A method for preparing Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material
By introducing sheet-like Al₂O₃-loaded graphene at the interface between carbon fiber and resin matrix, the problem of low interfacial strength between carbon fiber and resin matrix is solved, achieving high bending performance and low-cost production of carbon fiber/epoxy resin composites.
Patent Information
- Application Number
- CN202311531359.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-16
AI Technical Summary
The low interfacial strength, poor wettability, and insufficient adhesion between carbon fiber and resin matrix make carbon fiber composites prone to debonding under external forces, thus limiting their practical applications.
By introducing sheet-like Al₂O₃-loaded graphene at the interface between carbon fiber and resin matrix, and by optimizing the material composition and preparation process, Al₂O₃/graphene synergistic modification carbon fiber/epoxy resin composite material was prepared to improve the interfacial bonding strength.
It significantly improves the flexural properties of carbon fiber/epoxy resin composites, reduces production costs, and achieves high-efficiency interfacial bonding and dispersion.
Smart Images

Figure CN117327372B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of composite material science and technology, and specifically relates to a method for preparing Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material. Background Technology
[0002] Carbon fiber composites mainly consist of structural materials made by combining carbon fibers with matrices such as resins, metals, and ceramics. Among these, carbon fiber resin composites boast superior comprehensive indicators such as specific strength and specific modulus. With the advancement of lightweight technology research, carbon fiber resin-based composites have been widely used in aerospace, automotive, and leisure and entertainment industries. However, in practical applications, the carbon fiber and resin matrix still suffer from drawbacks such as low interfacial strength, poor wettability, and insufficient adhesion. These drawbacks make them prone to debonding under external forces, preventing carbon fiber composites from fully realizing their material advantages and severely limiting their practical applications.
[0003] Currently, to address the weak interfacial bonding between carbon fiber and resin, researchers have proposed a novel material structure design concept—multi-scale reinforcement. This involves introducing nanomaterials into composite materials, allowing them to act as "bridges" between the fibers and the resin matrix, serving as a "link" for transferring external loads from the resin matrix to the fibers, thereby improving the interfacial bonding strength of the composite. Surface modification of carbon fibers is currently the main method for multi-scale reinforcement of the interfacial strength of carbon fiber-resin composites and is a research hotspot both domestically and internationally. Commonly used nanomaterials for carbon fiber surface modification are mainly metal oxide nanoparticles (such as Al2O3, CuO, TiO2, etc.). These nanoparticles form bridges between the carbon fiber and the resin matrix, thus improving their interfacial adhesion. However, due to the high surface energy of metal nanoparticles, they are prone to aggregation. Conventional processing methods often fail to produce well-dispersed composites, and the resulting nanoagglomerates are large in size and have a loose and unstable structure, which can negatively impact the performance of the composite fibers. Graphene is a single-layer carbon nanomaterial with a rough, wrinkled, corrugated structure. Its unique two-dimensional honeycomb structure can increase the spatial scale effect of nanoparticles, effectively suppressing nanoparticle aggregation and enabling interlocking between the fiber and the matrix structure (i.e., mechanical interlocking theory), thereby obtaining high-performance composite materials. For example, Wang C et al. (Wang C, Zhao M, Li J, et al. Silver nanoparticles / graphene oxide-decorated carbon fiber synergistic reinforcement in epoxy-based composites[J]. Polymer, 2017, 131: 263-271.) found that when Ag and graphene are introduced simultaneously into the carbon fiber / resin interface, the unique two-dimensional honeycomb structure of graphene effectively suppresses the aggregation of Ag nanoparticles. Li H et al. (Li H, Wang S, Feng M, et al. Self-assembly and performances of wrinkled rGO@carbon fiber with embedded SnO2 nanoparticles as anode materials for structural lithium-ion battery[J]. Journal of Materials Science, 2018, 53, 11607-11619.) also pointed out that simultaneously introducing graphene and SnO2 into carbon fibers can significantly improve the dispersibility of SnO2. Therefore, simultaneously introducing metal nanoparticles and graphene multi-scale reinforcements at the interface between carbon fibers and the resin matrix can ensure high dispersion of nanoparticles while enabling the material to exhibit superior reinforcement and toughening effects.Carbon fiber / epoxy resin composites are widely used composite materials, and their comprehensive performance must be considered under the premise of readily available raw materials, low cost, and easy large-scale production. Therefore, Al2O3 / graphene is an ideal interface modification material. However, the method of using Al2O3 / graphene for synergistic modification of carbon fiber / epoxy resin composites is still in its early stages. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite materials, solving the problems of low interfacial strength, poor wettability, and insufficient adhesion between carbon fibers and the resin matrix. This method optimizes the material composition and preparation process, enabling low-cost production of strong and tough carbon fiber / epoxy resin composite materials, and significantly improving the bending performance of the material.
