High-temperature-resistant slow-release composite material, preparation method and application thereof
By preparing a composite material containing biodegradable heat-resistant polymers, surfactants, and inorganic particles, the problem of rapid dissolution of slow-release materials at high temperatures was solved, and the stable and slow release of surfactants was achieved, making it suitable for cleaning and foaming of high-temperature oil and gas wells.
Patent Information
- Application Number
- CN202210734106.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-27
AI Technical Summary
Existing slow-release materials dissolve and decompose rapidly at high temperatures, resulting in the rapid release of surfactants and a short release time, which cannot meet the needs of high-temperature oil and gas wells.
An intercalated composite material containing a biodegradable heat-resistant polymer, surfactant, and inorganic particles is prepared by melt blending and injection molding to form an intercalated composite material, which is coated with surfactant to achieve high-temperature slow release.
It achieves stable and slow release of surfactants under high temperature conditions, prolonging the sustained release time, and is suitable for cleaning, foaming, and corrosion inhibitor applications in high-temperature oil and gas wells.
Smart Images

Figure CN117343491B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid composite materials technology, specifically to a high-temperature resistant slow-release composite material, its preparation method, and its application. Background Technology
[0002] In oil and gas extraction, various chemical agents are widely used, such as corrosion inhibitors, wax inhibitors, scale inhibitors, natural gas hydrate inhibitors, and surfactants. These need to be frequently added to the formation, wellbore, and pipelines to reduce formation damage, increase oil and gas production, and ensure wellbore integrity and unobstructed flow. Surfactants can have cleaning, dispersing, oil displacement, and foaming effects. Adding too much product at once is wasteful; slow-release technology can reduce the number of operations. Slow-release systems can also effectively improve the utilization rate of active chemical components and reduce losses and volatilization caused by environmental factors. In natural gas extraction, as extraction time increases, downhole pressure decreases, and groundwater accumulates in the wellbore, reducing or even halting natural gas production. Foaming agents, acting as foaming agents, remove this water from the wellbore base fluid. These wellbore chemical foaming agents can be solid or liquid. Solid foaming rods are usually made into fast-dissolving solid rods and are periodically added to the wellbore through frequent well openings. Liquid foaming agents, on the other hand, are injected downhole via pumps, requiring investment in pipelines and pumps. Solid slow-release chemicals are an effective method to reduce the investment in well opening and liquid injection equipment.
[0003] Slow-release technology has applications in agriculture, pharmaceuticals, and oilfield chemicals. In the pharmaceutical field, encapsulating drugs in slow-release capsules can reduce the frequency of application and extend the effective duration of action several times over. In the field of pesticide slow-release agents, there are many varieties, including microcapsules. The capsule shell can be a natural, semi-synthetic, or fully synthetic polymer compound, including proteins, high-molecular-weight carbohydrates, cellulose, fatty acids and their derivatives, inorganic polymers, vinyl polymers, polyamides, polyurethanes, and polyesters. In the field of slow-release fertilizers, modified polyvinyl alcohol is mixed with inorganic materials such as diatomaceous earth, zeolite powder, biochar, phosphate rock powder, and sulfur as coating materials to control nitrogen loss and improve nitrogen fertilizer utilization.
[0004] Slow-release technology has been widely applied in oilfields, with field applications already existing in corrosion and scale inhibition. Currently, slow-release technology is also being used in other areas of oilfield development, such as drilling cement slurries. For example, slow-release salt inhibitors have been produced using a combination of epoxy resin and starch. Additionally, microencapsulation technology encapsulates cement accelerators to slow their release rate and improve the thickening properties of cement systems.
