A negative electrode sheet, a method for manufacturing the same, and use thereof
By using silicon nanowires in combination with conductive agents and binders in the negative electrode sheet of lithium-ion batteries, the volume expansion problem of silicon materials during charging and discharging is solved, and a high-performance and high-safety negative electrode sheet for lithium-ion batteries is achieved.
Patent Information
- Application Number
- CN202210718975.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The existing silicon anode material for lithium-ion batteries exhibits large volume changes during charge and discharge, resulting in poor cycle performance and safety performance, making it difficult to meet the requirements of high specific energy and high power density lithium-ion batteries.
Silicon nanowires are used as the active material. By controlling the amount added to 60-85 wt%, and mixing them with a first conductive agent, a binder, a second conductive agent and a thickener, a conductive network is formed to suppress the volume expansion of silicon during the lithium insertion/extraction process.
It improves the rate charge/discharge performance, cycle performance and safety performance of lithium-ion batteries, with an initial discharge specific capacity of over 3200 mAh/g and a capacity retention rate of over 85% after 100 cycles. The manufacturing process is simple and inexpensive.
Smart Images

Figure CN117334840B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery manufacturing technology, and particularly relates to a negative electrode sheet, its preparation method and application. Background Technology
[0002] Lithium-ion batteries have been widely used in portable electronic products and electric vehicles due to their excellent cost, manufacturing process, and cycle stability. Currently, commercially available lithium-ion batteries mainly use graphite-based anode materials with a specific capacity of 372 mAh / g. However, existing technology has approached its theoretical value, limiting the potential for further development of graphite-based anode materials. This cannot meet the miniaturization needs of portable electronic devices and the widespread demand for high-energy-density and high-power-density lithium-ion batteries in electric vehicles.
[0003] Silicon has a theoretical specific capacity of 4200 mAh / g, more than ten times that of graphite, and its resources are abundant, making it an ideal candidate material for developing next-generation high-energy-density and high-power-density lithium-ion battery anode materials. However, silicon undergoes a volume change of up to 400% during battery charge-discharge cycles, resulting in poor initial efficiency and cycle performance.
[0004] CN105609749A discloses a silicon nanowire and its application, employing a chemical etching process using an etchant. The etchant preferentially etches from the multiphase silicon alloy relative to the silicon phase, removing other phases to obtain silicon nanowires. A lithium-ion battery anode was obtained by mixing silicon nanowires, Super-P carbon black conductive agent, and PVDF binder in a mass ratio of 8:1:1, preparing a slurry using N-methylpyrrolidone as a solvent, and baking at 120°C for 12 hours. However, its initial discharge capacity was only 2510 mAh / g, and after 50 cycles, the maximum capacity retention was only 50%, failing to effectively alleviate the volume expansion of silicon during lithium insertion / extraction.
[0005] CN103000865A discloses a method for preparing carbon fiber-silicon nanowire anode material, the method comprising: (1) preparation of silicon nanowire anode material: firstly, a 5-10 nm thick gold film is vacuum-deposited on the surface of a silicon wafer; after purging an argon / hydrogen mixture into a tube furnace, the silicon wafer after gold film deposition is placed in the tube furnace, the tube furnace is heated to 700-800℃ and kept at that temperature for 3-4 hours, then cooled to 450-550℃, silane gas is introduced, the deposition time is 1.5-2.5 hours, and the furnace is cooled to room temperature to obtain a layer of silicon nanowires; (2) preparation of carbon fiber-silicon nanowire composite material by ball milling: the silicon nanowires obtained in step (1) are mixed with carbon nanofibers at a molar ratio of 1:1, and then mixed with polyurethane balls in a three-dimensional mixing tank to obtain carbon fiber-silicon nanowire composite material. Although the negative electrode material prepared by this method can retain about 80% of its capacity after 50 cycles, its initial discharge capacity is only 1700 mAh / g, and the preparation process is complex.
[0006] CN114388748A discloses a silicon-carbon anode slurry and its preparation process. The slurry includes a silicon-carbon anode active material, a conductive agent, a binder, a thickener, and a solvent. The silicon-carbon anode active material is composed of a silicon-based anode and a graphite anode. The preparation process includes the preparation of a dot-like conductive slurry, a silicon-based conductive slurry, a primary anode slurry, and a silicon-carbon anode slurry. This preparation process involves first mixing the silicon-based anode and a linear conductive agent, allowing the linear conductive agent to uniformly coat the surface of the silicon-based anode. This coating effectively mitigates the volume expansion effect of the silicon-based anode. However, the initial capacity and cycle performance of the anode sheet prepared using this anode slurry are not described.
[0007] Therefore, effectively mitigating the volume expansion of silicon materials during cycling is crucial for simultaneously improving the rate charge / discharge performance, cycle performance, and safety performance of batteries. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a negative electrode sheet, its preparation method, and its applications. The negative electrode sheet obtained by the preparation method provided by the present invention can effectively suppress the volume expansion of silicon during the lithium insertion / extraction process, thereby enabling the battery to have excellent rate charge / discharge performance, cycle performance, and safety performance. At the same time, the preparation process of the negative electrode sheet is simple, low in cost, and environmentally friendly.