[0005] To achieve the above objectives, the technical solution provided by the present invention is as follows:
[0006] A method for preparing Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material includes the following steps:
[0007] Preparation of Al2O3 / graphene dispersion: Graphene powder was fully dispersed in deionized water to obtain a graphene dispersion. Sodium dodecyl sulfonate and flake Al2O3 were then added sequentially and fully dispersed to obtain a mixture containing flake Al2O3 and graphene. The mixture was placed in a reactor and reacted at 180°C for 10 hours. The product was washed with deionized water by centrifugation and dried to obtain boehmite-supported graphene powder. Then, the obtained powder was calcined in a tube furnace under an argon atmosphere to obtain graphene composite powder supported on flake Al2O3. This powder was then fully dispersed in anhydrous ethanol to obtain an Al2O3 / graphene dispersion. The mass ratio of sodium dodecyl sulfonate to flake Al2O3 was 1:1, and the mass ratio of flake Al2O3 to graphene was (0.5–10):1.
[0008] S2. Surface modification of carbon fiber: After removing the sizing from the carbon fiber bundle, it is completely immersed in the Al2O3 / graphene dispersion with a mass ratio of (0.5~10):1 described in S1 and fully dispersed so that the Al2O3 / graphene powder is uniformly attached to the fiber surface. Then it is placed in an oven to dry, and Al2O3 / graphene modified carbon fiber bundle is obtained.
[0009] S3. Preparation of the composite material: Epoxy resin, curing agent, and accelerator are stirred evenly according to a certain mass ratio and air bubbles are removed to obtain a resin mixture. This mixture is then uniformly coated onto the surface of the Al2O3 / graphene modified carbon fiber tow from S2. The mixture is then vacuum impregnated at 50°C for 45–60 min to obtain a modified carbon fiber prepreg. The prepreg is placed in a metal mold, and a molding pressure of 20 MPa is set on a tablet press. After holding the pressure for 20 min, the metal mold is fixed with G-clamps and cured under certain conditions to obtain the Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material.
[0010] Preferred method for preparing sheet-like Al2O3 in S1: 10g of aluminum isopropoxide is added to a flask containing 40mL of anhydrous isopropanol. After stirring in a water bath until completely dissolved, a hydrolysate (a mixture of 2.6mL water and 20mL anhydrous isopropanol) is slowly added dropwise over a period of 30-40 minutes. After complete addition, the mixture is heated to 80℃ and refluxed for 6 hours to completely hydrolyze the aluminum isopropoxide. The hydrolysate is then washed clean with anhydrous ethanol by centrifugation, dried, and the initial product, pseudoboehmite, is obtained. This product is then calcined in a muffle furnace at 600℃ for 4 hours. After complete dehydration, sheet-like Al2O3 is obtained.
[0011] Preferably, the dispersion method in S1 and S2 is ultrasonic dispersion, and the dispersion time is 10 to 30 minutes; the drying method is drying in an oven at 80°C for 5 hours.
[0012] Preferably, the calcination method in S1 is to hold at 500℃ for 2 hours, with a heating rate of 5℃ / min.
