Negative active material, negative electrode sheet, energy storage device, and electric device
By employing negative electrode active materials with specific pore size distribution in lithium-ion batteries, the compatibility problem between energy density and kinetic performance has been solved, improving the energy density and kinetic performance of the batteries, as well as improving cycle performance and lithium plating.
Patent Information
- Application Number
- CN202311510087.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-13
AI Technical Summary
In the process of increasing the energy density of lithium-ion batteries, the dynamic performance deteriorates, making it difficult to achieve a balance between high energy density and high dynamic performance.
The negative electrode active material adopts a structure of mesopores with a pore size of 2nm to 50nm and macropores with a pore size of 100nm to 200nm. The total volume percentage of mesopores is A, and the total volume percentage of macropores is B. B/A satisfies 3.0≤B/A≤5.0. By controlling the pore size distribution, the liquid absorption capacity and electronic conductivity are improved, and the interlayer expansion of the negative electrode active material during battery cycling is buffered.
It improves the energy density and dynamic performance of the battery, enhances the cycle performance and first-efficiency of the battery, reduces the occurrence of lithium plating, and improves the liquid absorption capacity and electronic conductivity of the negative electrode.
Smart Images

Figure BDA0004547313530000231
Abstract
Description
Technical Field
[0001] This invention relates to the field of energy storage technology, specifically to a negative electrode active material, a negative electrode sheet, an energy storage device, and electrical equipment. Background Technology
[0002] Fossil fuels remain the primary mode of global energy consumption, making energy storage crucial for human development. Energy storage mainly includes physical energy storage and electrochemical energy storage. Among these, electrochemical energy storage has seen the fastest growth in the past decade, with rechargeable batteries dominating the market. Rechargeable batteries, also known as accumulators or storage batteries, are batteries that can be recharged after discharge to reactivate their active materials and continue to be used. Specifically, utilizing the reversibility of chemical reactions, a new battery can be constructed. That is, after a chemical reaction converts into electrical energy, the electrical energy can be used to repair the chemical system, and then the chemical reaction can be converted back into electrical energy; hence the name rechargeable battery.
[0003] The main rechargeable batteries on the market include nickel-metal hydride batteries, nickel-cadmium batteries, lead-acid (or lead-acid) batteries, lithium-ion batteries, and polymer lithium-ion batteries. Among them, lithium-ion batteries have advantages such as high energy density, safety and reliability, and environmental friendliness, and are widely used in transportation power supplies, power storage, 3C products, and aerospace and military industries.
[0004] With the development of lithium-ion batteries, the market has placed increasingly higher demands on their energy density. However, increasing energy density can also lead to a deterioration in the kinetic performance of lithium-ion batteries. From a technical perspective, it is difficult to achieve a perfect balance between high energy density and high kinetic performance. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a negative electrode active material, a negative electrode sheet, an energy storage device, and an electrical device. The negative electrode active material has pores with a specific pore size distribution, which enables the negative electrode sheet to have better liquid absorption capacity and better electronic conductivity, thus balancing the energy density and kinetic performance of the battery.
[0006] The technical solution is as follows:
[0007] A negative electrode active material includes: mesopores with a pore size of 2 nm to 50 nm and macropores with a pore size of 100 nm to 200 nm;
[0008] The total volume percentage of the mesopores is A, and the total volume percentage of the macropores is B, where B / A satisfies: 3.0 ≤ B / A ≤ 5.0.
[0009] Research has shown that mesoporous structures with pore sizes of 2nm to 50nm can effectively improve the liquid absorption capacity and electronic conductivity of the negative electrode active material, thereby improving the battery's kinetic performance. Macroporous structures with pore sizes of 100nm to 200nm can effectively buffer the damage to the interlayer structure caused by the expansion of the negative electrode active layers during cycling, thus improving the battery's cycle performance. Furthermore, when there are too few pores with pore sizes of 2nm to 50nm, insufficient battery kinetic performance can lead to lithium plating, resulting in decreased cycle performance. Conversely, too many pores with pore sizes of 2nm to 50nm can cause excessive lithium source consumption during battery film formation, reducing the battery's initial efficiency. When there are too few pores with pore sizes of 100nm to 200nm, the active layer may peel off during cycling due to lithium ion insertion and extraction, leading to failure. Conversely, too many pores with pore sizes of 100nm to 200nm can also cause insufficient kinetic performance, leading to lithium plating and cell failure during cycling. The present invention, through the specific pore size distribution described above, enables the negative electrode sheet to have better liquid absorption capacity and better electronic conductivity, which is beneficial to balancing the energy density and dynamic performance of the battery.
[0010] In some embodiments, the specific surface area of the negative electrode active material is 1.0 m². 2 / g~2.0m 2 / g, negative electrode active materials that meet this requirement are more conducive to electrolyte wetting, which in turn improves the diffusion rate of ions and improves the overall cycle performance of the battery.
[0011] In some embodiments, the negative electrode active material is selected from at least one of graphite, activated carbon, and silicon compounds. These negative electrode active materials are widely available, abundant, have relatively stable electrochemical performance, and their actual specific capacity density can be close to the theoretical specific capacity, which is more conducive to improving the performance of the negative electrode sheet while reducing costs.
[0012] In some embodiments, the sulfur content of the negative electrode active material is below 5 wt%, and controlling the sulfur content of the negative electrode active material is beneficial to improving the performance of the negative electrode sheet and the lithium battery.