[0009] To achieve this objective, the present invention adopts the following technical solution:
[0010] In a first aspect, the present invention provides a method for preparing a negative electrode sheet, the method comprising:
[0011] After mixing silicon nanowires and a first solvent, a first conductive agent, a binder, a second conductive agent, and a thickener are added sequentially to obtain a negative electrode slurry. The negative electrode slurry is then coated onto the surface of a current collector to obtain the negative electrode sheet.
[0012] With a total mass fraction of 100 wt% for the solid raw materials in the negative electrode slurry, the amount of silicon nanowires added is 60-85 wt%, for example, it can be 60 wt%, 62 wt%, 64 wt%, 66 wt%, 68 wt%, 70 wt%, 72 wt%, 74 wt%, 76 wt%, 78 wt%, 80 wt%, 82 wt%, or 85 wt%, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0013] In this invention, silicon nanowires are first dispersed in a first solvent, and then a first conductive agent, an adhesive liquid, a second conductive agent, and a thickener are added sequentially. This is because the first conductive agent and silicon nanowires are uniformly mixed to form a conductive link network, ensuring good conductivity between silicon nanowires. The adhesive ensures stable bonding between silicon nanowires and the first conductive agent. The addition of the second conductive agent further enhances the conductivity of the electrode sheet, and the thickener maintains the slurry at a certain viscosity, making it easy to coat onto copper foil to prepare a negative electrode sheet.
[0014] Meanwhile, this invention limits the amount of silicon nanowires added to 60-85 wt%. When the amount of silicon nanowires added is less than 60 wt%, the capacity per unit weight of the electrode decreases due to the low content of silicon nanowires as the active material. When the amount of silicon nanowires added is greater than 85 wt%, the cycle performance of the silicon nanowire negative electrode decreases because the increased content of silicon nanowires reduces the content of conductive carbon and binders, resulting in decreased electrode conductivity and separation and cracking between silicon nanowires. This invention only requires silicon nanowires as the active material of the negative electrode, without the need to add carbon materials or other active materials, to simultaneously improve the battery's rate charge / discharge performance, cycle performance, and safety performance.
[0015] Furthermore, in this invention, the solid raw materials of the negative electrode slurry refer to raw materials in solid form. For example, when silicon nanowires, the first conductive agent, the binder, the second conductive agent, and the thickener are all involved in the preparation of the negative electrode slurry in solid form such as powder, the total mass of the solid raw materials refers to the total mass of silicon nanowires, the first conductive agent, the binder, the second conductive agent, and the thickener. When silicon nanowires, the first conductive agent, and the thickener are involved in the preparation of the negative electrode slurry in solid form, and the binder is prepared into a binder slurry, and the second conductive agent is prepared into a second conductive agent slurry, the total mass of the solid raw materials refers to the total mass of the binder in the silicon nanowires, the first conductive agent, the binder slurry, the second conductive agent in the second conductive agent slurry, and the thickener.
[0016] This invention uses silicon nanowires as the active material. By first dispersing the silicon nanowires and then sequentially adding a first conductive agent, a binder, a second conductive agent, and a thickener, along with controlling the amount of silicon nanowires added to the range of 60-85 wt%, the volume expansion of silicon during the lithium insertion / extraction process can be effectively suppressed. This simultaneously improves the battery's rate charge / discharge performance, cycle performance, and safety performance. Furthermore, the preparation process of the negative electrode is simple, low-cost, and environmentally friendly.
[0017] As a preferred embodiment of the present invention, the preparation process of the silicon nanowires includes:
[0018] Silicon vapor is obtained by evaporating a silicon source once, and aluminum vapor is obtained by evaporating an aluminum source a second time. The silicon vapor is then passed into the aluminum vapor to react and obtain the silicon nanowires.
[0019] This invention employs aluminum, which has a low melting point and reducing properties, as a growth controller and catalyst in the preparation of silicon nanowires. Silicon nanowires begin to grow upon contact with aluminum vapor, resulting in silicon nanowires with excellent structural cycle stability. This is because silicon vapor dissolves in the aluminum droplets (nanoscale) within the furnace, continuously precipitating silicon atoms to grow silicon nanowires. Under certain temperature conditions, this method ensures uniform silicon nanowire growth with few impurities. Furthermore, the silicon nanowire preparation method provided by this invention does not require high raw material purity, has controllable costs, and features simple and reliable processes, facilitating large-scale mass production.
[0020] When silicon nanowires obtained by the above method are used as active materials for negative electrode sheets, the excellent structural cycle stability of silicon nanowires can further improve the initial discharge specific capacity and cycle capacity retention of the battery.
[0021] Preferably, the purity of the silicon source is ≥95%, for example, it can be 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99%, 99.5%, 99.9%, etc., but it is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0022] Preferably, the silicon source includes any one or a combination of at least two of silicon powder, silicon ingot, silicon dioxide, or silicon suboxide.
[0023] Preferably, the temperature of the first evaporation is 1600-2000℃, for example, it can be 1600℃, 1650℃, 1700℃, 1750℃, 1800℃, 1850℃, 1900℃, 2000℃, etc., but it is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0024] As a preferred technical solution of the present invention, the aluminum source includes any one or a combination of at least two of aluminum plates, aluminum powder or aluminum wire.