[0005] US20160009980A1 discloses a method using porous metal oxides such as alumina, zirconium oxide, and titanium oxide as a solid carrier and a binder. The composite material, consisting of a well-formed compressible particle adsorbed onto calcined porous metal oxides or entering the gaps within the calcined porous metal oxides, can be introduced into oil wells or gas wells to slowly release the effective components adsorbed within the porous material. US20180134939A1 discloses a method of cross-linking scale inhibitors and slow-release agents onto a carrier via chemical bonds, utilizing the cross-linking reaction of alcohols, amines, and acids. Downhole, the cross-linking bonds hydrolyze, slowly releasing the active substances. US20170058184A1 discloses a water-insoluble carrier composed of corn cob sand, used in oil and gas field enhancement or production processes to adsorb liquid chemical reagents such as scale inhibitors and surfactants. The pressure resistance and liquid insolubility of the corn cob sand allow for the slow release of active chemicals into the oil and gas well, achieving the purpose of slow release. US20120273197A1 discloses a composite material for well treatment operations such as hydraulic fracturing and sand control. This material allows one or more well treatment agents to be slowly released into the underground formation and / or into the wellbore penetrating the formation. It features a high specific surface area nanoscale calcined porous matrix (adsorbent) onto which the well treatment agent is coated. CN110157401A discloses a method for preparing a controllable long-lasting slow-release scale inhibitor capsule. The scale inhibitor and one of the slow-release components, an inorganic nanocarrier, are assembled into a homogeneous whole in the form of a solid solution. The capsule is then coated with a controllably dissolvable cross-linked polymer composed of carboxymethyl cellulose, polyvinyl alcohol, and porous zeolite. When the polymer dissolves in the environmental medium, the active substances are gradually released. Utilizing a dual controlled-release mechanism of polymer dissolution and desorption of the scale inhibitor from the inorganic nanocarrier, the capsule can be slowly released into the wellbore, thereby prolonging its protective effect. CN107304078A discloses an environmentally friendly slow-release polymer scale inhibitor, which uses a mixture of polyvinyl alcohol, sodium alginate and gelatin solution as a carrier material and boric acid as an additive to construct a slow-release wall material system to load the scale inhibitor, and performs slow release in a simulated oilfield water medium at 50°C.
[0006] Although slow-release technology is increasingly used in oil and gas field development, the complex environmental characteristics of high-temperature wells lead to exceptionally stringent requirements for slow-release materials. CN110564388A discloses a method for preparing a temperature-sensitive plugging colloid for oil and gas fields. This method involves multiphase physical adsorption and chemical pre-crosslinking of modified polyacrylamide, a trivalent crosslinking agent, a water-soluble slow-release agent, and an aqueous phase, resulting in a temperature-sensitive plugging colloid with delayed-release properties due to temperature-sensitive swelling. However, its applicable temperature range is only 60-90℃. CN110003875A presents research on slow-release foaming agents, mixing surfactants and foaming agents with 5-20% casings to achieve an action time of 120 hours (5 days). However, this technology has drawbacks, including an operating temperature below 90℃ and a shelf life of less than 3 months for animal materials and inconsistent batch quality. In these studies, the selection of slow-release materials for specific conditions (e.g., acid resistance, temperature resistance) remains a significant challenge.
[0007] In summary, most existing slow-release materials use slowly soluble materials to encapsulate surfactants to achieve a slow-release effect; however, the materials used dissolve and decompose rapidly at high temperatures, causing the surfactants to be released quickly, resulting in a short slow-release time.
[0008] Therefore, a new type of composite material is needed to solve the problems of short release time and low temperature resistance of existing slow-release materials for oil fields. Summary of the Invention
[0009] To address the problems existing in the prior art, this invention provides a high-temperature resistant slow-release composite material, its preparation method, and its application. The high-temperature resistant slow-release composite material of this invention contains surfactants, biodegradable heat-resistant polymers, and inorganic particles; the composite material of this invention exhibits good temperature resistance, stable release of active ingredients, and can be used in high-temperature oil and gas wells, reducing the need for frequent well opening and chemical injection.
[0010] One of the objectives of this invention is to provide a high-temperature resistant slow-release composite material.
