Preparation method and application of high-ratio foamable polyphenyl ether material

By preparing a high-ratio foaming nucleating agent, an acrylic acid-methyl methacrylate-silica-styrene branched prepolymer was constructed using emulsion polymerization. This solved the problems of brittleness and low closed-cell rate in foamable polyphenylene ether materials, achieving high-ratio foaming and improved strength, thus expanding the application range.

CN117343380BActive Publication Date: 2026-11-20WUXI HI TEC ENVIRONMENTAL MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311464705.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-07
Publication Date
2026-11-20
Estimated Expiration
2043-11-07

AI Technical Summary

Technical Problem

Existing expandable polyphenylene ether materials suffer from problems such as brittle foam, high molding pressure, and low closed-cell rate, which affect their market promotion.

Method used

By preparing a high-ratio foaming nucleating agent, an acrylic acid-methyl methacrylate-silica-styrene branched prepolymer was constructed using emulsion polymerization. This improved the compatibility and dispersion performance of the nucleating agent with the system, and formed a cross-linked network structure during the blending and granulation process, thereby enhancing melt strength and melt tension.

Benefits of technology

It improves the closed-cell rate and expansion ratio of foamed products, reduces molding pressure, enhances product toughness and overall strength, and expands application scope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117343380B_ABST
    Figure CN117343380B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a high-ratio foamable polyphenyl ether material. The application is configured into a core agent acrylic acid-methyl methacrylate-silicon dioxide-styrene branched pre-polymer through an emulsion polymerization mode, the compatibility and dispersion performance of the core agent and the system are improved through the fixing of styrene; in addition, the excess reactive groups (such as carboxyl and unsaturated double bond) of the system can improve the melt strength and melt tension of the product (a structure similar to crosslinking is generated, the melt viscosity and tension of the pre-polymer are improved) in the subsequent PPE blending and granulation process, so that the gas coating effect is favorable in the foaming process, and the foamable ratio and overall strength of the product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing high-expandable polyphenylene ether material and its application. Background Technology

[0002] Foamed materials are a new type of material that reduces its specific gravity while maintaining high strength by introducing internally regular voids. Their lightweight characteristics effectively meet today's demands for energy conservation and emission reduction. Generally, foamed materials require a certain melt strength; otherwise, during cell growth, they cannot effectively resist the interfacial tension caused by cell growth, leading to drawbacks such as low foaming ratio or inability to mold the material.

[0003] Common foamable materials, such as polystyrene (PS), polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE), polyetheretherketone (PEEK), and polyimide (PI), are polymers with high melt viscosity. Their foaming temperature gradually increases with increasing melt viscosity. With technological advancements, more new materials are becoming available for foaming. Through blending modification, the melt strength of products can be improved to meet the requirements of foaming.

[0004] Expandable polyphenylene oxide (mPPE) is a novel type of expandable material, obtained by blending and modifying polyphenylene oxide (PPE) with a certain proportion of high-impact polystyrene (HIPS). mPPE possesses advantages such as high temperature resistance, high dimensional stability, self-extinguishing properties, and high electrical insulation. Its foaming can be achieved through extrusion sheets and autoclaving. However, due to the inherent characteristics of the material, the foam often suffers from brittleness, high molding pressure, and low closed-cell ratio, which to some extent hinders its further market penetration. Therefore, how to modify it to improve the toughness of the foam while reducing molding pressure and increasing the closed-cell ratio and expansion ratio of the product is a key improvement project for this material to enter the market. Summary of the Invention

[0005] This invention starts with the preparation method of polyphenylene ether foaming nucleating agent. By improving the strength of the foamed melt and reducing the pressure required for foaming, the closed-cell rate of the foamed product is improved, the foaming ratio of the product is increased, and the defects such as high molding pressure and poor toughness of foamed beads are solved, thus expanding the application space and usage efficiency of the product.

[0006] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide a method for preparing high-expandable polyphenylene ether material.

[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0008] A method for preparing a high-expansion-ratio polyphenylene ether material includes the following steps:

[0009] Step 1: Pretreatment: Dry the polyphenylene ether in a high-temperature oven for later use; dry the polystyrene and flame retardant at 50°C for 4-6 hours.

[0010] The molecular weight of polyphenylene ether is 20,000-50,000 Da, preferably 25,000-30,000 Da; preferably, the drying temperature of polyphenylene ether is 100-120℃ for 6-8 hours.

[0011] Step 2: Pretreatment of silica: After drying the silica powder, pretreatment is carried out using plasma equipment, followed by grinding for later use; preferably, the plasma treatment power is 1 kW and the time is 120 min during grinding.

