Method of manufacturing a brake band, method of manufacturing a brake disc, brake disc and brake band

By using a brake band preform made of porous ceramic material and infiltrating it with aluminum alloy to form an aluminum metal matrix composite material, the problem of easy local deterioration of aluminum brake discs during friction is solved, and a high-strength, wear-resistant and economically produced aluminum brake disc is achieved.

CN117337364BActive Publication Date: 2026-11-20FRENI BREMBO SPA +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280016988.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-25
Filing Date
2022-02-22
Publication Date
2026-11-20
Estimated Expiration
2042-02-22

AI Technical Summary

Technical Problem

Existing aluminum brake discs are prone to localized deterioration during friction and are difficult to simultaneously possess the same mechanical strength and wear resistance as steel or gray cast iron discs. In addition, the production process is complex and costly.

Method used

Brake band preforms made of porous ceramic materials are formed by permeating liquid or semi-solid aluminum alloy to create an aluminum metal matrix composite material. The brake band includes a silicon carbide-reinforced central layer and a silicon-permeated outer layer, avoiding direct contact and simplifying the production process.

Benefits of technology

It achieves stability and mechanical strength of aluminum brake discs during friction, avoids localized deterioration, and has wear resistance and corrosion resistance comparable to steel discs or gray cast iron discs, while reducing production complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117337364B_ABST
    Figure CN117337364B_ABST
Patent Text Reader

Abstract

A method for manufacturing a brake band for a brake disc of a disc brake, the method comprising the steps of: a) preparing a mould having an internal cavity comprising a first portion having a shape corresponding to the shape of the brake band to be manufactured; b) preparing a band preform comprising a central layer, an upper outer layer and a lower outer layer, said upper and lower outer layers being arranged in opposite manner and on opposite sides of the central layer; c) placing the band preform inside the mould, at the first portion of the internal cavity; and d) injecting a liquid or semi-solid aluminium alloy inside the entire internal cavity of the mould, to infiltrate the central layer of the band preform made of porous ceramic material with the aluminium alloy only. The present application also comprises a method for manufacturing a brake disc, a brake disc and a brake band for a brake disc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a brake band for a brake disc, a method for manufacturing a brake disc, a brake disc manufactured by the above method, and a brake band for a brake disc. Background Technology

[0002] The brake disc of a vehicle's disc braking system comprises a ring-shaped structure or brake band and includes a central fixing element called a bell, through which the disc is attached to a rotating part of the vehicle suspension, such as a wheel hub. The brake band is provided with two opposing braking surfaces adapted to cooperate with friction elements (brake pads), which are housed in at least one gripping body that spans the brake band arrangement and is integral with a non-rotating component of the vehicle suspension. The controlled interaction between the two opposing brake pads and the two opposing braking surfaces of the brake band induces braking through friction, thereby allowing the vehicle to decelerate or stop.

[0003] Brake discs are typically made of gray cast iron or steel. In fact, these materials allow for good braking performance (especially in limiting wear) at a relatively low cost. Discs made of carbon or carbon ceramic materials offer even higher performance, but at a higher cost.

[0004] As an alternative to gray cast iron or steel discs, discs made of aluminum have been proposed to reduce disc weight. Aluminum discs are equipped with a protective coating. This coating serves two purposes: firstly, to reduce wear on the disc and thus ensure performance similar to cast iron discs; and secondly, to protect the aluminum base from the temperatures generated during braking, which are well above the softening temperature of aluminum (200°C to 400°C).

[0005] However, the protective coatings currently available and applied to aluminum discs, while providing abrasion resistance, are often prone to peeling, causing the coating to separate from the disc. This complicates the disc manufacturing process. In fact, the disc must undergo surface finishing and must also be prepared for attachment to the bell-shaped component.

[0006] It is clear from the above that aluminum or aluminum alloy discs with protective coatings cannot yet completely replace steel or gray cast iron discs.

[0007] However, aluminum has a lower density than steel and gray cast iron, making it a highly attractive potential alternative to steel and gray cast iron in the braking systems industry.

[0008] Therefore, in this field, there is a need for aluminum-based brake discs that can take advantage of the special operating properties of aluminum (primarily due to its low density) while achieving mechanical strength and wear characteristics at least comparable to steel or gray cast iron discs. Furthermore, these discs need to be manufactured using the simplest and most economical production process possible.

[0009] WO2019 / 123222A1 describes a method for manufacturing an aluminum disc using a porous ceramic preform infiltrated with molten aluminum (liquid or semi-solid). Unfortunately, the disc obtained in this way provides direct contact between the brake pad and the aluminum-based metal matrix, which can lead to potential localized degradation on the disc at points where the aluminum is overheated to its melting point due to friction. Summary of the Invention

[0010] Therefore, the industry urgently needs aluminum-based brake discs that do not deteriorate locally, and that can take advantage of the special operating characteristics of aluminum (mainly its low density), while also achieving mechanical strength and wear resistance comparable to steel or gray cast iron discs, and can be manufactured through the simplest and most economical production process possible.

[0011] In addition to the above requirements, the brake discs also need to have higher corrosion resistance than cast iron or steel discs, and lower emissions of polluting metal particles.

[0012] The above requirements are met by the method for manufacturing a brake band for a brake disc, the method for manufacturing a brake disc, the brake disc for a disc brake, and the brake band according to the present invention.

[0013] The method for manufacturing a brake band according to the present invention includes the following steps: a) Prepare a mold having an inner cavity, the inner cavity including a first part having a shape corresponding to the shape of the brake band to be manufactured; b) Prepare a preform comprising a central layer, an upper outer layer, and a lower outer layer, wherein the central layer is made of a porous ceramic material containing silicon carbide (SiC); the upper and lower outer layers are made of a porous ceramic material containing silicon carbide (SiC) and permeated with silicon (SiC+Si); the upper and lower outer layers are arranged in opposite directions and located on opposite sides of the central layer. c) Placing the preformed part inside the mold, at the first portion of the cavity; and; d) Injecting liquid or semi-solid aluminum alloy into the entire interior cavity of a mold to permeate only the central layer of the preform made of porous ceramic material with the aluminum alloy, thereby obtaining an aluminum matrix composite material reinforced by the central layer at a first portion, which partially defines the brake band to be manufactured.