[0011] The high-temperature resistant slow-release composite material contains a biodegradable heat-resistant polymer, a surfactant, and inorganic particles.
[0012] In a preferred embodiment of the present invention,
[0013] Based on a total weight of 100% for high-temperature resistant slow-release composite materials,
[0014] The biodegradable heat-resistant polymer content is 30-80%; preferably 50-75%; more preferably 60-75%.
[0015] The surfactant content is 1-60%; preferably 5-35%; more preferably 15-30%.
[0016] The inorganic particles comprise 1–50%; preferably 1–40%; more preferably 5–15%.
[0017] The biodegradable heat-resistant polymer described in this invention is a polymer that combines thermal stability with biodegradability or acid / alkali degradation. The thermal stability can be selected according to application requirements.
[0018] In a preferred embodiment of the present invention,
[0019] The degradable and heat-resistant polymer is polybutylene adipate terephthalate (PBAT).
[0020] Polybutylene adipate terephthalate (PBAT) is obtained by reacting butanediol, adipic acid and terephthalic acid. It is a completely biodegradable polymer material that can be hydrolyzed by acids and alkalis in the environment or decomposed by microorganisms, ultimately producing carbon dioxide and water. It does not have a negative impact on the environment and is inexpensive, making it a material with practical value. The preferred PBAT is Ecoflex, a fully biodegradable plastic produced by BASF in Germany.
[0021] In this invention, those skilled in the art can select the type of surfactant according to application requirements (e.g., cleaning agent, foaming agent, and corrosion inhibitor), which can be a single surfactant or a compounded surfactant.
[0022] In a preferred embodiment of the present invention,
[0023] The surfactant is at least one of anionic surfactants and amphoteric surfactants;
[0024] The anionic surfactant is preferably at least one of sodium alkyl sulfate, sodium alkyl sulfonate, sodium alkylbenzene sulfonate, and sodium alkyl taurate; more preferably at least one of sodium alkyl sulfonate and sodium alkylbenzene sulfonate; and / or,
[0025] The amphoteric surfactant is preferably at least one of alkylamine oxide and alkyl betaine, more preferably at least one of alkylamidopropylamine oxide, alkylamidopropyl betaine, and alkyl hydroxypropyl sulfobetaine.
[0026] In a preferred embodiment of the present invention,
[0027] The surfactant has an alkyl chain length of 8 to 16, and is preferably at least one of sodium dodecylbenzenesulfonate, sodium dodecyl sulfonate, sodium dodecyl sulfate, cocamidopropyl betaine, and cocamidopropyl hydroxysulfonate.
[0028] In this invention, the alkyl chain length refers to the length of the alkyl backbone. It is understood that side chains may or may not be connected to the alkyl backbone. This invention does not limit the type of side chains; for example, they can be alkyl side chains. Those skilled in the art can freely choose, as long as it improves the temperature-resistant slow-release properties of the composite material.
[0029] In a preferred embodiment of the present invention,
[0030] The surfactant also includes a nonionic surfactant as an auxiliary agent, and the nonionic surfactant is preferably an alkyl polyoxyethylene and / or an alkyl glycoside.
[0031] The alkyl polyoxyethylene is preferably at least one selected from alkyl polyoxyethylene ether, alkylamine polyoxyethylene ether, and castor oil polyoxyethylene ether; and / or
[0032] The alkyl glycoside is preferably a carbon chain C. 8-14 The alkyl glycoside or alkyl polysaccharide, more preferably at least one of APG810, APG814, and APG1214.
[0033] The degree of polymerization of the alkyl polyoxyethylene is preferably 4 to 10.
[0034] Under this preferred embodiment, it is more conducive to the uniform dispersion of surfactants in composite materials, and the sustained-release effect time of high-temperature resistant sustained-release composite materials is longer.
[0035] In a preferred embodiment of the present invention,
[0036] The inorganic particles are at least one of hydrophobic montmorillonite, organobentonite, SiO2, kaolin, and CaCO3, preferably at least one of hydrophobic montmorillonite, kaolin, and CaCO3. In this invention, the introduction of inorganic particles can further increase the coating density of the surfactant, the strength of the composite material, and prolong the slow release time.