[0013] Preferably, the carbon fiber surface desizing treatment step in S2 is as follows: the untreated carbon fiber bundle is completely immersed in acetone solution for 72 hours, and ultrasonically cleaned for 15 minutes every 6 hours during this period. After soaking, the fiber is taken out and ultrasonically cleaned in anhydrous ethanol for 30 minutes, and then dried at 80°C for 5 hours to obtain desizing carbon fiber bundle.
[0014] Preferably, in S3, the epoxy resin is E51 type epoxy resin, the curing agent is methyltetrahydrophthalic anhydride, and the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol, with a mass ratio of 10:7:0.1.
[0015] Preferably, in S3, the stirring method is magnetic stirring in a 30℃ water bath for 10-30 minutes; the degassing method is ultrasonic removal for 30-60 minutes.
[0016] Preferably, the metal mold size in S3 is 80mm*15mm*2mm.
[0017] Preferably, the curing conditions in S3 are 90℃ for 1 hour, 130℃ for 2 hours, and 150℃ for 2 hours.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] This invention differs from traditional methods of toughening carbon fiber / epoxy resin composites with metal nanoparticles. By introducing sheet-like Al2O3-loaded graphene at the interface between carbon fiber and resin matrix, the agglomeration phenomenon during the modification of single metal oxide nanoparticles can be effectively improved. Furthermore, since alumina is inexpensive, using Al2O3 / graphene composite powder as an interface modifier can not only effectively reduce production costs but also enable carbon fiber / epoxy resin composites to exhibit superior bending performance. Attached Figure Description
[0020] Figure 1 This is a scanning electron microscope image of the Al2O3 / graphene composite powder obtained in Example 6 of this invention.
[0021] Figure 2 This is the XRD pattern of the Al2O3 / graphene composite powder obtained in Example 6 of this invention.
[0022] Figure 3 This is a macroscopic morphology image of the sample from Example 6 of this invention after a three-point bending experiment.
[0023] Figure 4 This is a scanning electron microscope image of the sample from Example 6 of this invention after a three-point bending experiment.
[0024] Figure 5 These are bending performance data graphs of the samples from Examples 1 to 8 of this invention. Detailed Implementation
[0025] The present invention will now be described in detail through specific embodiments. The scope of the present invention is not limited to these specific embodiments.
[0026] Example 1:
[0027] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 0.5:1, comprising the following steps:
[0028] S1、(1) Preparation of flake Al2O3: 10g of aluminum isopropoxide was added to a flask containing 40mL of anhydrous isopropanol. After the mixture was completely dissolved by stirring in a water bath at room temperature, the hydrolysate (a mixture of 2.6mL of water and 20mL of anhydrous isopropanol) was slowly added dropwise over a period of 40min. After the addition was complete, the mixture was heated to 80℃ and refluxed for 6h to completely hydrolyze the aluminum isopropoxide. The hydrolysate was washed clean by centrifugation with anhydrous ethanol and dried at 90℃ for 12h to obtain the initial product, boehmite. The product was then calcined in a muffle furnace at 600℃ for 4h. After the product was completely dehydrated, flake Al2O3 was obtained.
[0029] (2) Preparation of Al2O3 / graphene dispersion: 50 mg of graphene powder was ultrasonically dispersed in 50 mL of deionized water for 10 min to obtain a graphene dispersion. Then, 25 mg of sodium dodecyl sulfonate and 25 mg of the sheet-like Al2O3 obtained in step (1) were added sequentially and ultrasonically dispersed for 30 min to obtain a mixture containing sheet-like Al2O3 and graphene. The mixture was placed in a reactor and reacted at 180 °C for 10 h. The product was washed three times by centrifugation with deionized water and dried at 80 °C for 5 h to obtain boehmite-supported graphene powder. Then, the obtained powder was calcined in a tube furnace at 500 °C for 2 h under an argon atmosphere (heating rate of 5 °C / min) to obtain a sheet-like Al2O3-supported graphene composite powder with a mass ratio of 0.5:1. The powder was ultrasonically dispersed in anhydrous ethanol for 15 min to obtain an Al2O3 / graphene dispersion with a mass ratio of 0.5:1.
