradation after use. By reacting and extruding copolymerizing glycolic acid or its derivatives under the initiation of polyethylene oxide, a polyglycolic acid-based biodegradable block copolymer containing hydrophilic segments of polyethylene oxide is obtained. Introducing other flexible block copolymer components with higher hydrophilicity into the polyglycolic acid segments enhances the binding force of the polyglycolic acid-based biodegradable material with water in cryogenic well environments, achieving effective plugging and exhibiting a faster degradation rate after use.
[0007] One objective of this invention is to provide a polyglycolic acid-based biodegradable material, obtained by reacting raw materials containing the following components, in parts by weight:
[0008] (1) 90 to 99.5 parts of glycolic acid or its derivatives, preferably 92 to 99 parts;
[0009] (2) 0.5 to 10 parts of polyethylene oxide polymer, preferably 1 to 8 parts.
[0010] According to a specific embodiment of the present invention, the biodegradable material has a structural formula including at least one of PEO-b-PGA and PGA-b-PEO-b-PGA; the biodegradable material has a structural formula of PEO-b-PGA or PGA-b-PEO-b-PGA, or may include both of the above structural formulas; the biodegradable material has one or two melting points; the number average molecular weight of the biodegradable material is 80,000 to 200,000 g / mol, preferably 90,000 to 150,000 g / mol.
[0011] According to a specific embodiment of the present invention, the water contact angle of the polyglycolic acid-based biodegradable material is below 50°, indicating a certain degree of hydrophilicity; after the biodegradable material is kept in deionized water at 37°C for 3 days, the tensile strength decreases by no less than 50%, indicating that the polyglycolic acid-based biodegradable material can guarantee certain mechanical properties, achieve effective sealing, and the degradation rate is significantly improved in a low-temperature well environment.
[0012] According to a specific embodiment of the present invention, the glycolic acid or its derivative is selected from at least one of glycolic acid, glycolide, methyl glycolate, and glycolic anhydride, preferably glycolide; the polyoxyethylene polymer is a polymer formed by ring-opening polymerization of ethylene oxide with water or alcohol, preferably, the viscosity-average molecular weight of the polyoxyethylene polymer is 20,000 to 300,000 g / mol, more preferably 50,000 to 200,000 g / mol.
[0013] According to a specific embodiment of the present invention, the polyglycolic acid-based biodegradable material further comprises, by weight, 0.01 to 0.1 parts of other additives, preferably 0.02 to 0.08 parts; the other additives may be any additive components commonly used in the art, for example, at least one selected from antioxidants and anti-hydrolysis agents, preferably, the antioxidants may be at least one selected from hindered phenolic antioxidants, phosphite antioxidants, and sulfur-containing antioxidants; the anti-hydrolysis agents may be at least one selected from bis(2,6-diisopropylbenzene)carbodiimide, polycarbodiimide, and low molecular weight epoxy prepolymers.
[0014] The second objective of this invention is to provide a method for preparing the above-mentioned polyglycolic acid-based biodegradable material, which includes mixing components including glycolic acid or its derivatives and polyethylene oxide polymer, and then performing a melt extrusion reaction to obtain the polyglycolic acid-based biodegradable material; the melt extrusion is preferably performed using a twin-screw extruder.
[0015] According to a specific embodiment of the present invention, a metal compound catalyst is further added to the components. The metal compound catalyst is selected from at least one of group IIA-VA metal salts and transition metal salts, preferably from at least one of stannous octoate, stannous chloride, aluminum isopropoxide, bismuth acetate, n-butyl titanate, and tetrabutyl stannate, and more preferably from stannous chloride. The metal compound catalyst is 0.01 to 0.5 parts by weight, preferably 0.03 to 0.3 parts by weight.
[0016] According to a specific embodiment of the present invention, other additives are also added to the components. These other additives include one or more of the following: antioxidants, metal passivators, compatibilizers, plasticizers, and anti-hydrolysis agents. All of the above additives can be commonly used additive components in the art.