[0013] The present invention also provides a method for preparing the negative electrode active material as described above, comprising the following steps:
[0014] A solid composite is prepared by molding a mixture containing a carbon source, catalyst, conductive agent and binder.
[0015] The solid composite was graphitized, and negative electrode active materials with different pore structures were obtained by controlling different graphitization times.
[0016] The raw materials are tightly bonded together through molding, and graphitization is combined with graphitization to transform non-graphitic carbon into graphitic carbon / graphite microcrystals with a three-dimensional regular and ordered graphite structure through physical changes under high temperature. By controlling different graphitization times, negative electrode active materials with different porous structures can be obtained. Graphitization also improves the product's bulk density, electrical conductivity, thermal conductivity, corrosion resistance, and machinability.
[0017] In some embodiments, the molding process is carried out at a pressure of 150 MPa to 250 MPa, which is beneficial for pressing the materials together, making them more stable and facilitating subsequent graphitization.
[0018] In some embodiments, the graphitization treatment temperature is 2500℃~3000℃ and the time is 15h~50h, which is beneficial to improve the degree of graphitization of the product. The better the degree of graphitization, the fewer cracks, which is more conducive to improving the performance of the negative electrode sheet and lithium battery.
[0019] In some embodiments, the carbon source is coke, and the sulfur content of the coke is less than 5 wt%. During graphitization, the release of sulfur promotes the formation of internal pores in the graphite. Controlling the sulfur content of the coke is beneficial to improving the performance of the negative electrode and the lithium battery.
[0020] The present invention also provides a negative electrode sheet, comprising: a negative electrode current collector and at least one negative electrode active layer disposed on the surface of the negative electrode current collector, wherein each negative electrode active layer comprises a negative electrode active material as described above, or a negative electrode active material prepared according to the preparation method described above. This negative electrode sheet has better liquid absorption capacity and better electronic conductivity.
[0021] In some embodiments, the negative electrode active layer has one layer and a thickness of 20 nm to 120 nm.
[0022] In some embodiments, the negative electrode active layer is multilayered, and the total volume ratio of macropores in the negative electrode active material in each negative electrode active layer decreases progressively along the direction away from the negative electrode current collector. Macropore structures help reduce material expansion during cycling, while mesopore structures facilitate lithium-ion intercalation. By controlling the macropore structure to gradually decrease and the mesopore structure to gradually increase along the direction away from the current collector, lithium ions can more easily intercalate into the negative electrode active material, improving the battery's kinetic performance, wetting performance, and cycle performance. Furthermore, by reducing material expansion during cycling through macropore structures in the negative electrode active material closer to the current collector, cycle performance is further improved. This avoids excessive volume expansion of the active material during cycling, which could lead to poor adhesion between the negative electrode active material and the current collector, thus affecting electron transport and causing deterioration in cycle performance.
[0023] In some embodiments, the negative electrode active layer is multi-layered, and the thickness of each negative electrode active layer decreases gradually along the direction away from the negative electrode current collector. This arrangement is more conducive to improving the liquid absorption capacity and electronic conductivity of the negative electrode sheet, while taking into account the energy density and dynamic performance of the battery.
[0024] In some embodiments, the negative electrode sheet includes: a negative electrode current collector and a first negative electrode active layer and a second negative electrode active layer sequentially disposed on the surface of the negative electrode current collector. The first negative electrode active layer satisfies: 4.5≤B / A≤5.0; the second negative electrode active layer satisfies: 3.0≤B / A<4.5, which is more conducive to improving the liquid absorption capacity and electronic conductivity of the negative electrode sheet, while taking into account the energy density and dynamic performance of the battery.
[0025] In some embodiments, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 1:(0.3~1.1). The upper active material improves the wettability of the battery and enhances the cycle performance; the lower active material reduces the expansion behavior of the material during cycling, further enhancing the cycle performance.
[0026] In some embodiments, the thickness of the first negative electrode active layer is 20 nm to 90 nm. Controlling the thickness within this range is beneficial for further improving the liquid absorption capacity and electronic conductivity of the negative electrode sheet, while taking into account the energy density and kinetic performance of the battery.
[0027] In some embodiments, each of the negative electrode active layers further comprises a negative electrode conductive agent and a negative electrode binder; in each active layer, the mass percentage of the negative electrode active material is independently 75% to 95%, the mass percentage of the negative electrode conductive agent is independently 2% to 15%, and the mass percentage of the negative electrode binder is independently 3% to 10%.
[0028] In some embodiments, each of the negative electrode conductive agents is selected from at least one of carbon nanotubes, carbon nanofibers, conductive graphite, graphene, acetylene black, and carbon black, which have the advantages of high conductivity and low resistance.
[0029] In some embodiments, each of the negative electrode binders is selected from at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, and polyacrylate. These binders can better adhere and retain the negative electrode active material on the current collector, enhance the electronic contact between the negative electrode active material and the conductive agent, and between the negative electrode active material and the current collector, and can better achieve the effects of dispersion, thickening, suspension, bonding, and facilitating lithium ion transport.
[0030] The present invention also provides an energy storage device, comprising the negative electrode active material as described above, or comprising the negative electrode sheet as described above.