[0025] Preferably, the surface of the aluminum source contains a coating.
[0026] Preferably, the material of the coating includes gold and / or silver.
[0027] Preferably, the temperature of the secondary evaporation is 500-800℃, for example, it can be 500℃, 520℃, 550℃, 580℃, 600℃, 630℃, 650℃, 670℃, 700℃, 730℃, 50℃, 780℃, 800℃, etc., but it is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0028] Preferably, the secondary evaporation is carried out in an argon atmosphere.
[0029] Preferably, the silicon vapor is introduced into the aluminum vapor at a rate of 2 to 5 g / min, for example, 2 g / min, 2.2 g / min, 2.4 g / min, 2.6 g / min, 2.8 g / min, 3 g / min, 3.2 g / min, 3.4 g / min, 3.6 g / min, 3.8 g / min, 4 g / min, 4.2 g / min, 4.4 g / min, 4.6 g / min, 4.8 g / min, 5 g / min, etc., but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0030] In this invention, the rate at which silicon vapor is introduced into aluminum vapor is limited to 2-5 g / min. If the rate is higher than 5 g / min, the silicon nanowires will be thicker and shorter in length; if the rate is lower than 2 g / min, the silicon nanowires will be thinner and shorter in length.
[0031] Preferably, the reaction temperature is 500–800°C, for example, 500°C, 520°C, 550°C, 580°C, 600°C, 630°C, 650°C, 670°C, 700°C, 730°C, 50°C, 780°C, 800°C, etc., but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0032] Preferably, the reaction time is 1 to 5 hours, for example, it can be 1 hour, 1.2 hours, 1.5 hours, 1.8 hours, 2 hours, 2.3 hours, 2.5 hours, 2.7 hours, 3 hours, 3.2 hours, 3.5 hours, 3.8 hours, 4 hours, 4.2 hours, 4.5 hours, 4.7 hours, 5 hours, etc., but it is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0033] Preferably, the silicon nanowire has a diameter of <200nm and a length of >100μm.
[0034] This invention regulates the speed at which silicon vapor is introduced into aluminum vapor, thereby controlling the size of silicon nanowires. When using silicon nanowires with a diameter <200nm and a length >100μm as the active material of the negative electrode, it helps to further improve the cycle stability, rate charge / discharge performance, and safety performance of the battery. This is because when the silicon wire diameter is <200nm, the silicon nanowires do not crack or shatter during the lithium insertion and extraction process, thus maintaining the integrity of the silicon wires. When the silicon wire length is >100μm, a better interconnection network can be formed between the silicon wires, which is beneficial to capacity utilization and improved cycle performance.
[0035] As a preferred embodiment of the present invention, the first solvent includes water and / or ethanol.
[0036] Preferably, the mixing time of the silicon nanowires and the first solvent is 10 to 60 minutes, for example, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0037] Preferably, the silicon nanowires and the first solvent are mixed under grinding conditions.
[0038] In this invention, silicon nanowires are placed in a mortar and a first solvent is added for grinding and mixing until homogeneous.
[0039] Preferably, the first conductive agent, the adhesive, the second conductive agent, and the thickener are added sequentially under stirring conditions.
[0040] In this invention, a first conductive agent, a binder, a second conductive agent, and a thickener are added sequentially to uniformly ground silicon nanowires while stirring.
[0041] Preferably, the stirring speed is 100 to 300 rpm, for example, it can be 100 rpm, 120 rpm, 150 rpm, 180 rpm, 200 rpm, 220 rpm, 250 rpm, 280 rpm or 300 rpm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0042] Preferably, after adding the first conductive agent, the binder, the second conductive agent and the thickener in sequence, stirring is continued for 30 to 120 minutes, for example, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes or 120 minutes, but not limited to the listed values, other unlisted values within this range are also applicable.
[0043] As a preferred embodiment of the present invention, the total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the first conductive agent added is 1 to 15 wt%, for example, it can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, or 15 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0044] Preferably, the total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the binder added is 5 to 20 wt%, for example, it can be 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, or 20 wt%, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0045] Preferably, the total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the second conductive agent added is 0.5 to 5 wt%, for example, it can be 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, or 5 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0046] Preferably, the total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the thickener added is 2 to 8 wt%, for example, it can be 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, or 8 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0047] In this invention, the preferred formulation of the negative electrode sheet includes: 60-85 wt% silicon nanowires, 1-15 wt% first conductive agent, 5-20 wt% binder, 0.5-5 wt% second conductive agent, and 2-8 wt% thickener. Using silicon nanowires, which exhibit excellent structural cycle stability, as the active material, and adjusting the content of each component in the negative electrode slurry to the above range, can better suppress the volume expansion of silicon during charging and discharging, further improving the cycle performance and rate charge / discharge performance of the battery. This is because the conductive agent and silicon nanowires form a conductive network, allowing the silicon nanowires to fully utilize their capacity. The binder ensures a strong bond between the silicon wires, conductive agent, and copper foil, while the thickener maintains stable slurry viscosity, facilitating the coating and preparation of the negative electrode sheet.