[0012] The preferred particle size of the ground silica powder is 10-50 nm.

[0013] Step 3: Preparation of high-ratio foaming nucleating agent: Mix acrylic acid, methyl methacrylate, emulsifier, and deionized water after quantitative distillation and drying. Use potassium persulfate as an initiator, and after constant temperature and thorough stirring and dispersion, add quantitative silica powder pretreated in step 2, stir thoroughly and evenly, then slowly add quantitative styrene monomer, slowly heat to 80°C, maintain the reaction for 4-6 hours, filter the reaction solution to remove water, and then dry it in a vacuum oven. The preferred emulsifier is sodium dodecylbenzenesulfonate (SDS). In the preparation system of high-ratio foaming nucleating agent, the mixing ratio of sodium dodecylbenzenesulfonate (SDS), acrylic acid, and water is 2:30:100.

[0014] During the preparation of the nucleating agent, the constant temperature stirring temperature is 60℃ and the rotation speed is 100r / min. Surface-hydroxylated silica powder after plasma treatment in step two is added, with the addition amount being 5%-10% of the system (by weight).

[0015] Preferably, in step 3, the amount of styrene monomer added is 30%-50% (by weight) of the system, of which the initiator (potassium persulfate) accounts for 2-3% (by weight), and the dropping rate is 1 drop / s; the total reaction time is 4-6 hours, and the emulsion is filtered to obtain the desired branched prepolymer of acrylic acid-methyl methacrylate-silica-styrene with a core-shell structure;

[0016] More preferably, in the preparation of the high-ratio foaming nucleating agent, the proportions of each material (by weight) are as follows:

[0017] Water: 100 parts

[0018] Acrylic acid: 5-10 parts

[0019] Methyl methacrylate: 20-30 parts

[0020] Emulsifier: 5 parts

[0021] Silica: 5-10 parts

[0022] Styrene: 30-50 parts

[0023] Initiator: 2-3 parts

[0024] Step 4: Preparation of high-ratio polyphenylene ether precursor: The polyphenylene ether, polystyrene, appropriate amount of flame retardant, and high-ratio foaming nucleating agent treated in Step 1 are co-extruded by twin screw extruder and then granulated to prepare a foaming precursor with a certain length-to-weight ratio;

[0025] Preferably, the molecular weight of polystyrene is 300,000-500,000 Da, and the flame retardant is preferably a phosphorus-based flame retardant, such as triphenyl phosphate (TPP) or resorcinol bis(diphenyl phosphate) (RDP), and the amount used is 8-15% of the mass fraction of the high-ratio polyphenylene ether foaming precursor system.

[0026] Preferably, the mass proportions of each component in the preparation of the high-ratio polyphenylene ether foaming precursor are as follows:

[0027] Polyphenylene ether: 50-70 parts

[0028] Polystyrene: 20-30 parts

[0029] Flame retardant: 8-15 parts

[0030] High-ratio nucleating agent: 2-5 parts.

[0031] Preferably, during co-extrusion using twin screws, the temperature is controlled at 240-260℃, the pellet length is 1.5-2.5mm, and the pellet weight is 0.3-0.5mg.

[0032] Step 5: Preparation of high-ratio polyphenylene ether foamed beads: The high-ratio polyphenylene ether precursor prepared in step 4 is impregnated under certain temperature and pressure by autoclaving, and then the pressure is released to obtain the desired high-ratio polyphenylene ether foamed beads.

[0033] Preferably, supercritical carbon dioxide autoclave foaming technology is used, with water as the carrier. After impregnation with gas under high temperature and high pressure in a reactor, the pressure is rapidly released to obtain the desired polyphenylene ether foamed beads. The foaming temperature is controlled at 170-190℃, the foaming back pressure is controlled at 1.5-3.0MPa, and the foamed particle density is about 50-250g / L.

[0034] Preferably, during autoclaving, water, kaolin, and surfactant are added to the high-ratio polyphenylene ether foaming precursor, with the following proportions by weight:

[0035] Water: 100 parts

[0036] High-ratio polyphenylene ether foaming precursor: 50 parts

[0037] Kaolin: 3 parts

[0038] Surfactant: 1 part.

[0039] The surfactant can be any one or more of sodium dodecylbenzenesulfonate, calcium stearate, triethanolamine, etc.

