Method for reducing aldehyde content in polyether polyols
By using a skeletal nickel catalyst matrix and a modified auxiliary metal to react with hydrogen at low temperature, the problems of high aldehyde content and odor in the synthesis of polyether polyols were solved, and the production of polyether polyols with low aldehyde content and low odor was achieved.
Patent Information
- Application Number
- CN202210745159.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-28
AI Technical Summary
In the existing technology for the synthesis of polyether polyols, the reaction temperature is high and the aldehyde removal effect is poor, resulting in high aldehyde content and unpleasant odor in the product.
A skeletal nickel catalyst matrix and a modified auxiliary metal (such as group IVB, group VIB, group IB and lanthanide metals) are used to react aldehyde-containing polyether polyols with hydrogen at temperatures below 100°C to remove impurity aldehydes.
It significantly reduces the aldehyde content and odor in polyether polyols, achieving low-temperature and efficient aldehyde removal, and has economic value for industrial applications.
Smart Images

Figure BDA0003719198890000091
Abstract
Description
Technical Field
[0001] This invention relates to a method for reducing the aldehyde content in polyether polyols. Background Technology
[0002] Polyether polyols are one of the main raw materials for synthesizing polyurethane materials. There are many methods for preparing polyether polyols, mainly including anionic polymerization, cationic polymerization, and coordination polymerization.
[0003] CN104004177A relates to a method for preparing polyether polyols, based on a polymeric compound that is solid at room temperature, and a solvent-free method for preparing polyether polyols with block polyether chain structures. Specifically, it is anionic polymerization using an inorganic strong base (e.g., KOH) as a catalyst. Inorganic strong bases have advantages such as low cost and easy removal from polyether polyols, and are widely used in industrial production for preparing low molecular weight polyether polyols. However, inorganic strong bases easily cause isomerization of propylene oxide, producing monohydroxy polyethers with unsaturated double bonds at the ends, which reduces the functionality and relative molecular weight of the polyether polyol. Especially when preparing high molecular weight products, the content of monohydroxy polyethers is very high, and aldehydes and ketones are also generated, resulting in unpleasant odors. For example, in the preparation of a trifunctional polyether triol with a relative molecular weight of 5000, the acetaldehyde content is 0.78 μg / g, the formaldehyde content is 2.46 μg / g, the acetaldehyde content is 8.48 μg / g, and the acrolein content is 1.12 μg / g, which has an unpleasant odor.
[0004] CN103289040A discloses a method for producing a polyether polyol stream with low free formaldehyde content. The method involves evacuating a polyether polyol stream with a free formaldehyde content greater than 100 ppm under vacuum conditions of -0.20 MPa to -0.09 MPa and a temperature of 70 to 150°C, and then degassing the system with an inert gas to remove residual monomers, thereby obtaining a polyether polyol stream with a free formaldehyde content of less than 30 ppm.
[0005] CN109096479A discloses a method for reducing the propionaldehyde content in polyether polyols. This method uses a specific peroxide and a specific catalyst to convert propionaldehyde in the polyether polyol into propionic acid, which is then reacted with a solid alkaline substance. The propionaldehyde content in the polyether is reduced by filtration. Specifically, the specific peroxide is hydrogen peroxide, used at 0.02–0.2% of the mass of the polyether polyol; the specific catalyst is a cobalt-based metal complex catalyst, used at 0.0005–0.002% of the mass of the polyether polyol; and the solid alkaline substance is porous magnesium silicate, used at 0.1–1% of the mass of the polyether polyol.
[0006] CN101163735A discloses a polyether polyol, polyester polyol, and polyurethane with low residual aldehyde content. It comprises incorporating an effective amount of a) a phenolic antioxidant, b) one or more compounds selected from (i) an amine antioxidant, (ii) a benzofuran-2-one, and (iii) a phosphite or phosphonite, or (iv) a mixture thereof.
[0007] The synthesis of polyether polyols generates aldehydes and ketones, which have unpleasant odors. Existing technologies for reducing aldehydes have poor removal efficiency and urgently need to be addressed. Summary of the Invention
[0008] The purpose of this invention is to overcome the problems of high reaction temperature and poor removal effect in the existing technology of reducing aldehydes in the synthesis of polyether polyols. This invention provides a method for reducing the aldehyde content in polyether polyols. Using the method of this invention, the reaction temperature can be significantly reduced, and polyether polyols with low odor and low aldehyde content can be obtained.