[0048] As a preferred embodiment of the present invention, the first conductive agent includes any one or a combination of at least two of conductive carbon black, acetylene black, carbon fiber, or conductive graphene.
[0049] Preferably, the adhesive is mixed with the second solvent to prepare an adhesive solution. After the silicon nanowires and the first solvent are mixed, the first conductive agent, the adhesive solution, the second conductive agent and the thickener are added in sequence to obtain the negative electrode slurry.
[0050] Preferably, the solid content of the adhesive liquid is 4 to 6 wt%, for example, it can be 4 wt%, 4.2 wt%, 4.4 wt%, 4.6 wt%, 5 wt%, 5.2 wt%, 5.4 wt%, 5.6 wt%, 5.8 wt%, or 6 wt%, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0051] Preferably, the adhesive comprises any one or a combination of at least two of styrene-butadiene rubber, polyethylene glycol, or polyvinyl acetate.
[0052] Preferably, the second solvent comprises water and / or ethanol.
[0053] Preferably, the second conductive agent is dispersed in a third solvent to form a second conductive agent slurry. After the silicon nanowires and the first solvent are mixed, the first conductive agent, the adhesive liquid, the second conductive agent slurry and the thickener are added in sequence to obtain the negative electrode slurry.
[0054] In this invention, the first conductive agent is used in the preparation of the negative electrode slurry in powder form, while the second conductive agent is used in the preparation of the negative electrode slurry in liquid form. This is because the second conductive agent is difficult to disperse, and pre-dispersion can make the slurry mix more evenly.
[0055] Preferably, the solid content of the second conductive agent slurry is 0.2 to 0.6 wt%, for example, it can be 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, or 0.6 wt%, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0056] Preferably, the second conductive agent comprises carbon nanotubes.
[0057] Preferably, the thickener comprises any one or a combination of at least two of sodium carboxymethyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, or polyvinylpyrrolidone.
[0058] Preferably, the viscosity of the negative electrode slurry is 1000 to 3000 cp, for example, it can be 1000 cp, 1200 cp, 1500 cp, 1800 cp, 2000 cp, 2200 cp, 2500 cp, 2800 cp or 3000 cp, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0059] Preferably, the solid content of the negative electrode slurry is 6 to 8 wt%, for example, it can be 6 wt%, 6.2 wt%, 6.4 wt%, 6.6 wt%, 6.8 wt%, 7 wt%, 7.2 wt%, 7.4 wt%, 7.6 wt%, 7.8 wt%, or 8 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0060] As a preferred embodiment of the present invention, the preparation method further includes:
[0061] The negative electrode slurry is coated onto the surface of the current collector and then dried to form a slurry coating on the surface of the current collector, thus obtaining the negative electrode sheet.
[0062] Preferably, the drying temperature is 70 to 90°C, for example, 70°C, 75°C, 80°C, 85°C or 90°C, but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0063] Preferably, the drying time is 60 to 240 minutes, for example, 60 minutes, 80 minutes, 100 minutes, 120 minutes, 140 minutes, 160 minutes, 180 minutes, 200 minutes, 220 minutes or 240 minutes, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0064] Preferably, the thickness of the slurry coating is 150 to 250 μm, for example, it can be 150 μm, 170 μm, 190 μm, 200 μm, 220 μm, 240 μm or 250 μm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0065] Preferably, after the slurry coating is formed on the surface of the current collector, the negative electrode sheet is obtained by rolling and cutting in sequence.
[0066] In a second aspect, the present invention provides a negative electrode sheet, the negative electrode sheet comprising a current collector and a slurry coating on the surface of the current collector, the negative electrode sheet being prepared by the preparation method described in the first aspect.
[0067] As a preferred embodiment of the present invention, the total mass of the slurry coating is 100 wt%, and the mass fraction of silicon nanowires in the slurry coating is 60-85 wt%, for example, it can be 60 wt%, 62 wt%, 64 wt%, 66 wt%, 68 wt%, 70 wt%, 72 wt%, 74 wt%, 76 wt%, 78 wt%, 80 wt%, 82 wt%, or 85 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0068] Preferably, the total mass of the slurry coating is 100 wt%, and the mass fraction of the first conductive agent in the slurry coating is 1 to 15 wt%, for example, it can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, or 15 wt%, but it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0069] Preferably, the total mass of the slurry coating is 100 wt%, and the mass fraction of the adhesive in the slurry coating is 5 to 20 wt%, for example, it can be 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, or 20 wt%, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0070] Preferably, the total mass of the slurry coating is 100 wt%, and the mass fraction of the second conductive agent in the slurry coating is 0.5 to 5 wt%, for example, it can be 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, or 5 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0071] Preferably, the total mass of the slurry coating is 100 wt%, and the mass fraction of the thickener in the slurry coating is 2 to 8 wt%, for example, it can be 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, or 8 wt%, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0072] Thirdly, the present invention provides a lithium-ion battery, the lithium-ion battery comprising the negative electrode sheet described in the second aspect of the claim.
[0073] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0074] (1) The negative electrode sheet obtained by the preparation method provided by the present invention can effectively suppress the volume expansion of silicon during the lithium insertion and extraction process, so that the battery can have excellent rate charge and discharge performance, cycle performance and safety performance. The initial discharge specific capacity is higher than 3200mAh / g, and after 100 charge and discharge cycles, the discharge specific capacity of the battery is still higher than 2750mAh / g, and the capacity retention rate is higher than 85%.