[0014] Advantageously, in order to manufacture a preformed part, the method includes the following steps: a1) Prepare a rough preform made of a porous ceramic material containing silicon carbide (SiC), the rough preform having an upper face and an opposite lower face connected by sidewalls that extend incidentally to the upper and lower faces, for example, the rough preform having a cylindrical geometry or a hollow cylindrical geometry (as shown in the figures), wherein the lower and upper faces are the bottom surfaces of the cylindrical shape and the sidewalls are the side surfaces of the cylindrical shape; a2) Deposit at least partially a masking layer on the sidewalls, the masking layer being adapted to prevent silicon (Si) from penetrating through the sidewalls in the subsequent permeation step a3); a3) A rough preform is penetrated to a given depth by passing silicon (Si) through the upper and lower surfaces to obtain a strip preform comprising a silicon-free central layer, a silicon-permeable (SiC+Si) upper outer layer, and a silicon-permeable (SiC+Si) lower outer layer, the upper and lower outer layers being arranged in opposite directions and located on opposite sides of the central layer.

[0015] Preferably, in step a2), the step of depositing the masking layer includes depositing a layer of boron nitride (BN).

[0016] Advantageously, in step a2), the deposition of the masking layer is applied to the entire sidewall, but not to the upper and lower surfaces of the rough preform.

[0017] Preferably, in step a3), the rough preform is placed in a crucible, a predetermined amount of silicon (Si) powder is added to the crucible, and the rough preform is heated to a temperature above 1414°C at atmospheric pressure and in an inert environment for at least 5 minutes. Preferably, the rough preform is heated to a temperature above 1414°C at atmospheric pressure and in an argon environment for at least 5 minutes.

[0018] Preferably, the rough preform is heated to a temperature between 1500°C and 1650°C for a period between 15 minutes and 90 minutes.

[0019] Even more preferably, the rough preform is heated to a temperature between 1550°C and 1600°C for a period of time between 30 minutes and 60 minutes.

[0020] Preferably, the rough preform has a thickness between 4 mm and 40 mm, including the extreme values; even more preferably, the rough preform has a thickness between 10 mm and 20 mm, which is the distance between the upper and lower surfaces. The predetermined amount of silicon is determined according to the size of the preform to obtain a thickness of at most 0.5 mm to 3 mm for the upper outer layer and / or the lower outer layer, preferably at most about 2 mm for the upper outer layer and / or the lower outer layer. Preferably, step d) of placing the aluminum alloy inside the mold is performed using semi-solid or liquid infiltration technology, extrusion casting technology, or die casting using liquid aluminum.

[0021] In the case of gravity infiltration, infiltration is preferably carried out in an inert environment, such as a nitrogen atmosphere.

[0022] Advantageously, the rough preform is obtained by sequentially molding, dewaxing, and sintering a large number of ceramic material particles coated with a polymer-bonded composition.

[0023] Preferably, sintering is carried out in two separate sintering cycles, wherein the first sintering cycle is carried out at a temperature not lower than 1600°C and the second sintering cycle is carried out at a temperature not lower than 2000°C, both the first and second sintering cycles are carried out in an inert environment, preferably the first sintering cycle is carried out at a temperature of about 1800°C, and preferably the second sintering cycle is carried out at a temperature in the range of 2100°C to 2200°C.

[0024] Furthermore, preferably, in step d), the mold is closed on the upper and lower outer layers of the preform, so as to prevent aluminum from penetrating on the upper and lower outer layers during the injection of aluminum into the mold, so that the outer braking surface of the brake band is free of aluminum.

[0025] The method for manufacturing a brake disc including a brake band and a bell-shaped element according to the present invention includes the following steps: a) Prepare a mold having an inner cavity, the inner cavity comprising a first part and a second part, the first part having a shape corresponding to the shape of the brake band of the brake disc to be manufactured, and the second part having a shape corresponding to the shape of the bell-shaped part of the brake disc to be manufactured, wherein the first part and the second part of the inner cavity are connected to each other. b) Prepare a preform comprising a core layer, an upper outer layer, and a lower outer layer. The core layer is made of a porous ceramic material containing silicon carbide (SiC). The upper and lower outer layers are made of a porous ceramic material containing silicon carbide (SiC) and permeated with silicon (SiC+Si). The upper and lower outer layers are arranged in opposite directions and located on opposite sides of the central layer. c) Place the preformed part inside the mold, at the first part of the inner cavity; d) Injecting liquid or semi-solid aluminum alloy into the entire cavity of a mold such that: the aluminum alloy is used to permeate only the central layer of a preform made of porous ceramic material to obtain a first portion of an aluminum matrix composite material reinforced by the central layer, which partially defines the brake band of the brake disc to be manufactured; and the aluminum alloy is used to fill a second portion to obtain an aluminum alloy fusion body that is integrally connected to the brake band made of the metal matrix composite material and defines the bell-shaped element of the brake disc to be manufactured.

[0026] The disc brake according to the invention includes a brake band and a bell-shaped element connected to the brake band.

[0027] Preferably, in an advantageous manner, the bell-shaped element is integrally connected with the brake band, and the bell-shaped element comprises an aluminum alloy co-cast with the metal matrix of the composite material forming the brake band.