[0017] According to a specific embodiment of the present invention, the melt extrusion can be carried out using a commonly used twin-screw extruder and extrusion reaction conditions. Preferably, the extrusion reaction conditions are as follows: the extrusion reaction temperature is 150-250°C, preferably 160-230°C; the extrusion reaction time is 3-20 min, preferably 5-10 min; and the extruder speed is 5-150 rpm, preferably 20-80 rpm.
[0018] A third objective of this invention is to provide a polyglycolic acid-based biodegradable material prepared by the above-described method. Specifically, the particle size of the polyglycolic acid-based biodegradable material is 0.1–4 mm, preferably 0.2–3.5 mm. The shape of the polyglycolic acid-based biodegradable material is not particularly limited; for example, it can be prepared into common spherical particles.
[0019] A fourth objective of this invention is to provide the above-mentioned polyglycolic acid-based biodegradable material, or the polyglycolic acid-based biodegradable material prepared by the above-mentioned preparation method, for use as a cryogenic well plugging material. The polyglycolic acid-based biodegradable material can be used directly or injection molded into spherical shapes for use as a cryogenic well plugging material.
[0020] In this invention, glycolic acid or its derivatives and polyethylene oxide polymers are polymerized under melt extrusion conditions in the presence of a catalyst to obtain a biodegradable polymer with regular blocks, exhibiting excellent mechanical properties. At the same time, the polyethylene oxide segments on the molecular chain after the crosslinking reaction exhibit suitable hydrophilicity. When used as a cryogenic well plugging material, it can maintain good mechanical properties in the initial stage, but the mechanical properties rapidly decline after 3 days, making it suitable for the needs of cryogenic well applications.
[0021] Compared with the prior art, the present invention has the following superior effects:
[0022] 1. The polyglycolic acid-based biodegradable material provided by this invention has good hydrophilicity, and its degradation rate is significantly improved in a low-temperature well environment;
[0023] 2. The polyglycolic acid-based biodegradable material provided by this invention can guarantee certain mechanical properties and achieve effective sealing.
[0024] 3. The present invention uses a twin-screw extruder for continuous polymerization, which saves time, simplifies the process, and has higher production efficiency compared with the batch reactor polymerization in the prior art;
[0025] 4. The preparation method provided by this invention is simple and efficient in production process and has broad application prospects. Attached Figure Description
[0026] Figure 1 The results are DSC test results of the polyglycolic acid-based biodegradable materials obtained in Examples 1, 3, 5, and 7.
[0027] Figure 2 The water contact angle test results for Comparative Example 1 and Examples 1, 4-7 were obtained from... Figure 2 As can be seen from the data, the polyglycolic acid-based biodegradable materials obtained in Examples 1 and 4-7 exhibit better hydrophilicity compared to Comparative Example 1.
[0028] Figure 3 To test the degradation of Comparative Example 1 and Examples 5 and 6 in water, Figure 3 In the diagram, the horizontal axis represents time, and the vertical axis represents tensile strength. Figure 3 As can be seen from the results, the tensile strength of the polyglycolic acid-based biodegradable materials prepared in Examples 5 and 6 decreased more significantly in water, indicating that the polyglycolic acid-based biodegradable materials prepared in this invention degraded at a faster rate in water.
[0029] Figure 4 Comparing the contact angles of Comparative Examples 2-5 and Examples 4-7, it can be seen that the contact angles of the materials prepared under blending conditions in Comparative Examples 2-5 are all greater than the contact angles of the materials obtained by melt polymerization in this invention, indicating that the polyglycolic acid-based biodegradable materials obtained by the reactive extrusion polymerization process of this invention exhibit better hydrophilicity. Detailed Implementation
[0030] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0031] The testing instruments and conditions used in this embodiment are as follows:
[0032] Melt Flow Index (MFR) determination method: According to ISO 1133 standard, the Instron CEAST MF20 melt flow indexer was used for determination. The barrel temperature was 230℃, the weight load was 1.05kg, the die diameter was 2.095mm, the preheating time was 30s, and the sample was automatically measured at set intervals. The average value was calculated for 5 measurements, and the result was expressed as grams per 10 minutes (g / 10min).