[0031] The present invention also provides an electrical device, including the energy storage device as described above, wherein the energy storage device supplies power to the electrical device. Detailed Implementation
[0032] To facilitate understanding of the present invention, a more complete description will be provided below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0034] When using “including,” “having,” and “contains” as described herein, the intention is to cover non-exclusive inclusion, unless an explicit qualifying term such as “only,” “consisting of,” etc., is used, in which case another component may be added.
[0035] In this invention, the terms "preferredly," "more preferably," "better," and "even better" refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of the invention. That is, in this invention, "preferredly," "more preferably," "better," and "even better" are merely descriptions of more effective implementations or examples, but do not constitute a limitation on the scope of protection of the invention.
[0036] In this invention, terms such as "further," "even more," and "particularly" are used for descriptive purposes and to indicate differences in content, but should not be construed as limiting the scope of protection of this invention.
[0037] In this invention, "at least one" means one or more, such as one, two, or more. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layered" means at least two layers, such as two layers, three layers, etc., unless otherwise explicitly specified. In the description of this invention, "several" means at least one, such as one, two, etc., unless otherwise explicitly specified.
[0038] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0039] Unless otherwise specified, all steps of this invention may be performed sequentially or randomly. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0040] Unless otherwise stated, a singular term may include a plural term and should not be understood as having a quantity of one.
[0041] In this invention, "above" or "below" both include the number itself. For example, "below 1" includes 1.
[0042] With the development of lithium-ion batteries, the market has placed increasingly higher demands on their energy density. However, increasing energy density can also lead to a deterioration in the kinetic performance of lithium-ion batteries. From a technical perspective, it is difficult to achieve a perfect balance between high energy density and high kinetic performance.
[0043] To address the aforementioned problems, this invention provides a negative electrode active material, a negative electrode sheet, an energy storage device, and an electrical device. The negative electrode active material has pores with a specific pore size distribution, which enables the negative electrode sheet to have better liquid absorption capacity and better electronic conductivity, thus balancing the energy density and kinetic performance of the battery.
[0044] The technical solution is as follows:
[0045] A negative electrode active material includes: mesopores with a pore size of 2 nm to 50 nm and macropores with a pore size of 100 nm to 200 nm;
[0046] The total volume percentage of the mesopores is A, and the total volume percentage of the macropores is B, where B / A satisfies: 3.0 ≤ B / A ≤ 5.0.
[0047] Research has shown that mesoporous structures with pore sizes of 2nm to 50nm can effectively improve the liquid absorption capacity and electronic conductivity of the negative electrode active material, thereby improving the battery's kinetic performance. Macroporous structures with pore sizes of 100nm to 200nm can effectively buffer the expansion between the negative electrode active layers during cycling, thus improving the battery's cycle performance. Furthermore, when there are too few pores in the 2nm to 50nm range, insufficient battery kinetic performance can lead to lithium plating, resulting in decreased cycle performance. Conversely, too many pores in the 0nm to 50nm range can cause excessive lithium source consumption during film formation, reducing the battery's initial efficiency. When there are too few pores in the 100nm to 200nm range, the active material's interlayer structure may fail during cycling due to lithium ion insertion and extraction, potentially causing the active layer (such as the graphite layer) to peel off. Conversely, too many pores in the 100nm to 200nm range can also lead to insufficient kinetic performance, resulting in lithium plating and cell failure during cycling. The present invention, through the specific pore size distribution described above, enables the negative electrode sheet to have better liquid absorption capacity and better electronic conductivity, which is beneficial to balancing the energy density and dynamic performance of the battery.
[0048] Understandably, in this invention, the pore size of the mesopore is 2nm to 50nm, including but not limited to 2nm, 4nm, 8nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm.
[0049] Understandably, in this invention, the aperture of the macropore is 100nm to 200nm, including but not limited to 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 18nm, 190nm or 200nm.
[0050] Understandably, in this invention, the total volume percentage of mesopores is A, which refers to the percentage of the total volume of all mesopores in the negative electrode active material to the total volume of all pores in the negative electrode active material; the total volume percentage of macropores is B, which refers to the percentage of the total volume of all macropores in the negative electrode active material to the total volume of all pores in the negative electrode active material.
[0051] Preferably, the present invention uses an ASAP2460 physical adsorption analyzer as the testing instrument. The dried and degassed sample is placed in liquid nitrogen, and the adsorption amount of nitrogen is measured by adjusting different test pressures. Adsorption and desorption isotherms are then plotted. The pore shape is determined based on the shape of the hysteresis loop, and pore size distribution curves are obtained according to different pore models. The raw pore size distribution data is imported into plotting software, and the peak areas of each part are calculated using a peak fitting method, corresponding to the values of parameters A and B.
[0052] Understandably, in this invention, B / A satisfies: 3.0 ≤ B / A ≤ 5.0, including but not limited to 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, or 5.0. Preferably, B / A satisfies: 3.04 ≤ B / A ≤ 4.95.
[0053] In some embodiments, the specific surface area of the negative electrode active material is 1.0 m². 2 / g~2.0m 2 A negative electrode active material with a specific surface area of 1.0 m² / g is more conducive to electrolyte wetting, which in turn improves the diffusion rate of ions and enhances the overall cycle performance of the battery. Understandably, the specific surface area of the negative electrode active material includes, but is not limited to, 1.0 m² / g. 2 / g, 1.2m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.8m 2 / g or 2.0m 2 / g.