[0040] Preparation of high-ratio expanded polyphenylene ether (EPE) molded parts: After drying the high-ratio EPE foamed beads obtained in step 5, they are pre-pressurized in a pre-pressurization tank, molded using a steam molding machine, and then dried to obtain the desired high-ratio EPE foamed molded parts. Preferably, after holding the pressure in the pre-pressurization tank for 5-6 hours at a pressure of 2.0-4.0 bar, the parts are then steam-molded using an EPP steam molding machine at a pressure of 3.8-4.5 bar, cooled, and dried to obtain the desired expanded polyphenylene ether molded parts.

[0041] The beneficial effects achieved by this invention are as follows: This invention constructs a branched prepolymer of acrylic acid-methyl methacrylate-silica-styrene through emulsion polymerization. By fixing styrene, the compatibility and dispersion performance of the nucleating agent with the system are improved. In addition, the excess reactive groups in the system (such as carboxyl groups and unsaturated double bonds) can improve the melt strength and melt tension of the product during the subsequent PPE blending and granulation process (generating a cross-linked structure, increasing the melt viscosity and tension of the prepolymer). This facilitates gas encapsulation during the foaming process, thereby improving the foaming ratio and overall strength of the product. Attached Figure Description

[0042] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:

[0043] Figure 1 These are electron microscope images of Embodiment 1 of the present invention;

[0044] Figure 2 This is a schematic diagram of the high-ratio foaming nucleating agent of the present invention;

[0045] Figure 3 This is an example diagram of a foaming system. Detailed Implementation

[0046] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0047] Example

[0048] The preparation of a high-expansion-ratio foamable polyphenylene ether material, wherein the composition of the high-ratio nucleating agent used in the reaction is shown in the table below:

[0049]

[0050] Among them, E / F / G / H were uniformly distributed in the comparative experiment of group B.

[0051] The specific settings for each embodiment are as follows:

[0052]

[0053]

[0054] Note:

[0055] 1. Formula for testing the internal pressure of foam particles (B, unit is Bar) is as follows:

[0056] B=0.00471×BD(W2)×(273+T) / W1

[0057] in:

[0058] ①BD represents the density of foamed particles, in g / L;

[0059] ②W2 represents the particle weight before and after pressurization, in grams;

[0060] ②T represents ambient temperature, in °C;

[0061] ③W1 represents the weight of the particle before pressure is applied, in grams.

[0062] Under the same pre-compression conditions, the higher the internal pressure of the particles, the higher the closed-cell rate, and the better the product quality during subsequent molding. Comparative Example 1 shows that the dispersion is poor and the internal pressure is also low.

[0063] Too low a closed-cell ratio will prevent the product from being molded in the future, meaning it cannot continue to expand at high temperatures, which will affect the welding performance of the product.

[0064] from Figure 1 It can be seen that the obtained high-ratio polyphenylene ether foam beads have a uniform distribution of pores.

[0065] like Figure 2As shown, the nucleating agent in this invention has a core-shell structure, with PS coating on the outside and a PMMA+PAA intercalation structure on the inside. PS is polystyrene polymerized from styrene, PMMA is polymethyl methacrylate polymerized from methyl methacrylate, and PAA is polyacrylic acid polymerized from acrylic acid. Because PAA possesses double bonds, its structure contains a certain number of free double bonds. In the subsequent PPE system, it can form a cross-linked network structure as shown in the right figure. At high temperatures, this increases melt tension and reduces fluidity after high-temperature plasticization.

[0066] Q: The reaction, via emulsion polymerization, yields the structure shown in the right figure. Its unique reaction site allows the product to acquire a core-shell structure as shown, with polystyrene on the outer layer and PMMA and PAA on the inner layer – a special structure.

[0067] like Figure 3 As shown, the free double bonds on the nucleating agent in the system can be polymerized through reaction, thereby giving the system a cross-linked network structure, fixing the polyphenylene ether molecular chain, increasing the viscosity of the system during the foaming process, and improving the foaming performance of the product; in the subsequent PPE blending and granulation process, it can improve the melt strength and melt tension of the product, and in the subsequent combustion test, it can effectively prevent melt drop and better enable the product to achieve v-0 combustion performance.