[0028] According to the present invention, the brake band includes a central portion made of an aluminum-matrix composite material reinforced with a silicon carbide (SiC) ceramic material. The composite material is obtained by infiltrating a central layer of a rough preform made of a porous silicon carbide (SiC) ceramic material with an aluminum alloy. The brake band also includes an upper portion connected to the central portion. The upper portion is made of a porous ceramic material containing silicon carbide (SiC) and infiltrated with silicon (to form SiC+Si), and the upper portion covers the central portion on one side. The brake band also includes a lower portion connected to the central portion on the opposite side—that is, on the side opposite to the upper portion. The lower portion is also made of a porous ceramic material containing silicon carbide (SiC) and infiltrated with silicon (to form SiC+Si). Furthermore, the lower portion covers the central portion on another side—that is, on the side opposite to the upper portion.

[0029] Preferably, the upper and lower portions have a thickness between 2 mm and 4 mm.

[0030] Preferably, the aluminum alloy matrix has a uniformly distributed structure within the composite material. Attached Figure Description

[0031] Further features and advantages of the invention will become more apparent from the following detailed description of preferred, non-limiting embodiments of the invention, in the accompanying drawings: - Figure 1 This is a perspective view of a brake disc according to an embodiment of the present invention; - Figure 2 The steps of a method for manufacturing a brake band for a brake disc according to an embodiment of the present invention are illustrated schematically. - Figure 3 This is a perspective view of a preform according to an embodiment of the present invention; - Figure 4 , Figure 5 , Figure 6 and Figure 7 Each step in a method of manufacturing a brake disc according to an embodiment of the present invention is shown, wherein these steps are arranged in order from... Figures 4 to 7 The order is as follows; in particular, Figure 7 The image shows a cross-section of the rough brake disc taken on the diametrical plane; the rough brake disc is immediately following... Figure 1 The intermediate product shown is the final brake disc obtained by removing unnecessary portions of the rough brake disc through subsequent processing.

[0032] Elements or parts thereof that are common to the embodiments described below will be indicated by the same reference numerals. Detailed Implementation

[0033] Referring to the foregoing figures, reference numeral 1 generally indicates a brake disc according to the invention.

[0034] According to the general embodiment of the invention shown in the accompanying drawings, the brake disc 1 includes a brake band 2 having two opposite external brake surfaces 2a and 2b, each of the two external brake surfaces 2a and 2b at least partially defining one of the two main faces of the disc.

[0035] The brake disc 1 also includes a bell-shaped element 3, which is connected to the brake band 2.

[0036] According to a first aspect of the invention, the brake band 2 includes a central portion 200' made of an aluminum-based metal matrix composite material reinforced with a ceramic material containing silicon carbide (SiC). The composite material is obtained by infiltrating a central layer of a rough preform 20' made of a porous ceramic material containing silicon carbide (SiC) with an aluminum alloy.

[0037] The aforementioned composite material belongs to the category of composite materials known in the industry as MMC (metal matrix composite).

[0038] Using the aluminum-containing MMC composite material in brake band 2 allows for even greater mechanical and chemical physical properties relative to aluminum, and simultaneously (relative to simple fusion of aluminum or aluminum alloys) added functional properties suitable for heavy-duty applications, such as those required in braking systems, without the need for a protective coating on the brake surface.

[0039] Furthermore, the brake band 2 also includes an upper portion 201', which is integrally connected to the central portion 200'. The upper portion 201' is obtained by silicon infiltration of a single initial rough preform 20' to a given depth D1, which determines the thickness of the upper portion 201'. Therefore, the upper portion 201' is made of a porous ceramic material containing silicon carbide (SiC) and infiltrated with silicon (SiC+Si). Additionally, the upper portion 201' covers one side of the central portion 200', ensuring that the central portion 200' does not contact the brake pad on said side when the brake disc is mounted on a disc brake.

[0040] In other words, the upper portion 201' is the region of the initial rough preform 20' in which silicon has been penetrated to a given depth.

[0041] Additionally, the brake band 2 includes a lower portion 202', which is integrally connected to the central portion 200'. The lower portion 202' is obtained by permeating a single rough preform 20' with silicon to a given depth D2, which determines the thickness of the lower portion 202'; preferably, this depth D2 is equal to D1. Therefore, the lower portion 202' is also made of a porous ceramic material containing silicon carbide (SiC) and permeated with silicon (SiC+Si). Furthermore, the lower portion 202' covers the central portion 200' on the other side—the side opposite to the upper portion 201'. In this way, the central portion 200' is positioned between the upper portion 201' and the lower portion 202'. Specifically, the outer braking surfaces 2a and 2b of the brake band 2 are the outermost surfaces of the upper portion 201' and the lower portion 202', respectively, and these outer braking surfaces 2a and 2b are not connected to the central portion 200' in the sense that they are integral.

[0042] Clearly, the central portion 200' is positioned between the upper portion 201' and the lower portion 202' in the axial direction of the brake band—that is, in the direction of the rotation axis of the brake band—when forming part of the brake disc 1. In other words, the central portion 200' is positioned between the upper portion 201' and the lower portion 202' in the direction of the braking force (i.e., pressure) acting on the external brake surfaces 2a and 2b through the friction element (brake caliper pad).

[0043] Preferably, the central portion 200', the upper portion 201', and the lower portion 202'—in the sense that each portion extends radially into the central band 2 as a whole—are respectively the central band, the upper band, and the lower band. In other words, the central portion 200', the upper portion 201', and the lower portion 202' each have an area in a plane perpendicular to the axial direction that is approximately equal to the area occupied by the entire brake band 2, for example, a disc-shaped or annular crown-shaped area.

[0044] In other words, the brake band 2 is obtained by penetrating silicon to a given depth (upper portion 201') and a given depth (lower portion 202') into a single rough preform 20'. Clearly, the penetration depth is much smaller than the total thickness of the preform 20', i.e., the penetration depth is much smaller than the height of the sidewall.

[0045] According to an advantageous embodiment, the upper portion 201' and the lower portion 202' have a thickness of 2 mm to 4 mm, preferably 3 mm. This allows for a suitable trade-off between stiffness, wear resistance, and weight.