[0075] (2) The preparation process of the negative electrode sheet provided by the present invention is simple and reliable, low in cost, and compatible with existing mass production processes; in addition, the solvent used is non-toxic, the equipment does not require explosion-proof facilities, and it is environmentally friendly. Attached Figure Description
[0076] Figure 1 The following is a process flow diagram of the preparation process of the negative electrode sheet provided in Embodiments 1-6 of the present invention.
[0077] Figure 2 This is a scanning electron microscope image of the silicon nanowires provided in Embodiment 1 of the present invention, with a magnification of 20 kV.
[0078] Figure 3 The image shown is a scanning electron microscope image with a magnification of 20 kV of the silicon nanowires provided in Embodiment 1 of the present invention after 100 cycles of charge and discharge.
[0079] Figure 4 The diagram shows the cycle stability of a battery assembled using the negative electrode sheet provided in Embodiment 1 of the present invention. Detailed Implementation
[0080] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0081] Example 1
[0082] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0083] (1) 3 kg of 98% pure silicon dioxide was heated to 1800℃ for a first evaporation to obtain silicon dioxide vapor; an aluminum plate with a silver coating was heated to 700℃ and subjected to a second evaporation under an argon atmosphere to obtain aluminum vapor; subsequently, the silicon dioxide vapor was introduced into the aluminum vapor at a rate of 2 g / min, and the reaction was carried out at 750℃ for 3 h to obtain silicon nanowires, such as... Figure 2 As shown;
[0084] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 80 wt% for 40 min, conductive carbon black (SP) at a mass fraction of 7 wt%, styrene-butadiene rubber solution at a solid content of 5.6 wt% (the amount of styrene-butadiene rubber solution added is based on the mass fraction of styrene-butadiene rubber, and the mass fraction of styrene-butadiene rubber is 7 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, and the mass fraction of carbon nanotubes is 3 wt%), and sodium carboxymethyl cellulose at a mass fraction of 3 wt%, the mixture is stirred for another 80 min to obtain a negative electrode slurry with a solid content of 7 wt% and a viscosity of 2000 cp.
[0085] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 80℃ for 120min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0086] In this embodiment, the mass fractions of conductive carbon black, styrene-butadiene rubber, carbon nanotubes, and sodium carboxymethyl cellulose are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0087] Example 2
[0088] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0089] (1) 2 kg of 95% pure silicon powder was heated to 2000℃ for a first evaporation to obtain silicon vapor; an aluminum block with a gold coating on its surface was heated to 800℃ and evaporated a second time under an argon atmosphere to obtain aluminum vapor; then the silicon vapor was introduced into the aluminum vapor at a rate of 5 g / min and reacted at 800℃ for 1 h to obtain silicon nanowires.
[0090] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 60 wt% for 10 min, conductive carbon black (SP) at a mass fraction of 15 wt%, styrene-butadiene rubber solution at a solid content of 5.6 wt% (the amount of styrene-butadiene rubber solution added is based on the mass fraction of styrene-butadiene rubber, and the mass fraction of styrene-butadiene rubber is 15 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, and the mass fraction of carbon nanotubes is 5 wt%), and sodium carboxymethyl cellulose at a mass fraction of 5 wt%, the mixture is stirred for 30 min to obtain a negative electrode slurry with a solid content of 7 wt% and a viscosity of 3000 cp.
[0091] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 70℃ for 240min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0092] In this embodiment, the mass fractions of conductive carbon black, styrene-butadiene rubber, carbon nanotubes, and sodium carboxymethyl cellulose are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0093] Example 3
[0094] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0095] (1) 1 kg of 96% pure silicon powder and 2 kg of 96% pure silicon dioxide were heated to 1700℃ for a first evaporation to obtain silicon vapor; an aluminum plate with a silver coating on its surface was heated to 600℃ and evaporated under an argon atmosphere to obtain aluminum vapor; then the silicon vapor was introduced into the aluminum vapor at a rate of 3 g / min and reacted at 600℃ for 2 h to obtain silicon nanowires;
[0096] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 65 wt% for 20 min, acetylene black at a mass fraction of 12 wt%, styrene-butadiene rubber solution at a solid content of 5.6 wt% (the amount of styrene-butadiene rubber solution added is based on the mass fraction of styrene-butadiene rubber, which is 14 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, which is 4 wt%), and sodium carboxymethyl cellulose at a mass fraction of 5 wt% were added. Then, stirring was continued for 100 min to obtain a negative electrode slurry with a solid content of 6 wt% and a viscosity of 2000 cp.
[0097] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 90℃ for 60min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0098] In this embodiment, the mass fractions of acetylene black, styrene-butadiene rubber, carbon nanotubes, and sodium carboxymethyl cellulose are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0099] Example 4
[0100] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0101] (1) 2.1 kg of silicon block with a purity of 97.2% was heated to 1600℃ for a first evaporation to obtain silicon vapor; an aluminum plate with a gold coating on its surface was heated to 500℃ and evaporated under an argon atmosphere to obtain aluminum vapor; then the silicon vapor was introduced into the aluminum vapor at a rate of 3 g / min and reacted at 500℃ for 5 h to obtain silicon nanowires.