[0033] Thermal performance analysis (DSC): Tests were performed on a Discovery series differential scanning calorimeter (DSC) manufactured by TA Instruments, using TA Instruments Trios version 3.1.5 software. This DSC instrument is equipped with a TARefrigerated Cooling System 90 mechanical refrigeration accessory. The test atmosphere was nitrogen at a flow rate of 50 mL / min, and the required sample volume was 5–10 mg. The test procedure was as follows: the temperature was first stabilized at 40℃, then increased to 250℃ at a rate of 10℃ / min and held at that temperature for 1 min to remove thermal history. The temperature was then decreased to -60℃ at a rate of 10℃ / min, followed by a reheat to 250℃ at a rate of 10℃ / min. The cooling process and the second heating process were recorded to study the thermal properties of the sample. The glass transition ("T") of the sample can be directly obtained from the DSC test using the software. g Melting temperature (T) m Information such as ""
[0034] Contact angle test: The test was conducted on a German KRUSS-DSA100 contact angle measuring instrument. The test procedure was as follows: the sample was laid flat on the sample stage, a suitable liquid was selected, and a small droplet of about 5L was squeezed out through a syringe and hung on the needle. The sample stage was moved to gently stick the small droplet onto the sample. After a set time, a picture was taken. The angle between the tangent of the contact edge between the droplet and the sample and the sample plane in the picture was analyzed by the software. This angle is the contact angle of the sample.
[0035] Mechanical property testing: The test was conducted on a universal testing instrument (model 3344) manufactured by Instron Corporation in the United States. The test temperature was 20℃, the test humidity was 65%, the tensile rate was 5mm / min, the effective length of the sample was 30mm, and the width was 4mm. The tensile stress and elongation at break of 5 samples from the same batch were recorded, and the average value was taken.
[0036] Degradation performance test: The raw material was injection molded into standard specimens with an effective length of 30 mm and a width of 4 mm. These specimens were then immersed in deionized water and placed in a constant temperature and humidity chamber at 37°C. The samples were removed periodically to test their mechanical properties and analyze their degradation rate under specific conditions.
[0037] The raw materials used in the examples and their sources are as follows:
[0038] The glycolide (GA) monomer used in this invention was produced by Jinan Daigang Biotechnology Co., Ltd., China. Three polyethylene oxide (PEO) monomers, with viscosity-average molecular weights of 50,000 g / mol, 100,000 g / mol, and 200,000 g / mol, were provided by China National Pharmaceutical Group Corporation. Stannous chloride (SnCl2) was provided by Shanghai Maclean Reagent Co., Ltd. Polyglycolic acid (PGA) was produced by Corbion AG, Netherlands, with a weight-average molecular weight of approximately 150,000 g / mol.
[0039] [Examples 1-7] Preparation of Polyglycolic Acid-Based Biodegradable Materials
[0040] Ethylene lactide powder was first dried in a vacuum oven at 60℃ for 5 hours to remove moisture. Then, GA / PEO were mixed in a mixer at a specific mass fraction ratio, as shown in Table 1 below, with a mixing time of 3 minutes. Subsequently, 0.3 parts by mass of Sn(Cl)₂ were added to the mixed powder and mixed thoroughly. Granulation was performed using a Eurolab 16 co-rotating twin-screw extruder (screw diameter 16 mm, L / D ratio L / D = 40) manufactured by Thermo Fisher Scientific, USA. This extruder has 11 sections from the feed port to the die, numbered 1-11. Section 1 only serves as the feeding section and does not provide heating. Due to slight variations in the properties of the raw materials used in this reaction extrusion, the temperatures in each section differ, as shown in Table 2 below. The extrusion reaction time was approximately 5 minutes. The screw speed was set at 50 rpm. During stable operation, the maximum torque was 20%-30%. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample is extruded from the die and cooled by air, it is cut into cylindrical particles with a diameter of 3 mm by a pelletizer. The particles are then dried in a vacuum oven at 30°C for 5 hours and then packaged for later use.