[0046] Compared to brake bands made solely of aluminum or one type of aluminum alloy, the presence of a ceramic reinforcement in the central portion 200', as well as the upper portion 201' and lower portion 202, allows for greater hardness, greater stiffness, a higher coefficient of friction, and greater wear resistance. All these properties make this brake band suitable for use with brake discs.

[0047] In this way, brake bands with the advantageous properties of aluminum (especially its lower density compared to steel and cast iron) can be formed, while avoiding the need for a protective coating on the brake surface and the limitations and inconveniences of brake bands in production and operation.

[0048] Preferably, the aforementioned ceramic material used to manufacture the reinforcing material is silicon carbide.

[0049] As will be discussed later in the description, the MMC composite material forming the central portion 200' is obtained by infiltrating a preform of porous ceramic material with an aluminum alloy. Advantageously, the ceramic materials listed above, including silicon carbide, can withstand the infiltration step through molten metal without altering the chemical and physical structure of the ceramic material, and without causing any degree of damage to the ceramic material macroscopically or microscopically. Therefore, ceramic materials are also particularly suitable for preparing the aforementioned composite material.

[0050] Preferably, the aluminum alloy is selected from known aluminum alloys used for casting, or from aluminum alloys containing at least magnesium, manganese or silicon.

[0051] Advantageously, the aluminum alloy matrix has a uniformly distributed structure within the composite material. As will be discussed below, this can be achieved by permeating a preform made of porous ceramic material with uniform porosity throughout its volume using the aluminum alloy. Due to the permeation process, the aluminum alloy permeates the pores of the ceramic material, thereby forming a uniform structure.

[0052] According to another aspect of the invention, the brake disc 1 is provided with a bell-shaped member 3 connected integrally with the brake band 2, and the brake disc 1 comprises an aluminum alloy co-cast with the metal matrix of the composite material forming the brake band 2.

[0053] As will be discussed in the description below, the bell-shaped part is preferably obtained in the same mold, wherein the same aluminum alloy is used to infiltrate the preform made of ceramic material. In this way, the formation of the composite material and the fusion of the bell-shaped part are achieved in the same operating step, thereby realizing a complete bond between the two materials.

[0054] Co-casting the bell-shaped components with the brake band allows for a significant simplification of the production process. In effect, this eliminates the need for dedicated production lines for the bell-shaped components and assembly lines for assembling them onto the band.

[0055] The combination of the two basic aspects of the present invention makes it possible to obtain an aluminum-based brake disc that, on the one hand, can take advantage of the special operating characteristics derived from aluminum (first and foremost, its low density), and on the other hand, can have mechanical and wear-resistant properties comparable to those of steel or gray cast iron discs, and can be manufactured through the simplest and most economical production process possible.

[0056] For the sake of simplicity, the brake band 2 and brake disc 1 will now be described in conjunction with the corresponding methods for manufacturing the brake band 2 and brake disc 1 according to the invention. The brake disc 1 is preferably, but not necessarily, manufactured using the method according to the invention described below.

[0057] According to a general embodiment of the method of the present invention, the method for manufacturing a brake disc 1 includes the following first operation step a): preparing a mold 10 having an inner cavity 11, the inner cavity 11 including a first part 11a and a second part 11b, the first part 11a having a shape corresponding to the shape of the brake band 2 of the brake disc 1 to be manufactured, and the second part 11b having a shape corresponding to the shape of the bell-shaped member 3 of the brake disc 1 to be manufactured.

[0058] The first part 11a and the second part 11b of the inner cavity 11 are connected to each other, as shown below. Figure 5 and Figure 6 As shown, Figure 5 and Figure 6 An example of a mold that can be used in accordance with the method according to the invention is shown schematically.

[0059] Advantageously, such as Figure 4 and Figure 5 As shown, the mold includes one or more inlet openings 13 for directly injecting aluminum alloy into a second portion of the cavity 11 of the mold 10. The inlet openings 13 extend coaxially with a circumferential extension of the second portion 11b, which has a shape corresponding to the shape of the bell-shaped element 3 of the brake disc 1 to be manufactured. Therefore, in terms of operability, aluminum alloy can be injected through the inlet openings 13, and the aluminum alloy subsequently propagates from the inlet openings 13 into the first portion 11a.

[0060] The method includes the following second operational step b): preparing a preform 20, which includes an upper outer layer 201, a lower outer layer 202, and a central layer 200 made of a porous ceramic material containing silicon carbide (SiC). The upper outer layer 201 and the lower outer layer 202 are made of a porous ceramic material containing silicon carbide (SiC) and permeated with silicon (SiC+Si). Furthermore, the upper outer layer 201 and the lower outer layer 202 are arranged in opposite directions and located on opposite sides of the central layer 200. In other words, the preform 20 is a multi-layer preform, wherein the lower outer layer 201, the central layer 200, and the upper outer layer 201 are arranged sequentially, one above the other.

[0061] As will be better explained below, preferably, the lower outer layer 201, the central layer 200 and the upper outer layer 201 are obtained by permeation of a single rough preform 20' above and below.

[0062] Advantageously, the silicon infiltration into the upper outer layer 201 and the lower outer layer 202 occupies space in the porous ceramic material, thereby preventing aluminum from migrating and infiltrating into the upper outer layer 201 and the lower outer layer 202 during the subsequent aluminum alloy infiltration step. In this way, aluminum remains confined to the central layer 200.

[0063] Preferably, the preform 20 has a shape that is substantially the same as the shape of the brake band 2 of the brake disc 1 to be manufactured. For example, the preform 20 is preferably a disc-shaped part, and more preferably, the preform 20 is a disc-shaped part with a central circular through hole.

[0064] The method also includes the following additional operational steps: -c) Arranging the aforementioned preformed component 20 within the mold, at the first portion 11a of the inner cavity 11; and -d) Inject liquid or semi-solid aluminum alloy into the entire inner cavity 11 of the mold 10.