[0068] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-expansion-ratio polyphenylene ether material, comprising the following steps: Step 1: Pretreatment: The polyphenylene ether is dried in a high-temperature oven and then set aside for later use; the polystyrene and flame retardant are dried. Step 2: Pretreatment of silica: After drying the silica powder, grind it using a plasma device for later use; Step 3: Preparation of high-ratio foaming nucleating agent: Mix acrylic acid, methyl methacrylate, emulsifier and water after quantitative distillation and drying, use potassium persulfate as initiator, and after constant temperature and thorough stirring and dispersion, add quantitative silica powder pretreated in step 2, stir thoroughly and evenly, then slowly add quantitative styrene monomer, heat and react for 4-6 hours, filter the reaction solution to remove water, and dry it in a vacuum oven to obtain acrylic acid-methyl methacrylate-silica-styrene branched prepolymer with core-shell structure; When preparing a high-ratio foaming nucleating agent, the weight percentages of each material are as follows: Water: 100 parts Acrylic acid: 5-10 parts Methyl methacrylate: 20-30 parts Emulsifier: 5 parts Silica: 5-10 parts Styrene: 30-50 parts Initiator: 2-3 parts; Step 4: Preparation of high-ratio polyphenylene ether precursor: The polyphenylene ether treated in step 1, polystyrene, an appropriate amount of flame retardant, and the high-ratio foaming nucleating agent prepared in step 3 are co-extruded by twin screw extrusion and then granulated to prepare the high-ratio polyphenylene ether precursor. The mass percentages of each component in the preparation of the high-ratio polyphenylene ether precursor are as follows: Polyphenylene ether: 50-70 parts Polystyrene: 20-30 parts Flame retardant: 8-15 parts High-ratio foaming nucleating agent: 2-5 parts; Step 5: Preparation of high-ratio polyphenylene ether foamed beads: The high-ratio polyphenylene ether precursor prepared in step 4 is impregnated under certain temperature and pressure by autoclaving, and then the pressure is released to obtain the desired high-ratio polyphenylene ether foamed beads.

2. The method for preparing the high-expansion polyphenylene ether material as described in claim 1, characterized in that, In step 1, the molecular weight of polyphenylene ether is 20,000-50,000 Da.

3. The method for preparing the high-expandability polyphenylene ether material as described in claim 1, characterized in that, In step 2, the plasma treatment power is 1 kW and the time is 120 min. The particle size of the ground silica powder is 10-50 nm.

4. The method for preparing the high-expandability polyphenylene ether material as described in claim 1, characterized in that, In step 3, the emulsifier is sodium dodecylbenzenesulfonate.

5. The method for preparing the high-expansion polyphenylene ether material as described in claim 4, characterized in that, In step 3, the high-ratio foaming nucleating agent is prepared by constant temperature stirring at 60℃ and rotation speed at 100r / min, with a styrene monomer dropping rate of 1 drop / s; the total reaction time is 4-6 hours, and the reaction solution is filtered to obtain the final product.

6. The method for preparing the high-expansion polyphenylene ether material as described in claim 1, characterized in that, In step 4, the molecular weight of polystyrene is 300,000-500,000 Da, and the flame retardant is resorcinol bis(diphenyl phosphate).

7. The method for preparing the high-expandability polyphenylene ether material as described in claim 1, characterized in that, In step 4, during co-extrusion using a twin-screw extruder, the temperature is controlled at 240-260℃, the pellet length is 1.5-2.5mm, and the pellet weight is 0.3-0.5mg.

8. The method for preparing the high-expansion polyphenylene ether material as described in claim 1, characterized in that, In step 5, supercritical carbon dioxide autoclave foaming technology is used, with water as the carrier. After impregnation with gas under high temperature and high pressure in the reactor, the pressure is rapidly released to obtain the desired polyphenylene ether foamed beads. The foaming temperature is controlled at 170-190℃, the foaming back pressure is controlled at 1.5-3.0MPa, and the foamed particle density is 50-250g / L.

9. The method for preparing the high-expansion polyphenylene ether material as described in claim 8, characterized in that, During autoclaving, water, kaolin, and surfactant are added to the high-ratio polyphenylene ether precursor. The proportions of each component by weight are as follows: Water: 100 parts High-ratio polyphenylene ether precursor: 50 parts Kaolin: 3 parts Surfactant: 1 part.

10. A high-expansion polyphenylene oxide molded part, characterized in that, After drying the high-ratio polyphenylene ether foamed beads obtained by the preparation method according to any one of claims 1-8, they are pressurized in a pre-pressurization tank for 5-6 hours at a pressure of 2.0-4.0 bar. Then, they are passed through an EPP steam forming equipment with a steam pressure of 3.8-4.5 bar, cooled and dried to obtain the desired high-ratio foamed polyphenylene ether molded parts.

Citation Information

Patent Citations

  • Preparation method of flame-retardant micro foamed polyphenyl ether composite material and flame-retardant micro foamed polyphenyl ether composite material

    CN109867942A

  • Preparation method of polyphenyl ether foamable particles

    CN115181319A