[0054] In some embodiments, the negative electrode active material is selected from at least one of graphite, activated carbon, and silicon compounds. These negative electrode active materials are widely available, abundant, have relatively stable electrochemical performance, and their actual specific capacity density can be close to the theoretical specific capacity, which is more conducive to improving the performance of the negative electrode sheet while reducing costs. Preferably, the negative electrode active material is graphite.
[0055] In some embodiments, the sulfur content of the negative electrode active material is below 5 wt%, which is beneficial for improving the performance of the negative electrode sheet and the lithium battery. Further, the sulfur content of the negative electrode active material is between 0.5 wt% and 5 wt%.
[0056] Preferably, this invention refers to the method for determining sulfur content in graphite anode materials for lithium-ion batteries in Appendix J of GB / T 24533-2019, "Method for Determination of Sulfur Content", and establishes a method for determining sulfur content in graphite anode materials for lithium-ion batteries using a Shimadzu ICPE-9820 inductively coupled plasma optical emission spectrometer (ICP-OES).
[0057] The present invention also provides a method for preparing the negative electrode active material as described above, comprising the following steps:
[0058] A solid composite is prepared by molding a mixture containing a carbon source, catalyst, conductive agent and binder.
[0059] The solid composite was graphitized, and negative electrode active materials with different pore structures were obtained by controlling different graphitization times.
[0060] The raw materials are tightly bonded together through molding, and graphitization is combined with graphitization to transform non-graphitic carbon into graphitic carbon / graphite microcrystals with a three-dimensional regular and ordered graphite structure through physical changes under high temperature. By controlling different graphitization times, negative electrode active materials with different porous structures can be obtained. Graphitization also improves the product's bulk density, electrical conductivity, thermal conductivity, corrosion resistance, and machinability.
[0061] In some embodiments, the molding process is carried out at a pressure of 150 MPa to 250 MPa, which is beneficial for pressing the materials together, making them more stable and facilitating subsequent graphitization.
[0062] In some embodiments, the graphitization treatment temperature is 2500℃~3000℃ and the time is 15h~50h, which is beneficial to improve the degree of graphitization of the product. The better the degree of graphitization, the fewer cracks, which is more conducive to improving the performance of the negative electrode sheet and lithium battery.
[0063] In some embodiments, the carbon source is coke, and the sulfur content of the coke is less than 5 wt%. During graphitization, the release of sulfur promotes the formation of internal pores in the graphite. Controlling the sulfur content of the coke is beneficial to improving the performance of the negative electrode and the lithium battery. Further, the sulfur content of the coke is 1 wt% to 5 wt%.
[0064] It is understood that the catalyst described in this invention is a conventional catalyst used in the preparation of negative electrode active materials in the art, and there are no requirements thereto. Optionally, the catalyst is iron(III) oxide (Fe3O4).
[0065] Similarly, the conductive agent used in the preparation of the negative electrode active material described in this invention is a conductive agent conventionally used in the art for preparing negative electrode active materials, and there are no specific requirements for this. Optionally, the conductive agent used in the preparation of the negative electrode active material is conductive carbon black.
[0066] Similarly, the binder used in the preparation of the negative electrode active material described in this invention is a binder conventionally used in the preparation of negative electrode active materials in the art, and there are no requirements regarding its use. Optionally, the binder used in the preparation of the negative electrode active material is asphalt.
[0067] The present invention also provides a negative electrode sheet, comprising: a negative electrode current collector and at least one negative electrode active layer disposed on the surface of the negative electrode current collector, wherein each negative electrode active layer comprises a negative electrode active material as described above, or a negative electrode active material prepared according to the preparation method described above. This negative electrode sheet has better liquid absorption capacity and better electronic conductivity.
[0068] In some embodiments, the negative electrode active layer is a single layer with a thickness of 20nm to 120nm, including but not limited to 20nm, 40nm, 50nm, 6nm, 80nm, 90nm, 100nm, 110nm or 120nm.
[0069] In some embodiments, the negative electrode active layer is multilayered, and the total volume ratio of macropores in the negative electrode active material in each negative electrode active layer decreases progressively along the direction away from the negative electrode current collector. Macropore structures help reduce material expansion during cycling, while mesopore structures facilitate lithium-ion intercalation. By controlling the macropore structure to gradually decrease and the mesopore structure to gradually increase along the direction away from the current collector, lithium ions can more easily intercalate into the negative electrode active material, improving the battery's kinetic performance, wetting performance, and cycle performance. Furthermore, by reducing material expansion during cycling through macropore structures in the negative electrode active material closer to the current collector, cycle performance is further improved. This avoids excessive volume expansion of the active material during cycling, which could lead to poor adhesion between the negative electrode active material and the current collector, thus affecting electron transport and causing deterioration in cycle performance.
[0070] In some embodiments, the negative electrode active layer is multi-layered, and the thickness of each negative electrode active layer decreases gradually along the direction away from the negative electrode current collector. This arrangement is more conducive to improving the liquid absorption capacity and electronic conductivity of the negative electrode sheet, while taking into account the energy density and dynamic performance of the battery.