[0065] An aluminum alloy is injected to penetrate only the central layer 200 of the preform 20, thereby obtaining an aluminum matrix composite material reinforced by the central layer 200 at the first portion 11a, which partially defines the brake band 2 of the brake disc to be manufactured. This is done by filling the second portion 11b with the aluminum alloy, thereby obtaining an aluminum alloy fusion body that is integrally connected to the brake band 2 made of the metal matrix composite material and defines the bell-shaped element 3 of the brake disc 1 to be manufactured.

[0066] According to the general embodiment, except that the mold 10 is shaped only for manufacturing the brake band 2 and not for manufacturing the bell-shaped element 3, the method for manufacturing the brake band 2 of the brake disc 1 includes a series of steps similar to those for manufacturing the brake disc. Therefore, in step a), compared to the steps of the method for manufacturing the brake disc, the mold does not include a second portion 11b having a shape corresponding to the shape of the bell-shaped element 3 of the brake disc 1 to be manufactured. Furthermore, in step d), compared to the method for manufacturing the brake disc 1, only aluminum alloy infiltration is performed to infiltrate the central layer 200 of the preform 20 with the aforementioned aluminum alloy, thereby obtaining an aluminum-based metal matrix composite material reinforced by the central preform 200 in the first portion 11a, which partially defines the brake band 2 to be manufactured. Clearly, in order to manufacture only the brake band, it is not necessary to provide aluminum alloy to fill the second portion 11b, because it is not necessary to simultaneously manufacture the bell-shaped element 2 of the brake disc by co-fusion. Although the mold used for manufacturing the brake band is not shown in the accompanying drawings, those skilled in the art can clearly and explicitly deduce how the mold 10 described above can be modified so that the mold 10 does not have a second part 11b for manufacturing the bell-shaped part.

[0067] Therefore, in a general embodiment, the method for manufacturing a brake band according to the present invention includes the following first operation step a): preparing a mold 10 having an inner cavity 11, the inner cavity 11 including a first portion 11a having a shape corresponding to the shape of the brake band 2 of the brake disc 1 to be manufactured.

[0068] Furthermore, in this case, the mold includes one or more inlet openings 13 for injecting aluminum alloy directly into a second part of the cavity 11 of the mold 10.

[0069] The method includes the following second operational step b): preparing a preform 20, which includes an upper outer layer 201, a lower outer layer 202, and a central layer 200 made of a porous ceramic material containing silicon carbide (SiC). The upper outer layer 201 and the lower outer layer 202 are made of a porous ceramic material containing silicon carbide (SiC) and permeated with silicon (SiC+Si). The upper outer layer 201 and the lower outer layer 202 are arranged in opposite directions and located on opposite sides of the central layer 200.

[0070] The method also includes the following additional operational steps: c) Arranging the preformed part 20 inside the mold, at the first portion 11a of the inner cavity 11; and d) Inject liquid or semi-solid aluminum alloy into the entire inner cavity 11 of mold 10.

[0071] An aluminum alloy is injected to penetrate the central layer 200 of the preform 20, thereby obtaining an aluminum matrix composite material reinforced by the central preform 200 at the first portion 11a, which partially defines the brake band 2 to be manufactured.

[0072] Advantageously, in order to manufacture the brake disc 1 and the brake band 2, step b) of injecting aluminum alloy into the mold can be carried out according to any technique suitable for the purpose.

[0073] In particular, step b) can be performed using liquid infiltration technology, squeeze casting technology, gravity infiltration technology, semi-solid infiltration technology, or by die casting using liquid aluminum.

[0074] In the case of gravity infiltration, infiltration is preferably carried out in an inert environment, such as a nitrogen atmosphere.

[0075] The aforementioned penetration techniques are well known to those skilled in the art, and therefore will not be described in detail here.

[0076] Preferably, step b) of injecting the aluminum alloy into the mold is performed using a semi-solid infiltration technique. In fact, it has been found that this technique is more suitable for infiltrating ceramic preforms, resulting in a disc made of MMC material with uniform characteristics throughout its structure at the end of the process, indicating complete infiltration of the preform. This technique is also particularly suitable for forming bell-shaped parts in the same process.

[0077] More specifically, the infiltration at the semi-solid stage occurs at a temperature between the liquidus and solidus of the aluminum alloy used, that is, when the alloy is in a semi-solid state. Due to the low viscosity of the semi-solid material, the injection process into the mold and the infiltration process proceed smoothly and with low turbulence.

[0078] Of particular advantage is that the presence of the silicon-permeated upper and lower outer bands prevents aluminum from permeating the upper and lower outer bands. The result is a pair of opposing brake surfaces 2a, 2b that are particularly suitable for use in brake discs because these opposing brake surfaces 2a, 2b are free of aluminum and have an improved coefficient of friction compared to prior art aluminum discs.

[0079] According to an advantageous embodiment, both the method for manufacturing the brake band and the method for manufacturing the brake disc include a series of operational steps performed prior to step b), such as in Figure 2The diagram is schematically shown. Specifically, the series of operational steps envisions the following initial operational step a1): preparing a rough preform 20' made of a porous ceramic material comprising silicon carbide (SiC). The rough preform 20' includes an upper surface 20a and an opposite lower surface 20b, which are connected by a sidewall 20c extending in association with the upper surface 20a and the lower surface 20b, preferably perpendicular to the upper surface 20a and the lower surface 20b. Preferably, the rough preform 20' has a central through-hole 5 and therefore an inner sidewall 20d opposite to the sidewall 20c.

[0080] Preferably, the rough preform 20' has a shape that is substantially the same as the shape of the brake band 2 of the brake disc 1 to be manufactured.

[0081] Additionally, the series of operational steps provides the following subsequent operational step a2): depositing at least partially a masking layer 21 on the sidewall 20c, the masking layer 21 being adapted to prevent silicon (Si) from penetrating through the sidewall 20c in the subsequent penetration step a3).