[0102] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 70 wt% for 60 min, conductive carbon black (SP) at a mass fraction of 10 wt%, polyethylene glycol adhesive at a solid content of 5.6 wt% (the amount of polyethylene glycol adhesive added is based on the mass fraction of polyethylene glycol, and the mass fraction of polyethylene glycol is 9 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, and the mass fraction of carbon nanotubes is 3 wt%), and sodium carboxymethyl cellulose at a mass fraction of 8 wt%, the mixture is stirred for 120 min to obtain a negative electrode slurry with a solid content of 8 wt% and a viscosity of 1000 cp.
[0103] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 80℃ for 120min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0104] In this embodiment, the mass fractions of conductive carbon black, polyethylene glycol, carbon nanotubes, and sodium carboxymethyl cellulose are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0105] Example 5
[0106] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0107] (1) 1.5 kg of silicon powder with a purity of 98.1% and 1 kg of silicon dioxide with a purity of 98% were heated to 1850℃ for a first evaporation to obtain silicon vapor; an aluminum plate with a gold coating on its surface was heated to 650℃ and evaporated a second time under an argon atmosphere to obtain aluminum vapor; then the silicon vapor was introduced into the aluminum vapor at a rate of 4 g / min and reacted at 650℃ for 2.5 h to obtain silicon nanowires;
[0108] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 85 wt% for 50 min, conductive carbon black (SP) at a mass fraction of 1 wt%, styrene-butadiene rubber solution at a solid content of 5.6 wt% (the amount of styrene-butadiene rubber solution added is based on the mass fraction of styrene-butadiene rubber, which is 8 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, which is 4 wt%), and polyvinylpyrrolidone at a mass fraction of 2 wt% were added sequentially under a stirring speed of 200 rpm. Then, stirring was continued for 80 min to obtain a negative electrode slurry with a solid content of 7 wt% and a viscosity of 2000 cp.
[0109] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 80℃ for 120min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0110] In this embodiment, the mass fractions of conductive carbon black, styrene-butadiene rubber, carbon nanotubes, and polyvinylpyrrolidone are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0111] Example 6
[0112] This embodiment provides a method for preparing a negative electrode sheet, such as... Figure 1 As shown, the preparation method includes:
[0113] (1) 3 kg of 98% pure silicon dioxide was heated to 1800℃ for a first evaporation to obtain silicon dioxide vapor; an aluminum plate with a silver coating on its surface was heated to 700℃ and evaporated under an argon atmosphere to obtain aluminum vapor; then the silicon dioxide vapor was introduced into the aluminum vapor at a rate of 2 g / min and reacted at 750℃ for 3 h to obtain silicon nanowires.
[0114] (2) After mixing and grinding the silicon nanowires obtained in step (1) with water at a mass fraction of 78 wt% for 50 min, conductive carbon black (SP) at a mass fraction of 5 wt%, styrene-butadiene rubber solution at a solid content of 5.6 wt% (the amount of styrene-butadiene rubber solution added is based on the mass fraction of styrene-butadiene rubber, which is 10 wt%), carbon nanotube slurry at a solid content of 0.4 wt% (the amount of carbon nanotube slurry added is based on the mass fraction of carbon nanotubes, which is 3 wt%), and sodium carboxymethyl cellulose at a mass fraction of 4 wt%, the mixture was stirred for 80 min to obtain a negative electrode slurry with a solid content of 7 wt% and a viscosity of 2500 cp.
[0115] (3) The negative electrode slurry prepared in step (2) is coated onto the surface of copper foil using a 200μm height scraper and dried in an oven at 80℃ for 120min. Then, it is rolled and cut to obtain the negative electrode sheet.
[0116] In this embodiment, the mass fractions of conductive carbon black, styrene-butadiene rubber, carbon nanotubes, and sodium carboxymethyl cellulose are all calculated based on a total mass fraction of 100 wt% of the solid raw materials in the negative electrode slurry.
[0117] Comparative Example 1
[0118] The difference between this comparative example and Example 1 is that acetylene black, styrene-butadiene rubber solution, carbon nanotube slurry and sodium carboxymethyl cellulose are added simultaneously in step (2), while the other process parameters and operating conditions are the same as in Example 1.
[0119] Comparative Example 2
[0120] The difference between this comparative example and Example 1 is that the mass fraction of silicon nanowires in step (2) is 55 wt%, and the reduced mass of silicon nanowires is allocated to conductive carbon black, styrene-butadiene rubber, carbon nanotubes and sodium carboxymethyl cellulose according to the formulation ratio. The remaining process parameters and operating steps are the same as in Example 1.
[0121] Comparative Example 3
[0122] The difference between this comparative example and Example 1 is that the mass fraction of silicon nanowires in step (2) is 90 wt%, and the increase in mass of silicon nanowires is equal to the total amount of conductive carbon black, styrene-butadiene rubber, carbon nanotubes and sodium carboxymethyl cellulose reduced according to the formula ratio. The remaining process parameters and operating steps are the same as in Example 1.