[0030] S2. Surface modification of carbon fibers: Untreated carbon fiber bundles were completely immersed in acetone solution for 72 hours, with ultrasonication for 15 minutes every 6 hours. After immersion, the fibers were removed and ultrasonically cleaned in anhydrous ethanol for 30 minutes, then dried at 80°C for 5 hours to obtain desized carbon fiber bundles. The desized carbon fiber bundles were completely immersed in the Al2O3 / graphene dispersion described in S1 and ultrasonically dispersed for 30 minutes to ensure that the Al2O3 / graphene powder was uniformly attached to the fiber surface. Subsequently, they were dried in an oven at 80°C for 5 hours to obtain Al2O3 / graphene modified carbon fiber bundles with a mass ratio of 0.5:1.
[0031] S3. Preparation of the composite material: 15g of E51 type epoxy resin, 10.5g of methyltetrahydrophthalic anhydride, and 0.015g of 2,4,6-tris(dimethylaminomethyl)phenol were mixed in a plastic beaker. After stirring in a water bath at 30℃ for 30min, the mixture was sonicated for 45min to remove air bubbles, resulting in a resin mixture. This mixture was then uniformly coated onto the surface of the Al2O3 / graphene modified carbon fiber tow described in S2. The mixture was then vacuum impregnated at 50℃ for 50min to obtain a modified carbon fiber prepreg. The prepreg was placed in a metal mold with dimensions of 80mm*15mm*2mm, and the molding pressure was set to 20MPa on a tablet press and held for 20min. Subsequently, the mold was fixed with G-clamps, and the mixture was cured at 90℃ for 1h, 130℃ for 2h, and 150℃ for 2h to obtain an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 0.5:1. To reduce experimental error, at least three parallel samples were prepared for each group for subsequent bending performance testing, and the results were averaged. The average bending strength of the modified carbon fiber / epoxy resin composite material obtained in this example was 595.7 MPa.
[0032] Example 2:
[0033] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 1:1. The difference from Example 1 is that in step S1(2), the amounts of sodium dodecyl sulfonate and flake Al2O3 are both changed to 50 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 644.51 MPa.
[0034] Example 3:
[0035] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 1.5:1. The difference from Example 1 is that in step S1(2), the amount of sodium dodecyl sulfonate and flake Al2O3 is changed to 75 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 658.72 MPa.
[0036] Example 4:
[0037] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 2:1. The difference from Example 1 is that in step S1(2), the amount of sodium dodecyl sulfonate and flake Al2O3 is changed to 100 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 774.29 MPa.
[0038] Example 5:
[0039] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 3:1. The difference from Example 1 is that in step S1(2), the amount of sodium dodecyl sulfonate and flake Al2O3 is changed to 150 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 805.32 MPa.
[0040] Example 6:
[0041] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 6:1. The difference from Example 1 is that in step S1(2), the amounts of sodium dodecyl sulfonate and flake Al2O3 are both changed to 300 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 854.32 MPa.
[0042] Example 7:
[0043] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 8:1. The difference from Example 1 is that in step S1(2), the amount of sodium dodecyl sulfonate and flake Al2O3 is changed to 400 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 657.89 MPa.
[0044] Example 8:
[0045] This embodiment provides a method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material with a mass ratio of 10:1. The difference from Example 1 is that in step S1(2), the amounts of sodium dodecyl sulfonate and flake Al2O3 are both changed to 500 mg. The average flexural strength of the modified carbon fiber / epoxy resin composite material obtained in this embodiment is 533.07 MPa.
[0046] Test conditions
[0047] Mechanical property testing: The bending properties of Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite materials were measured on a ZWC Z100 universal testing machine in Germany, according to the GB / T 1449-2005 test standard.
[0048] The samples from Examples 1 to 8 of the present invention all have good bending properties.