[0082] The use of silicon to permeate the wall 20c prevents aluminum alloy from entering the preform during the aluminum alloy permeation step.

[0083] Preferably, in step a2), the step of depositing the masking layer 21 includes depositing a layer of boron nitride (BN).

[0084] According to an advantageous variant, the deposition of the masking layer 21 is applied to the entire sidewall 20c, but not to the upper surface 20a and lower surface 20b of the rough preform 20'.

[0085] According to another variation, the deposition of the masking layer 21 is applied to the entire inner wall 20d, but not to the upper surface 20a and lower surface 20b of the rough preform 20'.

[0086] According to another variation, the deposition of the masking layer 21 is applied to the entire inner wall 20d and side wall 20c.

[0087] Due to the masking layer 21, it is advantageously ensured that silicon does not permeate through the sidewalls 20c and / or 20d. Depending on how the mold 10 is manufactured, this allows aluminum to permeate into the central layer 200 through the sidewalls 20c and / or 20d when the masking layer 21 is removed.

[0088] The series of operational steps provides the following additional operational step a3): The rough preform 20' is permeated with silicon (Si) through the upper surface 20a and the lower surface 20b to a specified depth to obtain a strip preform 20 comprising an unpermeated intermediate layer 200, a silicon-permeated (SiC+Si) upper outer layer 201, and a silicon-permeated (SiC+Si) lower outer layer 202. The upper outer layer 201 and the lower outer layer 202 are arranged opposite each other on opposite sides of the intermediate layer 200.

[0089] Preferably, in step a3), the rough preform 20' is placed in a crucible, a predetermined amount of silicon (Si) powder is added to the crucible, and the rough preform 20' is heated to a temperature above 1420°C and sustained for at least 5 minutes at atmospheric pressure and in an inert environment, preferably in an argon environment.

[0090] This process can be accomplished using an industrial furnace of appropriate size. Additionally, preferably, after the infiltration process and before proceeding with the subsequent steps described below, the upper and lower external preforms are leveled (ground).

[0091] According to one embodiment of the method, the rough preform 20' is heated to a temperature in the range of 1500°C to 1650°C for a period of 15 minutes to 90 minutes.

[0092] More advantageously, the rough preform 20' is heated to a temperature in the range of 1550°C to 1600°C for a period of 30 to 60 minutes, thereby allowing for sufficient and uniform silicon penetration for a thickness suitable for manufacturing the brake disc, and surprisingly, with a more uniform propagation front.

[0093] Preferably, the rough preform 20' has a thickness between 4 mm and 40 mm including the end value; even more preferably, the rough preform 20' has a thickness between 10 mm and 20 mm, the thickness being the distance between the upper surface 20a and the lower surface 20b, and the predetermined amount of silicon depends on the diameter of the preform.

[0094] For example, the volume of the silicon-permeable layer can be calculated as: Vtot = π(R² - r²)h, where radii R and r are the outer radius R and inner radius r of the annular crown described by the rough preform 20', respectively, and h is the desired silicon permeation depth. The apparent density is defined as: Da = Mass of porous product / Total volume of porous product (including voids) And the porosity is limited to: P=1-D 固体 / Da, Wherein, the solid density D 固体 It is the density of non-porous products. The pre-ordered quantity of silicon (Msi) can be calculated as follows: Msi = Silicon Volume Silicon density, Where, silicon volume = Vtot P.

[0095] In this way, given a preform with a certain porosity and volume for which a silicon-infiltrated layer is to be formed, the quality of the silicon to be used can be determined a priori.

[0096] According to a preferred embodiment of the method for manufacturing the brake band 2 or the method for manufacturing the brake disc 1, the rough preform 20' made of porous ceramic material is obtained by performing the following sequential steps on a large number of ceramic material particles coated with a polymer bonding composition: molding, debonding (or dewaxing) and sintering.

[0097] Advantageously, the aforementioned ceramic material particles are powder particles referred to as "ready-to-press." This commercially available powder, together with the pressing technology, allows for the production of "net-shape molded" products without the need for any other ingredients or additives besides the powder itself.

[0098] Preferably, the ceramic material used to form the particles is silicon carbide.

[0099] Preferably, the polymeric composition used to coat the ceramic material particles is selected from thermoplastic polymers and thermosetting polymers.

[0100] Preferably, the molding of a large number of ceramic material particles is accomplished uniaxially or isostatically or using any other technique that allows for the production of preforms of this size and shape.

[0101] At the end of the molding process, aggregates of the aforementioned ceramic material particles are obtained, which are linked by ceramic microstructures promoted by a corresponding coating of the polymer-bonded composition. The aggregates contain organic residues from the particle coating. These organic residues are removed in a debonding (or dewaxing) step.

[0102] Advantageously, the debinding is carried out under airflow conditions at a temperature below 700°C until the organic phase present in a large number of ceramic material particles after molding is completely eliminated.

[0103] According to the variant, debinding occurs under inert environmental conditions.

[0104] At the end of the debinding step, a green body consisting essentially of only ceramic material is obtained. This green body is then subjected to a sintering stage, which transforms it into a continuous structure by forming bridges that connect the individual ceramic particles. This produces a body exhibiting uniform properties throughout the structure.

[0105] Preferably, sintering is carried out in two separate sintering cycles. The first sintering cycle is carried out at a temperature of not less than 1600°C, preferably about 1800°C, and the second sintering cycle is carried out at a temperature of not less than 2000°C, preferably in the range of 2100°C to 2200°C, and both the first and second sintering cycles are carried out in an inert environment.

[0106] Advantageously, the resulting rough preform 20' made of porous ceramic material has a uniform density and porosity distribution throughout its entire volume. This characteristic makes the preform suitable for manufacturing a uniformly distributed aluminum alloy matrix after infiltration with the aluminum alloy.