[0009] To achieve the above objective, the present invention provides a method for reducing the aldehyde content in polyether polyols. The method includes: reacting an aldehyde-containing polyether polyol with hydrogen gas in the presence of a catalyst, wherein the catalyst contains a skeletal nickel catalyst matrix and a modified auxiliary metal, wherein the auxiliary metal is selected from one or more of group IVB metals, group VIB metals, group IB metals and lanthanides.
[0010] In the presence of the metal-modified framework nickel catalyst described in this invention, the reaction of aldehyde-containing polyether polyols with hydrogen gas can remove the impurity aldehydes encapsulated in the polyether polyols at temperatures below 100°C, significantly reducing the aldehyde content in the polyether polyols and yielding polyether polyols with low aldehyde content and low odor.
[0011] The method of this invention can remove aldehydes at lower temperatures, and has a significant advantage in aldehyde removal efficiency. The method of this invention has high economic value for industrial applications. Detailed Implementation
[0012] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0013] This invention provides a method for reducing the aldehyde content in polyether polyols. The method includes reacting an aldehyde-containing polyether polyol with hydrogen gas in the presence of a catalyst. The catalyst comprises a skeletal nickel catalyst matrix and a modified auxiliary metal selected from one or more group IVB, VIB, IB, and lanthanides. The method of this invention can remove aldehydes at lower temperatures and exhibits a significant advantage in aldehyde removal efficiency, overcoming the shortcomings of existing technologies such as high reaction temperatures and low removal efficiency.
[0014] In the presence of the metal-modified framework nickel catalyst described in this invention, the reaction of aldehyde-containing polyether polyols with hydrogen gas can remove the impurity aldehydes encapsulated in the polyether polyols at temperatures below 100°C, significantly reducing the aldehyde content in the polyether polyols and yielding polyether polyols with low aldehyde content and low odor.
[0015] In this invention, preferably, the molar ratio of the auxiliary metal to nickel in the catalyst is 0.1-0.7:1, more preferably 0.2-0.3:1; this is beneficial for further reducing the aldehyde content in the polyether polyol.
[0016] According to a preferred embodiment of the present invention, the porosity of the catalyst is 20-70%, preferably 50-60%, which is beneficial for further reducing the aldehyde content in the polyether polyol.
[0017] According to a preferred embodiment of the present invention, the auxiliary metal is selected from one or more of copper, molybdenum, titanium, cerium and manganese, preferably molybdenum.
[0018] According to a preferred embodiment of the present invention, the molar ratio of copper, molybdenum, titanium, cerium, manganese and nickel, in terms of elements, is (0.05-0.5):(0.05-0.5):(0-0.7):(0.05-0.5):(0-0.5):1, preferably (0.06-0.3):(0.2-0.3):(0-0.5):(0.1-0.3):(0-0.5):1.
[0019] According to a preferred embodiment of the present invention, the catalyst is an alloy catalyst containing nickel, aluminum and a fluxing metal, preferably with a nickel to aluminum mass ratio of 1:1.1-1.5.
[0020] In this invention, all metal-modified framework nickel catalysts with the aforementioned properties can achieve the purpose of this invention. This invention does not have any special requirements for the preparation method of the catalyst. According to a preferred embodiment of this invention, the preparation method of the catalyst includes: preparing an alloy containing a cooperating metal and nickel, contacting the alloy with an aqueous solution of an alkaline substance for leaching, and washing it until neutral after leaching to obtain a framework nickel catalyst.
[0021] In this invention, it is preferred to prepare an alloy containing a fluxing metal, nickel and aluminum, wherein the mass ratio of nickel to aluminum is 1:1.1-1.5.
[0022] According to a preferred embodiment of the present invention, the alkaline substance is an alkali metal hydroxide, more preferably sodium hydroxide and / or potassium hydroxide.
[0023] According to a preferred embodiment of the present invention, the concentration of the alkaline substance aqueous solution is 0.1-2 mol / L, preferably 1-2 mol / L.
[0024] According to a preferred embodiment of the present invention, the immersion conditions include: an immersion temperature of 40-100°C, preferably 60-80°C, and more preferably 70-80°C.
[0025] According to a preferred embodiment of the present invention, the cleaning conditions include: cleaning with deionized water, washing the catalyst surface to pH=7, and storing the catalyst in water.
[0026] According to a preferred embodiment of the present invention, the reaction conditions include an inlet temperature of 80-100°C. In the presence of the metal-modified nickel catalyst of the present invention, the reaction of an aldehyde-containing polyether polyol with hydrogen gas enables the removal of aldehyde impurities encapsulated in the polyether polyol at temperatures below 100°C, significantly reducing the aldehyde content in the polyether polyol and yielding a low-aldehyde-content, low-odor polyether polyol.