[0123] The negative electrode sheets prepared in Examples 1-6 and Comparative Examples 1-3 were assembled into CR2032 coin cells: lithium sheet was used as counter electrode, Lelgard 2400 was used as separator, and 1 mol / L lithium hexafluorophosphate / ethyl carbonate + dimethyl carbonate (volume ratio 3:7) was used as electrolyte.
[0124] The constant current charge-discharge test was conducted using the Xinwei BTS battery testing system. The half-cell was charged and discharged using a current of 0.1C at a test temperature of 25℃.
[0125] The performance test results of the batteries assembled from the negative electrode sheets of Examples 1-6 and Comparative Examples 1-3 are shown in Table 1.
[0126] Table 1
[0127]
[0128]
[0129] From the data analysis in Table 1, we can conclude that:
[0130] (1) The batteries assembled from the negative electrode sheets prepared in Examples 1-6, as shown in Table 1, all have an initial discharge specific capacity higher than 3200 mAh / g. After 100 charge-discharge cycles, the discharge specific capacity of the batteries is still higher than 2750 mAh / g, and the capacity retention rate is also higher than 85%. Figure 3 It can be seen that the silicon nanowires prepared in Example 1 can still maintain their nanowire structure after 100 charge-discharge cycles, indicating that the nanowires obtained by the preparation method of the present invention have high structural stability; at the same time, from Figure 4 This further confirms that the battery assembled using the negative electrode sheet prepared by the method provided by this invention has excellent cycle stability. This demonstrates that the negative electrode sheet prepared by the method provided by this invention can effectively suppress the volume expansion of silicon during the lithium insertion / extraction process, thereby enabling the battery to possess excellent rate charge / discharge performance, cycle performance, and safety performance.
[0131] (2) The battery assembled from the negative electrode sheet prepared in Comparative Example 1 has a lower initial discharge specific capacity than that of Example 1, and its discharge specific capacity is only 1250 mAh / g after 50 charge-discharge cycles, and its capacity retention rate has dropped to 50%. However, the discharge specific capacity of Example 1 is 2781 mAh / g after 100 charge-discharge cycles, and its capacity retention rate can still reach 85.3%. That is, the cycle performance of the battery in Comparative Example 1 is much lower than that in Example 1. This is because Comparative Example 1 adds a first conductive agent, a binder solution, a second conductive agent and a thickener at the same time, resulting in poor conductivity of the obtained negative electrode sheet.
[0132] (3) The battery assembled from the negative electrode sheet prepared in Comparative Example 2 had a lower initial discharge specific capacity, a lower discharge specific capacity after 100 charge-discharge cycles, and a lower capacity retention rate than that of Example 1. The battery assembled from the negative electrode sheet prepared in Comparative Example 3 had a lower initial discharge specific capacity than that of Example 1, and its discharge specific capacity was only 1360 mAh / g after 50 charge-discharge cycles, with its capacity retention rate dropping to 80%. In contrast, the discharge specific capacity of Example 1 was 2781 mAh / g after 100 charge-discharge cycles, and its capacity retention rate was still 85.3%. That is, the overall performance of the batteries in Comparative Example 2 and Comparative Example 3 was much lower than that of Example 1. This is because the amount of silicon nanowires added in Comparative Example 2 was too low, and the amount of silicon nanowires added in Comparative Example 3 was too high. This shows that adjusting the amount of silicon nanowires added to a suitable range can effectively improve the electrochemical performance of the negative electrode sheet, thereby improving the electrochemical performance of the battery.
[0133] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a negative electrode sheet, characterized in that, The preparation method includes: Silicon nanowires and a first solvent are mixed under grinding conditions for 10-60 minutes. Then, a first conductive agent, a binder, a second conductive agent, and a thickener are added sequentially under stirring conditions at a speed of 100-300 rpm. Stirring is continued for 30-120 minutes to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of a current collector to obtain the negative electrode sheet. The total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of silicon nanowires added is 60-85 wt%. The first conductive agent and silicon nanowires are uniformly mixed to form a conductive link network.
2. The preparation method according to claim 1, characterized in that, The preparation process of the silicon nanowires includes: Silicon vapor is obtained by evaporating a silicon source once, and aluminum vapor is obtained by evaporating an aluminum source a second time. The silicon vapor is then passed into the aluminum vapor to react and obtain the silicon nanowires.
3. The preparation method according to claim 2, characterized in that, The purity of the silicon source is ≥95%.
4. The preparation method according to claim 2, characterized in that, The silicon source includes any one or a combination of at least two of silicon powder, silicon ingot, silicon dioxide, or silicon suboxide.
5. The preparation method according to claim 2, characterized in that, The temperature of the first evaporation is 1600~2000℃.
6. The preparation method according to claim 2, characterized in that, The aluminum source includes any one or a combination of at least two of aluminum plates, aluminum powder, or aluminum wire.
7. The preparation method according to claim 2, characterized in that, The surface of the aluminum source has a coating.
8. The preparation method according to claim 7, characterized in that, The coating material includes gold and / or silver.
9. The preparation method according to claim 2, characterized in that, The temperature for the secondary evaporation is 500~800℃.