[0071] In some embodiments, the negative electrode sheet includes: a negative electrode current collector and a first negative electrode active layer and a second negative electrode active layer sequentially disposed on the surface of the negative electrode current collector. The first negative electrode active layer satisfies: 4.5 ≤ B / A ≤ 5.0; the second negative electrode active layer satisfies: 3.0 ≤ B / A < 4.5, which is more conducive to improving the liquid absorption capacity and electronic conductivity of the negative electrode sheet, while taking into account the energy density and dynamic performance of the battery. It is understood that in the first negative electrode active layer, B / A includes, but is not limited to, 4.5, 4.6, 4.7, 4.8, 4.9, or 5.0. In the second negative electrode active layer, B / A includes, but is not limited to, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, or 4.4. Preferably, the first negative electrode active layer satisfies: 4.5≤B / A≤5.0; the second negative electrode active layer satisfies: 3≤B / A≤3.5.
[0072] In some embodiments, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 1:(0.3-1.1). This improves the battery's wettability and cycle performance through the upper active material, and further enhances cycle performance by reducing material expansion during cycling through the lower active material. Understandably, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer includes, but is not limited to, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.0, 1:1.075, or 1:1.1. Preferably, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 1:(0.4-1). More preferably, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 1:(0.4-0.98).
[0073] In some embodiments, each of the negative electrode active layers further comprises a negative electrode conductive agent and a negative electrode binder; in each active layer, the mass percentage of the negative electrode active material is independently 75% to 95%, the mass percentage of the negative electrode conductive agent is independently 2% to 15%, and the mass percentage of the negative electrode binder is independently 3% to 10%.
[0074] Understandably, in the negative electrode active layer, the mass percentage of the negative electrode active material is 75% to 95%, including but not limited to 75%, 80%, 85%, 90%, 92%, 93%, 94%, 94.5%, and 95%; the mass percentage of the negative electrode conductive agent is 2% to 15%, including but not limited to 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.6%, 3.8%, 4.0%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%; and the mass percentage of the negative electrode binder is 3% to 10%, including but not limited to 3%, 3.2%, 3.5%, 3.6%, 3.8%, 4.0%, 4.5%, 5%, 6%, 7%, 8%, 9%, or 10%.
[0075] In some embodiments, each of the negative electrode conductive agents is selected from at least one of carbon nanotubes, carbon nanofibers, conductive graphite, graphene, acetylene black, and carbon black, which have the advantages of high conductivity and low resistance. Further, the carbon black is selected from at least one of Ketjen black, channel black, furnace black, and hot-dip galvanized black.
[0076] In some embodiments, each of the negative electrode binders is selected from at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, and polyacrylate. These binders can better adhere and retain the negative electrode active material on the current collector, enhance the electronic contact between the negative electrode active material and the conductive agent, and between the negative electrode active material and the current collector, and can better perform the effects of dispersion, thickening, suspension, bonding, and facilitating lithium-ion transport. Preferably, each of the negative electrode binders is sodium carboxymethyl cellulose, such as one or a mixture of sodium carboxymethyl cellulose and lithium carboxymethyl cellulose.
[0077] In some embodiments, the negative current collector is selected from metal foil or porous metal plate. Preferably, the current collector is metal foil, such as copper foil or aluminum foil, and more preferably copper foil.
[0078] In addition, the present invention also provides a method for preparing the above-mentioned negative electrode sheet.
[0079] In some embodiments, the method for preparing the above-mentioned negative electrode sheet includes the following steps:
[0080] S100: Prepare the slurry according to the above design of the negative electrode sheet.
[0081] S200: A slurry is coated on the surface of the negative electrode current collector to form the negative electrode active layer.
[0082] In some embodiments, the negative electrode sheet includes multiple active layers, and the method for preparing the negative electrode sheet includes the following steps:
[0083] S100: According to the above design of the negative electrode sheet, prepare the first slurry and the second slurry respectively.
[0084] S200: A first slurry and a second slurry are coated on the surface of the negative electrode current collector to prepare a first negative electrode active layer and a second negative electrode active layer.
[0085] In some embodiments, the first slurry and the second slurry can be applied sequentially in step S200, or the first slurry and the second slurry can be applied simultaneously using a double-layer coating machine.
[0086] In some embodiments, in step S200, the first and second slurries are dried and cold-pressed to form a first and second negative electrode active layer on the surface of the negative electrode current collector.
[0087] Understandably, as the number of designed negative electrode active layers increases, the types of slurry also increase accordingly.
[0088] The present invention also provides an energy storage device comprising the negative electrode active material as described above, or comprising the negative electrode sheet as described above. It is understood that the energy storage device of the present invention has the beneficial effects described above for the negative electrode active material or negative electrode sheet, which will not be repeated here. In general, the energy storage device has high energy density and good kinetic performance.
[0089] Optionally, the energy storage device is a battery. Further, the battery is a lithium-ion battery.
[0090] In one embodiment, the battery is selected from one of button cells, pouch cells, prismatic cells, and cylindrical cells.
[0091] In one embodiment, the battery further includes a positive electrode sheet, the positive electrode sheet including a positive current collector and a positive active layer disposed on the surface of the positive current collector;
[0092] The positive electrode active layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder.
[0093] In some embodiments, the positive current collector is selected from metal foil or porous metal plate. Preferably, the current collector is metal foil, such as copper foil or aluminum foil, and more preferably aluminum foil.
[0094] In one embodiment, the positive electrode active material is selected from one or a mixture of several of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and lithium titanate.