[0027] In this invention, the pressure can be adjusted. According to a preferred embodiment of the invention, the reaction conditions include a pressure of 2.5-3 MPa. This is beneficial for further reducing the aldehyde content in the polyether polyol.
[0028] According to a preferred embodiment of the present invention, the reaction conditions include: a flow rate of 0.1-1 mL / min for the aldehyde-containing polyether polyol; and a hydrogen flow rate of 100-200 mL / min, which is beneficial to further reduce the aldehyde content in the polyether polyol.
[0029] According to a preferred embodiment of the present invention, the polyether polyol has a molecular weight of 4000-8000 g / mol and is obtained by anionic polymerization; preferably, anionic polymerization using KOH catalyst is used; this is beneficial for further reducing the aldehyde content in the polyether polyol.
[0030] According to a preferred embodiment of the present invention, the reactor for the reaction is a fixed-bed reactor.
[0031] According to a preferred embodiment of the present invention, the conditions after the reaction are such that the total aldehyde residue in the polyether polyol is ≤10 mg / m³. 3The unsaturated bond content is ≤0.075mmol / g; the method described in this invention can significantly reduce the aldehyde content in polyether polyols.
[0032] In this invention, there is no particular limitation on the aldehyde concentration of the aldehyde-containing polyether polyol. According to a preferred embodiment of the invention, the aldehyde content in the aldehyde-containing polyether polyol is 200-500 mg / m³. 3 This is beneficial for further reducing the aldehyde content in polyether polyols.
[0033] The present invention will be described in detail below through embodiments.
[0034] In the following examples, aldehyde content was detected using an Agilent 1200 liquid chromatograph. The total aldehyde residue was calculated according to GB / T37196-2018. The unsaturated bond determination method was SH / T 0630-1996. The odor evaluation method was based on the Shanghai Volkswagen odor rating method.
[0035] In Examples 1-7, the polyether polyols were obtained by anionic polymerization using KOH catalyst.
[0036] Example 1
[0037] A Ni / Mo / Al alloy was prepared by melting nickel, molybdenum, and aluminum in a ratio of 1:0.25:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 56%.
[0038] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0039] Example 2
[0040] A Ni / Cu / Al alloy was prepared by melting nickel, copper, and aluminum in a ratio of 1:0.25:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 50%.
[0041] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0042] Example 3
[0043] A Ni / Ce / Al alloy was prepared by melting nickel, cerium, and aluminum in a ratio of 1:0.25:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 58%.
[0044] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0045] Example 4
[0046] A Ni / Mo / Al alloy was prepared by melting nickel, molybdenum, and aluminum in a ratio of 1:0.6:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 51%.
[0047] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0048] Example 5
[0049] A Ni / Cu / Al alloy was prepared by melting nickel, copper, and aluminum in a ratio of 1:0.6:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 48%.
[0050] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0051] Example 6
[0052] A Ni / Mo / Al alloy was prepared by melting nickel, molybdenum, and aluminum in a ratio of 1:0.6:1.2. The alloy was then leached with a 0.5 mol / L sodium hydroxide solution at 60°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst porosity was 41%.
[0053] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 80°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 150 mL / min, and the system pressure was raised to 4 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 0.5 mL / min. Aldehyde content data after hydrogenation are shown in Table 1, and odor data are shown in Table 2.
[0054] Example 7
[0055] The catalyst prepared in Example 1 differs in that,
[0056] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 80°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 200 mL / min, and the system pressure was raised to 2.5 MPa. Once the pressure stabilized, the feed pump (containing aldehyde-based polyether polyol with a molecular weight of 5000 and an aldehyde content of 280 mg / m³) was turned on. 3 The flow rate was 1 mL / min. Aldehyde content data after hydrogenation are shown in Table 1, and odor data are shown in Table 2.
[0057] Example 8
[0058] The difference from Example 1 is that the polyether polyol was prepared using an MMC bimetallic catalyst.
[0059] A Ni / Mo / Al alloy was prepared by melting nickel, molybdenum, and aluminum in a ratio of 1:0.25:1.2. The alloy was then leached with a 1 mol / L sodium hydroxide solution at 80°C for 1 hour. After leaching, the alloy was washed with deionized water until neutral to obtain the catalyst. The catalyst had a porosity of 56%.