[0041] Table 1. Raw materials and proportions of the polyglycolic acid-based biodegradable materials in Examples 1-7
[0042] Sample Name <![CDATA[M V (PEO)]]> PEO feed percentage (%) Example 1 50000 2 Example 2 50000 5 Example 3 50000 8 Example 4 100000 1 Example 5 100000 2 Example 6 200000 1 Example 7 200000 2
[0043] Table 2. Temperatures of each heating section of the reactive extruder in Examples 1-7
[0044]
[0045] [Example 8] DSC testing of polyglycolic acid-based biodegradable materials
[0046] The polyglycolic acid-based biodegradable materials prepared in Examples 1-7, as well as the homopolymer PGA and three different viscosity-average molecular weight polyethylene oxides, were subjected to differential scanning calorimetry (DSC) tests according to the steps described above, resulting in a second heating curve. The melting temperature (T0) was directly obtained from the curve using specialized software. m ), glass transition (T) g Information such as )
[0047] Table 3. Thermal performance parameters of polyglycolic acid-based biodegradable materials and PGA and PEO in Examples 1-7
[0048] Sample Name <![CDATA[T g (℃)]]> <![CDATA[T m(PEO) (℃)]]> <![CDATA[T m(PGA) (℃)]]> PGA 47.5 - 225.40 Example 1 47.7 - 219.21 Example 2 46.9 57.14 220.35 Example 3 45.7 57.31 221.51 Example 4 46.3 - 222.47 Example 5 46.8 - 221.61 Example 6 46.9 222.15 Example 7 47.2 - 221.48 PEO50000 - 59.06 - PEO100000 - 61.54 - PEO200000 - 62.23 -
[0049] from Figure 1As shown in Table 3, in Examples 1 and 4-7, adding a small amount of PEO (<5%) as an initiator for polymerization resulted in biodegradable materials with only one glass transition temperature and one melting point attributed to PGA in thermodynamic tests, and the melting point of the PGA segments did not change significantly. This is because the low PEO content prevented it from reflecting the thermal characteristics of the segments. When the PEO content increased to above 5%, a faint PEO melting peak appeared, confirming that some PEO segments were indeed present in the PGA polymer and formed an independent phase. Meanwhile, the melting temperature of the PGA segments remained around 220°C, indicating that the obtained biodegradable materials contained longer PGA blocks.
[0050] [Example 9] Melt Flow Index Test of Polyglycolic Acid-Based Biodegradable Materials
[0051] The particles obtained in Examples 1 to 7 and the PGA homopolymer were subjected to melt index determination in an Instron CEAST MF20 melt indexer. The test conditions and test results are shown in Table 4.
[0052] Table 4. Melt index of pure PGA and biodegradable materials obtained in Examples 1-7
[0053] Sample Name Test conditions Melt index (g / 10min) PGA 230℃, 1.05kg 14.01 Example 1 230℃, 1.05kg 24.43 Example 2 230℃, 1.05kg 29.06 Example 3 230℃, 1.05kg 34.72 Example 4 230℃, 1.05kg 27.58 Example 5 230℃, 1.05kg 31.24 Example 6 230℃, 1.05kg 28.43 Example 7 230℃, 1.05kg 30.26
[0054] As shown in Table 4, the flow properties of the PGA block polymer modified materials in Examples 1-3 gradually increased with the gradual increase of PEO content. However, when the PEO content was low and the molecular weight of PEO was different (Examples 4 and 6), the change in melt index was not obvious, and the flow properties of the PGA copolymer changed slightly and could be ignored.
[0055] [Example 10] Contact Angle Test of Polyglycolic Acid-Based Biodegradable Materials
[0056] The polyglycolic acid-based biodegradable material particles obtained in Examples 1-7 were pressed into thin sheets on a hot plate, and the water contact angle was tested using a German KRUSS-DSA100 contact angle meter to analyze the hydrophilicity of the samples. The results are shown in Table 5 below. Figure 2 As shown.
[0057] Table 5. Water contact angles of Examples 1-7 and PGA
[0058] Sample Name Contact angle (°) Example 1 50.2 Example 2 21.3 Example 3 20.8 Example 4 46.2 Example 5 38.7 Example 6 42.3 Example 7 20.4 PGA 68.1
[0059] The contact angle of the PEO-induced PGA polymer was significantly reduced, confirming an improvement in its hydrophilicity. Furthermore, the hydrophilicity increased with increasing PEO content.