[0095] In one embodiment, the positive electrode conductive agent is selected from one or a mixture of several of acetylene black, graphene, carbon nanotubes and carbon black.
[0096] In one embodiment, the positive electrode binder is selected from one or a mixture of several of polyvinylidene fluoride (PVDF), polyimide (PI), polyacrylic acid (PAA), and polytetrafluoroethylene (PTFE).
[0097] In one embodiment, the battery further includes a separator, optionally made of polypropylene (PP) or polyethylene (PE).
[0098] In one embodiment, the battery further includes an electrolyte.
[0099] Optionally, the solvent in the electrolyte is a mixed solvent composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1. The lithium salt in the electrolyte is LiPF6, and further, its concentration in the electrolyte is 1 mol / L.
[0100] The present invention also provides a method for preparing a battery, comprising the following steps:
[0101] (1) Preparation of the positive electrode sheet:
[0102] The positive electrode active material, positive electrode conductive agent, and positive electrode binder are mixed in a solvent, stirred until homogeneous, and then uniformly coated onto the positive electrode current collector. After drying, the positive electrode sheet is obtained. Metal foil or porous metal plates can be used as the positive electrode current collector. Aluminum foil is preferred.
[0103] (2) Preparation of negative electrode sheet:
[0104] A negative electrode active slurry is provided, wherein the components of the negative electrode active slurry include a negative electrode active material, a negative electrode conductive agent, and a binder;
[0105] The negative electrode active slurry is coated on the surface of the negative electrode current collector to form a negative electrode active layer.
[0106] (3) Preparation of electrolyte:
[0107] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed, and then a dry lithium salt is dissolved in the mixed organic solvent to prepare an electrolyte.
[0108] Optionally, the volume ratio of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) is 1:1:1. Optionally, the lithium salt is LiPF6, and further, its concentration in the electrolyte is 1 mol / L.
[0109] (4) Provide a diaphragm.
[0110] (5) Battery fabrication:
[0111] The positive electrode, negative electrode, separator, and electrolyte are assembled into a battery cell.
[0112] The present invention also provides an electrical device including the energy storage device described above, wherein the energy storage device supplies power to the electrical device. It is understood that the electrical device of the present invention has the beneficial effects described above for the negative electrode active material or negative electrode sheet, which will not be repeated here. Optionally, the electrical device may include a battery pack composed of multiple lithium-ion batteries as described above. Optionally, the electrical device may be a lighting fixture, etc.
[0113] The present invention will be described below through specific embodiments. It should be noted that the specific embodiments below are for illustrative purposes only and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods that do not specifically describe the conditions or steps are conventional methods, and the reagents and materials used can be obtained commercially.
[0114] Example 1
[0115] This embodiment provides a negative electrode active material and its preparation method, a negative electrode sheet and its preparation method, and a lithium battery and its preparation method, as detailed below:
[0116] (1) Preparation of the positive electrode sheet:
[0117] Lithium iron phosphate, polyvinylidene fluoride (PVDF), and acetylene black were added to NMP solvent at a mass ratio of 96:2:2 and stirred until homogeneous. The mixture was then coated onto an aluminum foil current collector and dried to form a positive electrode active material layer. This layer was then cut into positive electrode sheets for later use, with an areal density of 24 mg / cm³. 2 The compacted density is 2.6 g / cm³. 3 .
[0118] (2) Preparation of negative electrode sheet:
[0119] Coke raw material with a sulfur content of 2.2 wt% was crushed and mixed to serve as a carbon source. The carbon source, catalyst iron oxide, conductive carbon black, and binder asphalt were mechanically fused for 25 min to obtain a mixture. The mixture was then pressurized into isostatic blocks at a pressure of 200 MPa. The isostatic blocks were graphitized at 2900℃ for 32 h according to the parameters in Table 1. By controlling different graphitization times, graphite with different pore structures was obtained, which was subsequently used as a negative electrode active material.
[0120] According to the parameters in Table 1, the negative electrode active material, conductive agent acetylene black, thickener (CMC), and binder (SBR) were mixed in a mass ratio of 96.4:1:1.2:1.4. Deionized water was then added to the mixture, and the mixture was stirred under vacuum until homogeneous, yielding a negative electrode slurry. This slurry was uniformly coated onto the surface of the negative electrode current collector copper foil, and then dried, cold-pressed, and slit to obtain an areal density of 12 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 The negative electrode sheet.
[0121] (3) Preparation of electrolyte:
[0122] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare an electrolyte.
[0123] (4) Preparation of the diaphragm:
[0124] A polyethylene film with a thickness of 12 micrometers was selected.
[0125] (5) Battery assembly:
[0126] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to act as a separator. The electrolyte is then added, and the cells are assembled into a button cell.
[0127] Example 2
[0128] This embodiment is basically the same as Embodiment 1. The difference from Embodiment 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, i.e., the B1 / A1 ratios are different, as shown in Table 1.
[0129] Example 3
[0130] This embodiment is basically the same as Embodiment 1. The difference from Embodiment 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, i.e., the B1 / A1 ratios are different, as shown in Table 1.
[0131] Example 4
[0132] This embodiment is basically the same as Embodiment 1. The difference from Embodiment 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, i.e., the B1 / A1 ratios are different, as shown in Table 1.