10. The preparation method according to claim 2, characterized in that, The secondary evaporation is carried out in an argon atmosphere.
11. The preparation method according to claim 2, characterized in that, The silicon vapor is introduced into the aluminum vapor at a rate of 2~5 g / min.
12. The preparation method according to claim 2, characterized in that, The reaction temperature is 500~800℃.
13. The preparation method according to claim 2, characterized in that, The reaction time is 1 to 5 hours.
14. The preparation method according to claim 1, characterized in that, The silicon nanowires have a diameter of <200nm and a length of >100μm.
15. The preparation method according to claim 1, characterized in that, The first solvent includes water and / or ethanol.
16. The preparation method according to claim 1, characterized in that, With the total mass fraction of solid raw materials in the negative electrode slurry being 100wt%, the amount of the first conductive agent added is 1~15wt%.
17. The preparation method according to claim 1, characterized in that, The total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the binder added is 5~20 wt%.
18. The preparation method according to claim 1, characterized in that, The total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of the second conductive agent added is 0.5~5 wt%.
19. The preparation method according to claim 1, characterized in that, The total mass fraction of the solid raw materials in the negative electrode slurry is 100 wt%, and the amount of thickener added is 2-8 wt%.
20. The preparation method according to claim 1, characterized in that, The first conductive agent includes any one or a combination of at least two of conductive carbon black, acetylene black, carbon fiber, or conductive graphene.
21. The preparation method according to claim 1, characterized in that, The adhesive is mixed with the second solvent to prepare an adhesive solution. After the silicon nanowires and the first solvent are mixed, the first conductive agent, the adhesive solution, the second conductive agent and the thickener are added in sequence to obtain the negative electrode slurry.
22. The preparation method according to claim 21, characterized in that, The solid content of the adhesive solution is 4~6wt%.
23. The preparation method according to claim 1, characterized in that, The adhesive comprises any one or a combination of at least two of styrene-butadiene rubber, polyethylene glycol, or polyvinyl acetate.
24. The preparation method according to claim 21, characterized in that, The second solvent includes water and / or ethanol.
25. The preparation method according to claim 21, characterized in that, The second conductive agent is dispersed in a third solvent to form a second conductive agent slurry. After the silicon nanowires and the first solvent are mixed, the first conductive agent, the adhesive liquid, the second conductive agent slurry and the thickener are added in sequence to obtain the negative electrode slurry.
26. The preparation method according to claim 25, characterized in that, The solid content of the second conductive agent slurry is 0.2~0.6wt%.
27. The preparation method according to claim 1, characterized in that, The second conductive agent includes carbon nanotubes.
28. The preparation method according to claim 1, characterized in that, The thickener includes any one or a combination of at least two of sodium carboxymethyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, or polyvinylpyrrolidone.
29. The preparation method according to claim 1, characterized in that, The viscosity of the negative electrode slurry is 1000~3000cp.
30. The preparation method according to claim 1, characterized in that, The solid content of the negative electrode slurry is 6-8 wt%.
31. The preparation method according to claim 1, characterized in that, The preparation method further includes: The negative electrode slurry is coated onto the surface of the current collector and then dried to form a slurry coating on the surface of the current collector, thus obtaining the negative electrode sheet.
32. The preparation method according to claim 31, characterized in that, The drying process is carried out at a temperature of 70~90℃.
33. The preparation method according to claim 31, characterized in that, The drying process takes 60 to 240 minutes.
34. The preparation method according to claim 31, characterized in that, The thickness of the slurry coating is 150~250μm.
35. The preparation method according to claim 31, characterized in that, After the slurry coating is formed on the surface of the current collector, it is rolled and cut in sequence to obtain the negative electrode sheet.
36. A negative electrode sheet, characterized in that, The negative electrode sheet includes a current collector and a slurry coating on the surface of the current collector, and the negative electrode sheet is prepared by the preparation method according to any one of claims 1-35.
37. The negative electrode sheet according to claim 36, characterized in that, With a total mass of 100wt% for the slurry coating, the mass fraction of silicon nanowires in the slurry coating is 60-85wt%.
38. The negative electrode sheet according to claim 36, characterized in that, With a total mass of 100wt% for the slurry coating, the mass fraction of the first conductive agent in the slurry coating is 1~15wt%.
39. The negative electrode sheet according to claim 36, characterized in that, The total mass of the slurry coating is 100 wt%, and the mass fraction of the adhesive in the slurry coating is 5-20 wt%.
40. The negative electrode sheet according to claim 36, characterized in that, With a total mass of 100wt% for the slurry coating, the mass fraction of the second conductive agent in the slurry coating is 0.5~5wt%.
41. The negative electrode sheet according to claim 36, characterized in that, With a total mass of 100wt% for the slurry coating, the mass fraction of the thickener in the slurry coating is 2-8wt%.
42. A lithium-ion battery, characterized in that, The lithium-ion battery includes the negative electrode sheet as described in any one of claims 36-41.
Citation Information
Patent Citations
Method for preparing carbon fiber-silicon nanowire negative electrode material
CN103000865A
Silicon nanowire and application thereof
CN105609749A
Silicon nanowire and preparation method and application thereof
CN116730345A
Method for manufacturing silicon nanowire
JP2009161404A