[0060] The leached catalyst, along with water, was loaded into a fixed-bed reactor. After purging with nitrogen, the inlet temperature was raised to 90°C, at which point the nitrogen was shut off. The hydrogen flow rate was adjusted to 100 mL / min, and the system pressure was raised to 3.0 MPa. Once the pressure stabilized, the feed pump was turned on. (The polyether polyol was prepared using an MMC bimetallic catalyst with a molecular weight of 5000 and an aldehyde content of 280 mg / m³.) 3 The flow rate was 0.1 mL / min. The aldehyde content data after hydrogenation are shown in Table 1, and the odor data are shown in Table 2.
[0061] Example 9
[0062] The difference from Example 1 is that a multi-metal alloy was prepared by melting nickel, copper, molybdenum, cerium, and aluminum in a ratio of 1:0.06:0.25:0.1:1.2, while all other conditions were the same.
[0063] Table 1
[0064]
[0065] Table 2
[0066] Sample number Odor level Example 1 1.0 Example 2 2.5 Example 3 2.5 Example 4 3.5 Example 5 4.6 Example 6 4.8 Example 7 4.8 Example 8 5.0 Example 9 0.8
[0067] As can be seen from the results in Tables 1 and 2, the method for reducing the aldehyde content in polyether polyols described in this invention can significantly reduce the aldehyde content in polyether polyols, resulting in polyether polyols with low aldehyde content and low odor.
[0068] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for reducing the aldehyde content in polyether polyols, characterized in that, The method includes reacting an aldehyde-containing polyether polyol with hydrogen gas in the presence of a catalyst. The catalyst is an alloy catalyst containing a skeletal nickel catalyst matrix, aluminum, and a modified auxiliary metal, wherein the mass ratio of nickel to aluminum is 1:1.1-1.5; the molar ratio of the auxiliary metal to nickel is 0.1-0.7:1; and the auxiliary metal is selected from one or more of copper, molybdenum, and cerium. The catalyst has a porosity of 50-60%.
2. The method according to claim 1, wherein, The molar ratio of the auxiliary metal to nickel is 0.2-0.3:
1.
3. The method according to claim 1, wherein, The molar ratio of copper, molybdenum, cerium and nickel, in terms of elements, is (0.05-0.5):(0.05-0.5):(0.05-0.5):
1.
4. The method according to claim 3, wherein, The molar ratio of copper, molybdenum, cerium and nickel, in terms of elements, is (0.06-0.3): (0.2-0.3): (0.1-0.3):
1.
5. The method according to any one of claims 1-4, wherein, The catalyst preparation method includes: preparing an alloy containing a fluxing metal, nickel and aluminum, wherein the mass ratio of nickel to aluminum is 1:1.1-1.5; leaching the alloy with an aqueous solution of an alkaline substance; and washing the alloy until it is neutral after leaching.
6. The method according to claim 5, wherein, The alkaline substance is an alkali metal hydroxide.
7. The method according to claim 6, wherein, The alkaline substance is sodium hydroxide and / or potassium hydroxide.
8. The method according to claim 5, wherein, The concentration of the alkaline substance in the aqueous solution is 0.1-2 mol / L.
9. The method according to claim 8, wherein, The concentration of the alkaline substance in the aqueous solution is 1-2 mol / L.
10. The method according to claim 5, wherein, The leaching conditions include a leaching temperature of 40-100℃.
11. The method according to claim 10, wherein, The leaching conditions include a leaching temperature of 70-80℃.
12. The method according to claim 1, wherein, The reaction conditions include: an inlet temperature of 80-100℃; a pressure of 2.5-3MPa; a flow rate of 0.1-1mL / min for the aldehyde-containing polyether polyol; and a hydrogen flow rate of 100-200mL / min.
13. The method according to claim 1, wherein, The polyether polyol has a molecular weight of 4000-8000 g / mol and is obtained by anionic polymerization; and / or The reactor used for the reaction is a fixed-bed reactor.
14. The method according to claim 13, wherein, The polyether polyol has a molecular weight of 4000-8000 g / mol and is obtained by anionic polymerization using KOH catalyst.
15. The method according to claim 1, wherein, The reaction conditions ensured that the total aldehyde residue in the polyether polyol was ≤10 mg / m³. 3 Unsaturated bonds ≤0.075 mmol / g; and / or The aldehyde content in polyether polyols containing aldehydes is 200-500 mg / m³. 3 .
Citation Information
Patent Citations
Polyether polyols, polyester polyols and polyurethanes of low residual aldehyde content
CN101163735A
Production method of polyether polyol-containing material flow with low free formaldehyde
CN103289040A
Method for manufacturing polyether polyols
CN104004177A
Method for reducing content of propionaldehyde in polyether polyol
CN109096479A
Catalyst, preparation method thereof and method for reducing aldehyde content in polyether polyol
CN114433098A