[0133] Example 5
[0134] This embodiment is basically the same as Embodiment 1. The difference from Embodiment 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, i.e., the B1 / A1 ratios are different, as shown in Table 1.
[0135] Example 6
[0136] This embodiment is basically the same as Embodiment 5, except that two negative electrode active materials are prepared in this embodiment, and the negative electrode sheet in this embodiment includes two negative electrode active layers, as detailed below:
[0137] (1) Preparation of the positive electrode sheet:
[0138] Same as Example 5.
[0139] (2) Preparation of negative electrode sheet:
[0140] Coke raw material with a sulfur content of 4.3 wt% was crushed and mixed to serve as a carbon source. The carbon source, iron(III) oxide catalyst, conductive carbon black conductive agent, and asphalt binder were mechanically fused for 25 min to obtain a mixture. The mixture was then pressurized into an isostatic block at a pressure of 200 MPa. The isostatic block was graphitized at 2900℃ for 16 h according to the parameters in Table 1. By controlling different graphitization times, graphite with different pore structures was obtained, which was subsequently used as the first negative electrode active material.
[0141] Coke raw material with a sulfur content of 2.6 wt% was crushed and mixed to serve as a carbon source. The carbon source, iron oxide catalyst, conductive carbon black, and binder asphalt were mechanically fused for 25 min to obtain a mixture. The mixture was then pressurized into an isostatic block at a pressure of 200 MPa. The isostatic block was graphitized at 2900℃ for 27 h according to the parameters in Table 1. By controlling different graphitization times, graphite with different pore structures was obtained, which was subsequently used as the second negative electrode active material.
[0142] According to the parameters in Table 1, the first negative electrode active material, conductive agent acetylene black, thickener (CMC), and binder (SBR) were mixed in a mass ratio of 96.4:1:1.2:1.4. Deionized water was then added to the mixture, and the mixture was stirred under vacuum until homogeneous, yielding a negative electrode slurry. This negative electrode slurry was uniformly coated onto the surface of the negative electrode current collector copper foil, and then dried to obtain the first negative electrode active layer. The second negative electrode active material, conductive agent acetylene black, thickener (CMC), and binder (SBR) were mixed in a mass ratio of 96.4:1:1.2:1.4. Deionized water was then added to the mixture, and the mixture was stirred under vacuum until homogeneous, yielding a negative electrode slurry. This negative electrode slurry was uniformly coated onto the surface of the first negative electrode active layer, and then dried, cold-pressed, and slit to obtain a surface density of 12 mg / cm³. 2 The compacted density is 1.5 g / cm³. 3 .
[0143] (3) Preparation of electrolyte:
[0144] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare an electrolyte.
[0145] (4) Preparation of the diaphragm:
[0146] A polyethylene film with a thickness of 12 micrometers was selected.
[0147] (5) Battery assembly:
[0148] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to act as a separator. The electrolyte is then added, and the cells are assembled into a button cell.
[0149] Example 7
[0150] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer are changed in this embodiment, as shown in Table 1.
[0151] Example 8
[0152] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer are changed in this embodiment, as shown in Table 1.
[0153] Example 9
[0154] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer are changed in this embodiment, as shown in Table 1.
[0155] Example 10
[0156] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer are changed in this embodiment, as shown in Table 1.
[0157] Example 11
[0158] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer is changed in this embodiment, as shown in Table 1.
[0159] Example 12
[0160] This embodiment is basically the same as embodiment 6, except that the thickness of the first negative electrode active layer and the second negative electrode active layer is changed in this embodiment, as shown in Table 1.
[0161] Example 13
[0162] This embodiment is basically the same as Embodiment 7, except that the sulfur content and graphitization time of the coke raw material in the preparation method of the second negative electrode active material are changed, that is, the ratio of B2 / A2 in the second negative electrode active layer is changed, as shown in Table 1.
[0163] Example 14
[0164] This embodiment is basically the same as Embodiment 7, except that the sulfur content and graphitization time of the coke raw material in the preparation method of the second negative electrode active material are changed, that is, the ratio of B2 / A2 in the second negative electrode active layer is changed, as shown in Table 1.
[0165] Comparative Example 1
[0166] This comparative example is basically the same as Example 1. The difference from Example 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, and the B1 / A1 ratios are different. See Table 1 for details.
[0167] Comparative Example 2
[0168] This comparative example is basically the same as Example 1. The difference from Example 1 is that the sulfur content and graphitization time of the coke raw material in the preparation method of the negative electrode active material are different, as are the volume ratios of mesopores and macropores in the negative electrode active material, and the B1 / A1 ratios are different. See Table 1 for details.
[0169] test:
[0170] (1) Pore size distribution of the negative electrode active material:
[0171] The testing instrument was an ASAP2460 physical adsorption analyzer. The dried and degassed sample was placed in liquid nitrogen, and the adsorption amount of nitrogen was measured by adjusting different test pressures. Adsorption and desorption isotherms were plotted. The pore shape was determined based on the shape of the hysteresis loop, and pore size distribution curves were obtained according to different pore models. The raw pore size distribution data was imported into plotting software, and the peak areas of each part were calculated using peak fitting, corresponding to the number of parameters A and B.