[0107] According to a specific embodiment, the method for manufacturing the brake band specifies that the rough preform 20' has a density of 40%. In this embodiment, a 13 mm high rough preform is placed in a graphite crucible, and silicon powder is present on the upper and lower outer surfaces of the rough preform, the weight of which is between 10 and 20 grams, and a boron nitride masking layer 21 is present on the sidewall 2c. The preform is thermally cyclicated in a furnace to allow silicon to fuse and permeate at atmospheric pressure and in flowing argon gas at a temperature between 1430°C and 1550°C for a duration between 1 hour and 3 hours. Advantageously, at a temperature of 1550°C, a time of 60 minutes, and a silicon content of 14 grams, the average thickness of the upper and lower outer layers obtained is between 2 mm and 3 mm (minimum thickness of 2 mm, preferably maximum thickness of 2.6 mm).

[0108] Obviously, when the preform 20 is obtained as described above, the central layer 200 corresponds to the central portion 200' of the brake band 20, and the upper outer layer 201 and the lower outer layer 202 correspond to the upper outer band 201' and the lower outer band 202' of the brake band 20, respectively.

[0109] Advantageously, in the method according to the invention, such as in... Figures 5 to 6In step d) as seen in the diagram, the mold is closed on the upper outer layer 201 and the lower outer layer 202, preventing aluminum from seeping into the upper outer layer 201 and the lower outer layer 202 during the injection of aluminum into the mold, thereby ensuring that the outer braking surfaces 2a and 2b of the disc are free of aluminum. In other words, it prevents the aluminum alloy from flowing and spreading on the upper outer layer 201 and the lower outer layer 202, i.e., on the sides of each outer layer 201 and 202 that are not connected to the central layer 200.

[0110] As can be understood from the description already provided, the brake band, brake disc, and method for manufacturing the brake disc and brake band according to the invention enable the overcoming of the deficiencies present in the prior art.

[0111] In fact, by placing two external brake bands made of ceramic material between the brake pads and a central portion made of a composite material with a metal matrix—which is made of MMC (metal matrix composite) aluminum alloy—the brake bands and brake discs of this invention allow for the reduction—if not elimination—of problems associated with localized degradation due to overheating of aluminum found in the prior art, as discovered in the prior art. Furthermore, the external brake bands allow for the simultaneous generation of greater braking force due to the pads being attached to a material with a higher coefficient of friction. Simultaneously, high efficiency, simplicity, low implementation costs, and reduced corrosion are ensured. Reduced corrosion is particularly advantageous for electric vehicles, where the introduction of regenerative braking involves the discontinuous use of disc brakes, which can lead to corrosion.

[0112] To meet possible and specific needs, those skilled in the art can make various modifications and variations to the present invention described above, all of which are included within the scope of the present invention as defined in the appended claims.

Claims

1. A method for manufacturing a brake band (2) for a brake disc (1) of a disc brake, the method comprising the following steps: a) Prepare a mold (10) having an inner cavity (11) including a first part (11a) having a shape corresponding to the shape of the brake band (2) to be manufactured; b) Prepare a preform (20) comprising a central layer (200), an upper outer layer (201) and a lower outer layer (202), wherein the central layer (200) is made of a porous ceramic material containing silicon carbide, the upper outer layer (201) and the lower outer layer (202) are made of a porous ceramic material containing silicon carbide and permeated with silicon, and the upper outer layer (201) and the lower outer layer (202) are arranged in opposite directions and located on opposite sides of the central layer (200); c) Placing the preform (20) inside the mold, at the first portion (11a) of the inner cavity (11); and d) Injecting liquid or semi-solid aluminum alloy into the entire interior cavity (11) of the mold (10) to permeate only the central layer (200) of the preform (20) made of porous ceramic material with the aluminum alloy, thereby obtaining an aluminum matrix composite material reinforced by the central layer (200) at the first portion (11a), the aluminum matrix composite material partially defining the brake band (2) to be manufactured.

2. The method according to claim 1, wherein, Prior to step b) of manufacturing the preform (20), the method includes the following steps: a1) Arrange a rough preform (20') made of a porous ceramic material containing silicon carbide, the rough preform (20') having an upper surface (20a) and an opposite lower surface (20b) connected together by a sidewall (20c), the sidewall (20c) extending to be associated with the upper surface (20a) and the lower surface (20b); a2) Deposit at least partially a masking layer (21) on the sidewall (20c), the masking layer (21) being adapted to prevent silicon from penetrating through the sidewall (20c) in the subsequent penetration step a3). a3) The rough preform (20') is penetrated to a given depth by passing silicon through the upper surface (20a) and the lower surface (20b) to obtain the strip preform (20), which includes an unpermeable central layer (200), a silicon-permeable upper outer layer (201) and a silicon-permeable lower outer layer (202), the upper outer layer (201) and the lower outer layer (202) being arranged in opposite directions and located on opposite sides of the central layer (200).

3. The method according to claim 2, wherein, In step a2), the step of depositing the masking layer (21) includes depositing a layer of boron nitride.

4. The method according to claim 2, wherein, In step a2), the deposition of the masking layer (21) is applied to the entire sidewall (20c) but not to the upper surface (20a) and the lower surface (20b) of the rough preform (20').

5. The method according to any one of claims 2 to 4, wherein, In step a3), the rough preform (20') is positioned in a crucible, a predetermined amount of silicon powder is added to the crucible, and the rough preform (20') is heated to a temperature above 1414°C at atmospheric pressure and in an inert environment for at least 5 minutes.

6. The method according to any one of claims 2 to 4, wherein, In step a3), the rough preform (20') is positioned in a crucible, a predetermined amount of silicon powder is added to the crucible, and the rough preform (20') is heated to a temperature above 1414°C at atmospheric pressure and in an argon atmosphere for at least 5 minutes.

7. The method according to claim 5, wherein, The rough preform (20') is heated to a temperature between 1500°C and 1650°C for a period between 15 minutes and 90 minutes.