[0049] Figure 1 This is a scanning electron microscope (SEM) image of the Al2O3 / graphene composite powder obtained in Example 6 of this invention. From... Figure 1It can be seen that the sheet-like Al2O3 adheres to the surface of graphene, and its unique sheet-like structure increases the surface roughness, which greatly promotes the formation of the three-dimensional structure inside the material. The interfacial bonding force also increases, thereby enhancing the mechanical properties of the composite material.
[0050] Figure 2 This is the XRD pattern of the Al2O3 / graphene composite powder obtained in Example 6 of this invention. From... Figure 2 It can be seen that relatively sharp diffraction peaks appear at 26.38° and 54.54°. By comparing with the standard card JCPDS#41-1487, it can be known that these peaks originate from the (002) and (004) crystal planes of the graphene crystal structure. When Al2O3 is loaded on the graphene surface, a series of new diffraction peaks appear at 31.97°, 37.68°, 39.42°, 45.84° and 66.84°. By comparing with the standard card JCPDS#79-1558, it can be seen that the above diffraction peaks correspond to the (220), (311), (222), (400) and (440) crystal planes of γ-Al2O3, respectively, indicating that the present invention has successfully prepared Al2O3 / graphene composite powder.
[0051] Figure 3 This is a macroscopic morphology image of the sample from Example 6 of this invention after a three-point bending experiment. From... Figure 3 It can be seen that the composite material did not completely break after the bending test, indicating that the carbon fiber plays a full role as a stress-bearing body, proving that the present invention can achieve the purpose of toughening and modifying carbon fiber epoxy resin composite materials.
[0052] Figure 4 This is a scanning electron microscope (SEM) image of the sample from Example 6 of this invention after a three-point bending experiment. From... Figure 4 It can be seen that the fracture surface is relatively smooth after bending and breaking, indicating good interfacial bonding. In addition, there are many serrated fracture surfaces at the fracture point of the carbon fiber, which indicates that more fracture energy is required when the sample breaks, so that the high strength of the carbon fiber is fully utilized, thereby improving the bending performance of the Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material.
[0053] Figure 5 The graph shows the bending performance data for Examples 1-8. From... Figure 5It can be seen that the flexural strength of the Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material exhibits a trend of first increasing and then decreasing as the Al2O3 / graphene synergistic modification ratio increases. The sample exhibits the lowest flexural strength (595.7 MPa) when the Al2O3 / graphene ratio is 0.5:1. In contrast, the sample in Example 6 exhibits the highest flexural strength (854.32 MPa) when the Al2O3 / graphene ratio is 6:1, representing a 43.41% improvement over the composite material prepared with the lowest Al2O3 / graphene ratio of 0.5:1. When the Al2O3 / graphene ratio is too high (as in Example 8), the flexural strength is lower than that of Example 1 (533.07 MPa).
[0054] Therefore, a higher Al2O3 / graphene ratio is not necessarily better. This is because when the Al2O3 / graphene ratio is too high, the excessively high surface energy of Al2O3 causes it to agglomerate on the graphene, reducing the interfacial bonding between the fiber and the resin matrix. This prevents the fiber from efficiently bearing stress, ultimately leading to a significant decrease in the flexural properties of the Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite. Therefore, only an appropriate Al2O3 / graphene ratio can effectively improve the interfacial bonding between carbon fiber and epoxy resin, enabling structural interlocking between the fiber and the resin matrix—that is, achieving the mechanical interlocking theory—and ultimately improving the flexural properties of the composite.
[0055] The embodiments described above are merely illustrative of the principles of the present invention and are not intended to limit the invention. Any improvements, modifications, and equivalent substitutions made in accordance with the present invention are protected by the present invention.