[0037] In a preferred embodiment of the present invention,
[0038] The inorganic particles have a particle size of 30 nm to 5 μm, preferably 30 nm to 200 nm.
[0039] Other commonly used additives in the art, such as inert inorganic salts, can also be added to the high-temperature resistant slow-release composite material of the present invention. The inert inorganic salts are preferably Na2SO4 or NaCl, and their dosage is also conventional. Those skilled in the art can add them according to the actual situation.
[0040] The second objective of this invention is to provide a method for preparing a high-temperature resistant slow-release composite material, which is one of the objectives of this invention.
[0041] The method includes melting and blending components including a biodegradable heat-resistant polymer, a surfactant, and inorganic particles, followed by injection molding to obtain the high-temperature resistant slow-release composite material.
[0042] The melt blending equipment and injection molding equipment used above can be commonly used equipment in the plastics processing field, such as torque rheometers, screw extruders, and injection molding machines.
[0043] In a preferred embodiment of the present invention,
[0044] The melt blending temperature is 140–250°C, preferably 150–250°C, and more preferably 150–170°C.
[0045] A third objective of this invention is to provide a high-temperature resistant slow-release composite material, either as one of the objectives of this invention or as a high-temperature resistant slow-release composite material prepared by the method of another objective of this invention, for use as a foaming agent.
[0046] The inventors of this invention discovered during experimentation that a temperature-resistant, slow-release material can be formed by mixing and melting an active ingredient (e.g., a surfactant) with a biodegradable, heat-resistant polymer and inorganic particles. This material is better suited for oil and gas wells, and the preparation method is simple and easy to operate. This invention preferably uses polybutylene adipate terephthalate (PBAT) copolymer as one of the raw materials, and adds inorganic particles. Under hot-melt conditions, the active component is uniformly stirred and dispersed in the solid material to form a solid material with slow-release and temperature-resistant properties. This material also possesses acid resistance and salt resistance. This invention achieves the encapsulation of surfactants (e.g., foaming agents) in solid materials, which can address the problem of frequent well opening and injection of foaming agents for high-temperature gas well drainage and gas production. Other biodegradable polymers, such as polylactic acid (PLA) and polyglycolic acid (PGA), have poor temperature resistance, poor salt resistance, and poor compatibility with surfactants.
[0047] The high-temperature resistant slow-release composite material of this invention contains polybutylene adipate terephthalate (PEG). This polymer, when intercalated with inorganic particles and surfactants, forms a composite high-temperature resistant slow-release material. This material encapsulates the surfactant, giving it excellent temperature resistance while also exhibiting good slow-release properties. The active ingredient is released stably and can slowly release the active ingredient—the surfactant—in the high-temperature environment of the wellbore. It can be used as a cleaning agent, foaming agent, or corrosion inhibitor, and can be applied in fields such as oil and gas wellbore cleaning, foaming drainage, and corrosion inhibition. The introduction of nano-inorganic particles further improves the performance of the composite material, increases the slow-release time, and enhances its temperature resistance.
[0048] The preparation method provided by the present invention can produce the aforementioned high-temperature resistant slow-release composite material with specific composition. By using specific raw materials in appropriate amounts, they can work together to form an organic-inorganic composite structure. At the same time, the surfactant is uniformly dispersed and coated, forming a composite material with both slow release and temperature resistance. When applied, the surfactant can be slowly released at high temperature (e.g., 130°C).
[0049] In the method of this invention, biodegradable polymers and inorganic materials are melt-blended and simultaneously coated with surfactants to form an intercalated composite material (i.e., a temperature-resistant slow-release composite material). This composite material exhibits good temperature resistance and allows for the slow release of the surfactant, resulting in a long-lasting sustained-release effect. The specific proportions of each raw material component ensure that the surfactant is coated while the composite is being formed, resulting in a composite material that possesses both temperature resistance and sustained-release properties. However, under the same conditions, if the proportions of the raw materials used are inappropriate, the composite may not form, or the amount of coated surfactant may be insufficient, leading to stratification or a short release time.