[0060] [Example 11] Mechanical property testing of polyglycolic acid-based biodegradable materials
[0061] The mechanical properties of the pure PGA polymer and the polyglycolic acid-based biodegradable materials obtained in Examples 5 and 6 were tested respectively. The elongation at break and tensile strength of the two were compared. In Examples 5 and 6, even with the addition of PEO segments, the tensile strength could still be maintained at around 100 MPa, which showed high mechanical strength. This indicates that the mechanical properties of the PGA copolymer can still be maintained even with the addition of a small amount of PEO segments.
[0062] Table 6. Tensile property tests of Example 5.6 and pure PGA
[0063] Sample Name Tensile strength (MPa) Elongation at break (%) PGA 108.5 12.7 Example 5 99.5 6.28 Example 6 107.2 8.36
[0064] [Example 12] Degradation behavior test of polyglycolic acid-based biodegradable materials
[0065] The two groups of polyglycolic acid-based biodegradable materials from Examples 5 and 6 were injection molded into several strips. Degradation performance tests were conducted according to the above-described test methods. The percentage of tensile strength to initial strength obtained from the tests represents the material's degradation change over time. Figure 3 As shown.
[0066] Depend on Figure 3 As can be seen, the degradation rate is significantly faster after the addition of PEO segments. By the second day, the strength had dropped to less than 50% of the initial strength, indicating that polyglycolic acid-based biodegradable materials have a fast degradation rate.
[0067] [Comparative Example 1] Degradation performance test of PGA homopolymer
[0068] Corbion's PGA raw material was pressed into thin sheets on a hot plate, and the water contact angle was tested using a German KRUSS-DSA100 contact angle meter to analyze the hydrophilicity of the samples. The obtained contact angle of PGA was 68.1°. Figure 1 As shown, pure PGA has poor hydrophilicity, and its water contact angle is significantly improved compared to that of PEO-added PGA.
[0069] Corbion's PGA raw material was injection molded into several specimens, and degradation performance tests were conducted according to the above-mentioned test method. The percentage of tensile strength to initial strength obtained from the test is the material's degradation change over time. Figure 2 As shown, after three days in water, the tensile strength of PGA remained above 90%, without significant decrease, indicating a low degradation rate. Only after the fourth day did its tensile strength show a significant decline.
[0070] [Comparative Examples 2-5] Performance Testing of PGA Blends
[0071] The PGA polymer was first dried in a vacuum oven at 60℃ for 5 hours to remove moisture, and then added to the PEO polymer in a mixer for 10 minutes. Granulation was performed using a Eurolab 16 co-rotating twin-screw extruder (screw diameter 16 mm, L / D ratio L / D = 40) manufactured by Thermo Fisher Scientific. This extruder has 11 sections from the feed port to the die, numbered 1-11. Section 1 only serves as the feed port and does not provide heating. The temperatures of each section of the extruder are shown in Table 8. The extrusion reaction time was approximately 3 minutes, and the screw speed was set at 100 rpm, labeled as comparative examples 2, 3, 4, and 5.
[0072] Table 7. Raw materials and proportions for Comparative Examples 2–5
[0073] Sample Name <![CDATA[M V (PEO)]]> PEO feed percentage (%) Comparative Example 2 100000 1 Comparative Example 3 100000 2 Comparative Example 4 200000 1 Comparative Example 5 200000 2
[0074] Table 8. Temperatures of each heating section in the reactive extruder of Comparative Examples 2–5
[0075]
[0076] The contact angles of the products obtained in Examples 2-5 were tested, and the results are as follows. Figure 4 As shown, Figure 4 The results show that the products obtained by blending in Comparative Examples 2-5 have higher water contact angles than the materials obtained by polymerization (Examples 4-7), indicating that the modification effect of blending is significantly different from the hydrophilic modification effect of polymerization.