8. The method according to claim 7, wherein, The rough preform (20') is heated to a temperature between 1550°C and 1600°C for a period between 30 minutes and 60 minutes.

9. The method according to claim 5, wherein, The rough preform (20') has a thickness between 4 mm and 40 mm including an end value, the thickness being the distance between the upper surface (20a) and the lower surface (20b), and the predetermined amount of silicon is a function of the diameter of the rough preform.

10. The method according to any one of claims 1 to 4, wherein, Step d) of introducing the aluminum alloy into the interior of the mold is carried out according to semi-solid or liquid infiltration technology, or according to gravity infiltration technology, or by die casting of liquid aluminum, or according to squeeze casting technology.

11. The method according to any one of claims 2 to 4, wherein, The rough preform (20') is obtained by sequentially molding, dewaxing and sintering a large number of ceramic material particles coated with a polymer-bonded composition.

12. The method according to claim 11, wherein, The sintering is carried out in two separate sintering cycles, wherein the first sintering cycle is carried out at a temperature of not less than 1600°C and the second sintering cycle is carried out at a temperature of not less than 2000°C, both of which are carried out in an inert environment.

13. The method according to claim 11, wherein, The sintering is carried out in two separate sintering cycles, wherein the first sintering cycle is carried out at a temperature of about 1800°C and the second sintering cycle is carried out at a temperature of not less than 2000°C, both of which are carried out in an inert environment.

14. The method according to claim 11, wherein, The sintering is carried out in two separate sintering cycles, wherein the first sintering cycle is carried out at a temperature not lower than 1600°C and the second sintering cycle is carried out at a temperature in the range of 2100°C to 2200°C, both of which are carried out in an inert environment.

15. The method according to claim 11, wherein, The sintering is carried out in two separate sintering cycles, wherein the first sintering cycle is carried out at a temperature of about 1800°C and the second sintering cycle is carried out at a temperature in the range of 2100°C to 2200°C, both of which are carried out in an inert environment.

16. The method according to any one of claims 1 to 4, wherein, In step d), the mold (10) is closed on the upper outer layer (201) and the lower outer layer (202) of the preform (20) to prevent aluminum from penetrating above the upper outer layer (201) and below the lower outer layer (202) during the introduction of aluminum into the mold, so that the outer braking surfaces (2a, 2b) of the brake band (2) are free of aluminum.

17. A method for manufacturing a brake disc, the brake disc comprising a brake band (2) and a bell-shaped element (3), the method comprising the following steps: a) Prepare a mold (10) having an inner cavity (11) comprising a first part (11a) and a second part (11b), the first part (11a) having a shape corresponding to the shape of the brake band (2) of the brake disc (1) to be manufactured, and the second part (11b) having a shape corresponding to the shape of the bell-shaped member (3) of the brake disc (1) to be manufactured, wherein the first part (11a) and the second part (11b) of the inner cavity (11) are in communication with each other; b) Prepare a preform (20) comprising a central layer (200), an upper outer layer (201) and a lower outer layer (202), wherein the central layer (200) is made of a porous ceramic material containing silicon carbide, the upper outer layer (201) and the lower outer layer (202) are made of a porous ceramic material containing silicon carbide and permeated with silicon, and the upper outer layer (201) and the lower outer layer (202) are arranged in opposite directions and located on opposite sides of the central layer (200); c) Placing the preform (20) inside the mold, at the first portion (11a) of the inner cavity (11); and d) Injecting liquid or semi-solid aluminum alloy into the entire interior cavity (11) of the mold (10) such that: the aluminum alloy is used to permeate only the central layer (200) of the preform (20) made of porous ceramic material, thereby obtaining an aluminum metal matrix composite material reinforced by the central layer (200) at the first portion (11a), the aluminum metal matrix composite material partially defining the brake band (2) of the brake disc to be manufactured; and filling the second portion (11b) with the aluminum alloy to obtain an aluminum alloy fusion body that is integrally connected with the brake band (2) made of metal matrix composite material and defines the bell-shaped element (3) of the brake disc (1) to be manufactured.

18. A brake band (2) for a brake disc of a disc brake, said brake band (2) comprising: The central portion (200') is made of an aluminum matrix composite material reinforced with a silicon carbide-containing ceramic material, which is obtained by infiltrating a central layer (200) of a rough preform (20') made of a porous ceramic material containing silicon carbide with an aluminum alloy. An upper portion (201') is connected to the central portion (200'), the upper portion (201') being made of a porous ceramic material containing silicon carbide and permeated with silicon, and the upper portion (201') covering the central portion (200') on one side. The lower portion (202') is connected to the central portion (200') on the opposite side, i.e. on the opposite side relative to the upper portion (201'), the lower portion (202') is made of a porous ceramic material containing silicon carbide and permeated with silicon, and the lower portion (202') covers the central portion (200') on the other side, i.e. on the opposite side relative to the upper portion (201').

19. The brake band (2) according to claim 18, wherein, The upper portion and the lower portion (202') have a thickness between 0.5 mm and 4 mm.

20. A brake disc for a disc brake, the brake disc comprising a brake band (2) according to claim 18 or 19 and a bell-shaped member (3) connected to the brake band (2).

21. The brake disc for a disc brake according to claim 20, wherein, The bell-shaped element (3) is connected to the brake band (2) as a single piece, and the bell-shaped element (3) comprises an aluminum alloy co-cast with the metal matrix of the aluminum metal matrix composite material constituting the brake band (2).

22. The brake disc for a disc brake according to claim 20 or 21, wherein, The aluminum alloy matrix has a uniformly distributed structure within the aluminum metal matrix composite material.

Citation Information

Patent Citations

  • Method for manufacturing a brake disc and brake disc for disc brake

    WO2019123222A1

  • Method for manufacturing a brake disc and brake disc for disc brake

    CN111656040A

  • Ceramic preform and method

    US20160108980A1