Claims
1. A method for preparing Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material, characterized in that, Includes the following steps: S1. Preparation of Al2O3 / graphene dispersion: Graphene powder was fully dispersed in deionized water to obtain a graphene dispersion. Sodium dodecyl sulfonate and flake Al2O3 were then added sequentially and fully dispersed to obtain a mixture containing flake Al2O3 and graphene. The mixture was placed in a reactor and reacted at 180 °C for 10 h. The product was washed by centrifugation with deionized water and dried to obtain boehmite-supported graphene powder. The obtained powder was calcined in a tube furnace under an argon atmosphere to obtain graphene composite powder supported by flake Al2O3. The powder was then fully dispersed in anhydrous ethanol to obtain an Al2O3 / graphene dispersion. The mass ratio of sodium dodecyl sulfonate to flake Al2O3 was 1:1, and the mass ratio of flake Al2O3 to graphene was (0.5~10):
1. S2. Surface modification of carbon fiber: After removing the sizing from the carbon fiber bundle, it is completely immersed in the Al2O3 / graphene dispersion with a mass ratio of (0.5~10):1 described in S1 and fully dispersed so that the Al2O3 / graphene powder is uniformly attached to the fiber surface. Then it is placed in an oven to dry, and Al2O3 / graphene modified carbon fiber bundle is obtained. S3. Preparation of composite material: Epoxy resin, curing agent and accelerator are stirred evenly according to a certain mass ratio and the air bubbles are removed to obtain a resin mixture. The mixture is evenly coated on the surface of the Al2O3 / graphene modified carbon fiber tow in S2. Vacuum impregnation is carried out at 50 ℃ for 45~60 min to obtain modified carbon fiber prepreg. The prepreg is placed in a metal mold and the molding pressure is set to 20 MPa on a tablet press. After holding the pressure for 20 min, the metal mold is fixed with G-type clamps and cured under certain conditions to obtain Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material.
2. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The preparation method of the sheet-like Al2O3 in S1 is as follows: 10 g of aluminum isopropoxide is added to a flask containing 40 mL of anhydrous isopropanol. After stirring in a water bath until completely dissolved, a hydrolysate obtained by mixing 2.6 mL of water and 20 mL of anhydrous isopropanol is slowly added dropwise over a time of 30-40 min. After the addition is complete, the temperature is raised to 80 °C and refluxed for 6 h to completely hydrolyze the aluminum isopropoxide. The hydrolysate is then washed clean with anhydrous ethanol by centrifugation, dried, and the initial product, pseudoboehmite, is obtained. The product is then calcined in a muffle furnace at 600 °C for 4 h. After complete dehydration, sheet-like Al2O3 is obtained.
3. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The dispersion method in S1 and S2 is ultrasonic dispersion, and the dispersion time is 10~30 min; the drying method is drying in an oven at 80 ℃ for 5 h.
4. The preparation method of Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The calcination method in S1 is to hold at 500 ℃ for 2 h with a heating rate of 5 ℃ / min.
5. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The carbon fiber surface desizing treatment step in S2 is as follows: the untreated carbon fiber bundle is completely immersed in acetone solution for 72 h, and ultrasonically cleaned for 15 min every 6 h during the soaking period. After the soaking is completed, the fiber is taken out and ultrasonically cleaned in anhydrous ethanol for 30 min, and then dried at 80 ℃ for 5 h to obtain desizing carbon fiber bundle.
6. The preparation method of Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The epoxy resin in S3 is E51 type epoxy resin, the curing agent is methyltetrahydrophthalic anhydride, and the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol, with a mass ratio of 10:7:0.
1.
7. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The stirring method in S3 is magnetic stirring in a 30℃ water bath for 10~30 min; the degassing method is ultrasonic removal for 30~60 min.
8. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The dimensions of the metal mold in S3 are 80 mm × 15 mm × 2 mm.
9. The method for preparing an Al2O3 / graphene synergistic modified carbon fiber / epoxy resin composite material according to claim 1, characterized in that, The curing conditions in S3 are: 90 ℃ for 1 h, 130 ℃ for 2 h, and 150 ℃ for 2 h.
Citation Information
Patent Citations
Preparation method of modified carbon fiber toughened silicon carbide ceramic material and modified carbon fiber toughened silicon carbide ceramic material
CN113698221A
Carbon fiber and graphene compounded high-strength porous material, and gas diffusion layer and preparation method therefor
WO2023024770A1