Claims
1. A polyglycolic acid-based biodegradable material, obtained by reacting raw materials comprising the following components, in parts by weight: (1) 92-99 parts of glycolic acid or its derivatives, wherein the glycolic acid or its derivatives are selected from at least one of glycolic acid, glycolide, methyl glycolate, and glycolic anhydride; (2) 1-8 parts of polyethylene oxide polymer; the components comprising glycolic acid or its derivatives and polyethylene oxide polymer are mixed and melt-extruded to obtain the polyglycolic acid-based biodegradable material, wherein a metal compound catalyst is also added to the components, wherein the metal compound catalyst is selected from at least one of group IIA-VA metal salts and transition metal salts, and the viscosity-average molecular weight of the polyethylene oxide polymer is 20,000-300,000 g / mol; the water contact angle of the biodegradable material is below 50°, the number-average molecular weight of the biodegradable material is 80,000-200,000 g / mol, and the structural formula of the biodegradable material comprises PEO- b -PGA, PGA- b -PEO- b - At least one of the PGAs.
2. The biodegradable material according to claim 1, characterized in that, The biodegradable material has one or two melting points.
3. The biodegradable material according to claim 2, characterized in that, The number-average molecular weight of the biodegradable material is 90,000 to 150,000 g / mol.
4. The biodegradable material according to claim 3, characterized in that, The glycolic acid or its derivatives are selected from glycolide; and / or, The viscosity-average molecular weight of the poly(ethylene oxide) polymer is 50,000 to 200,000 g / mol.
5. The biodegradable material according to claim 1, characterized in that, The biodegradable material also contains 0.01 to 0.1 parts by weight of other additives.
6. The biodegradable material according to claim 5, characterized in that, The biodegradable material also contains 0.02 to 0.08 parts by weight of other additives.
7. The biodegradable material according to claim 5, characterized in that, The other additives are selected from at least one of antioxidants, metal passivators, compatibilizers, plasticizers, and anti-hydrolysis agents.
8. A method for preparing a polyglycolic acid-based biodegradable material according to any one of claims 1 to 7, comprising: The polyglycolic acid-based biodegradable material is obtained by mixing and melting and extruding components including glycolic acid or its derivatives and polyethylene oxide polymer.
9. The preparation method according to claim 8, characterized in that, The melt extrusion is performed using a twin-screw extruder.
10. The preparation method according to claim 8, characterized in that, Other additives are also added to the components.
11. The preparation method according to claim 10, characterized in that, The metal compound catalyst is 0.01 to 0.5 parts by weight.
12. The preparation method according to claim 11, characterized in that, The metal compound catalyst is selected from at least one of stannous octoate, stannous chloride, aluminum isopropoxide, bismuth acetate, n-butyl titanate, and tetrabutyl stannate; and / or, The metal compound catalyst is 0.03 to 0.3 parts by weight.
13. The preparation method according to claim 12, characterized in that, The metal compound catalyst is selected from stannous chloride.
14. The preparation method according to claim 8, characterized in that, The conditions for the extrusion reaction are: The extrusion reaction temperature is 150~250℃; and / or, The extrusion reaction time is 3-20 min; and / or, The extruder speed is 5~150 rpm.
15. The preparation method according to claim 14, characterized in that, The conditions for the extrusion reaction are: The extrusion reaction temperature is 160~230℃; and / or, The extrusion reaction time is 5-10 min; and / or, The extruder operates at a speed of 20-80 rpm.
16. A polyglycolic acid-based biodegradable material prepared by the preparation method according to any one of claims 8 to 15, characterized in that, The particle size of the polyglycolic acid-based biodegradable material is 0.1~4 mm.
17. The polyglycolic acid-based biodegradable material according to claim 16, characterized in that, The particle size of the polyglycolic acid-based biodegradable material is 0.2~3.5 mm.
18. A polyglycolic acid-based biodegradable material according to any one of claims 1 to 7 or the polyglycolic acid-based biodegradable material according to claim 16 or 17, used as a cryogenic well plugging material.
Citation Information
Patent Citations
Rubber member for downhole tools, downhole tool, and method for recovering hydrocarbon resource
CN105189636A
Hydrocarbon resource recovery drilling tool and hydrocarbon resource recovery method
CN106761546A
Shaped material for downhole tool member, downhole tool member, and downhole tool
CN108368572A
Degradable material suitable for underground reservoir fracturing operation and preparation method thereof
CN111995996A
Polyglycolic acid biodegradable block copolyester and copolyester film thereof as well as preparation methods and applications of polyglycolic acid biodegradable block copolyester and copolyester film
CN116003760A