[0172] (2) Examine battery performance:
[0173] 1) Charge / discharge performance test conditions: At room temperature (25℃), the lithium-ion batteries obtained in the comparative example and the embodiment were charged to 3.65V at a constant power rate of 0.5P (P is power, P = nominal capacity × 3.2V), rested for 5 minutes, and then discharged to 2.5V at a rate of 0.5P. The discharge capacity was measured, and this was considered one cycle. The capacity retention rate (%) was calculated according to the following formula:
[0174] It is understandable that 2000cls refers to 2000 cycles, or 2000 loops.
[0175] 2000cls capacity retention rate (%) = discharge capacity of the 2000th cycle / initial discharge capacity (i.e., the discharge capacity of the first cycle × 100%).
[0176] 2000cls cycle expansion rate = (Battery thickness after the 2000th discharge cycle - Battery thickness after the first discharge cycle) / Battery thickness after the first discharge cycle × 100%.
[0177] 2) Lithium plating test
[0178] At 25°C, the batteries prepared in the examples and comparative examples were charged to 3.65V at a rate of 0.5C and discharged to 2.5V at a rate of 0.5C for three full charge and discharge cycles. Then, the batteries prepared in the examples and comparative examples were discharged to 2.5V at a rate of 1C and charged to 3.65V at a rate of 1C for 10 cycles. After these cycles, the batteries were disassembled to check the lithium plating.
[0179] Lithium plating degree determination: The degree is determined by judging the area of lithium plating on the electrode surface; 0% lithium plating area: no lithium plating; 0% < lithium plating area ≤ 20%: slight lithium plating; 20% ≤ lithium plating area ≤ 50%: moderate lithium plating; lithium plating area > 50%: severe lithium plating.
[0180] The main parameters of the negative electrode active material, preparation method, composition of the negative electrode active layer, and composition and test data of the lithium-ion battery in Examples 1 to 14 and Comparative Examples 1 to 2 are recorded in Table 1.
[0181] Table 1
[0182]
[0183] Note: In Table 1, "--" indicates none.
[0184] As shown in Table 1, when the B / A ratio is below the lower limit, the proportion of macropores is relatively small. Due to the expansion during the cycling process, the graphite interlayer structure is damaged, resulting in a decrease in cycling performance. When the B / A ratio is above the upper limit, the proportion of micropores is relatively small, the kinetic performance is poor, and slight lithium plating occurs during the cycling process, resulting in a decrease in cycling performance.
[0185] As can be seen from the comparative examples, when the upper layer thickness is too high, although it can improve the wettability of the electrode, the expansion of the electrode causes the active material to peel off from the current collector, resulting in a decrease in cycle performance. When the upper layer thickness is too low, the wettability is poor, which leads to increased polarization inside the cell and lithium plating, resulting in a decrease in cycle performance.
[0186] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0187] The above-described embodiments are merely illustrative of several implementation methods of the present invention, facilitating a detailed understanding of the technical solutions of the present invention, but should not be construed as limiting the scope of protection of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. It should be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided by the present invention through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this invention patent should be determined by the content of the appended claims, and the specification can be used to interpret the content of the claims.
Claims
1. A negative electrode sheet, characterized in that, include: The negative electrode current collector and a first negative electrode active layer and a second negative electrode active layer are sequentially disposed on the surface of the negative electrode current collector. Both the first negative electrode active layer and the second negative electrode active layer include a negative electrode active material. The negative electrode active material includes mesopores with a pore size of 2nm to 50nm and macropores with a pore size of 100nm to 200nm. In the negative electrode active material of the first negative electrode active layer, the total volume percentage of the mesopores is A1, and the total volume percentage of the macropores is B1, satisfying: 4.9≤B1 / A1≤5; In the negative electrode active material of the second negative electrode active layer, the total volume percentage of the mesopores is A2, and the total volume percentage of the macropores is B2, satisfying: 3.2≤B2 / A2≤3.3; The thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 1:(0.4~0.9).
2. The negative electrode sheet according to claim 1, characterized in that, B1 / A1 is 4.91, and B2 / A2 is 3.
29.
3. The negative electrode sheet according to claim 1, characterized in that, The specific surface area of the negative electrode active material is 1.0 m². 2 / g~2.0m 2 / g.
4. The negative electrode sheet according to any one of claims 1 to 3, characterized in that, The negative electrode active material is selected from one or a combination of graphite, soft carbon, hard carbon and silicon compounds.
5. The negative electrode sheet according to any one of claims 1 to 3, characterized in that, The sulfur content of the negative electrode active material is below 5 wt%.
6. The negative electrode sheet according to claim 5, characterized in that, The sulfur content of the negative electrode active material is 1wt%~5wt%.
7. The negative electrode sheet according to claim 6, characterized in that, The sulfur content in the negative electrode active material of the first negative electrode active layer is 4.3 wt%.
8. The negative electrode sheet according to claim 6, characterized in that, The sulfur content in the negative electrode active material of the second negative electrode active layer is 2.6 wt%.
9. An energy storage device, characterized in that, Includes the negative electrode sheet as described in any one of claims 1 to 8.
10. An electrical appliance, characterized in that, The device includes the energy storage device of claim 9, wherein the energy storage device supplies power to the electrical equipment.
Citation Information
Patent Citations
Preparation method of hierarchical porous carbon aerogel for lithium ion battery negative electrode
CN111099574A
Negative pole piece and lithium ion battery
CN115224237A
Negative pole piece, preparation method thereof and secondary battery
CN115295764A
Battery and electric device
CN116093249A