[0050] In this invention, it is understood that all raw materials are completely converted into composite materials.
[0051] In this invention, the melt blending process can prepare a composite material. The polymer is softened and mixed above its melting point. Preferably, after polymerization and melting, the mixture is stirred and then injection molded. This preferred method is more conducive to the formation of a composite.
[0052] The temperature-resistant slow-release composite material provided by this invention can slowly release active substances - surfactants under high temperature (e.g., 80-150℃) and acidic (e.g., pH 4-5) conditions in the wellbore, and can be used as a cleaning agent, foaming agent or corrosion inhibitor.
[0053] By incorporating a foaming agent into the temperature-resistant slow-release composite material of this invention, the problem of frequent well opening and injection of foaming agents can be solved for high-temperature gas well drainage and gas production. Attached Figure Description
[0054] Figure 1 The initial appearance of the slow-release composite material in Comparative Example 1 is shown.
[0055] Figure 2 The image shows the appearance of the slow-release composite material of Comparative Example 1 after 6 hours of slow-release evaluation experiment.
[0056] Figure 3 The image shows the appearance of the slow-release composite material of Comparative Example 2 after 6 hours of slow-release evaluation experiment.
[0057] Figure 4 The image shows the appearance of the slow-release composite material of Comparative Example 3 after 20 hours of slow-release evaluation experiment.
[0058] Figure 5 This is an initial appearance diagram of the high-temperature resistant slow-release composite material of Example 4;
[0059] Figure 6 This is an image of the high-temperature resistant slow-release composite material of Example 4 after 48 hours of slow-release evaluation experiment;
[0060] Figure 7 This is an image of the high-temperature resistant slow-release composite material of Example 5 after 48 hours of slow-release evaluation experiment;
[0061] Figure 8 This is a view of the high-temperature resistant slow-release composite material of Example 6 after 48 hours of slow-release evaluation experiment. Detailed Implementation
[0062] The present invention will now be described in detail with reference to specific embodiments and accompanying drawings. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0063] All raw materials used in the examples are commercially available.
[0064] Comparative Examples 1-3
[0065] Sodium dodecylbenzenesulfonate (SDBS, 97%), a solid surfactant, was mixed with biodegradable polymer resins: polylactic acid (PLA) from Zhejiang Hisun Biotechnology Co., Ltd., polyglycolic acid (PGA), and polybutylene adipate terephthalate (PBAT) from BASF (model C1200). The mixtures were stirred (25 rpm) on a torque rheometer at temperatures above the resin melting point (220°C) to form uniform premixes. The premixes were then injection molded at 220°C under hot melt conditions to form composite solid rods (4g each). The experimental dosage comparison data are shown in Table 1.
[0066] The slow-release evaluation experiment was conducted as follows: 4g of the above-mentioned injection-molded composite solid rod containing surfactant was placed in a pressure-resistant bottle containing 60mL of simulated underground brine and sealed. The brine contained the following components: calcium chloride 8.37g / L, magnesium chloride 0.42g / L, sodium sulfate 1.21g / L, and sodium chloride 60.74g / L. Carbon dioxide was introduced into the simulated groundwater until saturation, simulating an acidic underground environment. The experiment was conducted at a constant temperature of 130℃, with the carbon dioxide-saturated simulated underground brine replaced every 24 hours. The sample's appearance and shape were observed.
[0067] Table 1.
[0068] Composition\Number Comparative Example 1 Comparative Example 2 Comparative Example 3 PGA 50% PLA 50% PBAT 50% SDBS 50% 50% 50% Dissolution time (in hours) in 130℃ salt water <6 <6 20
[0069] Its typical test start and sustained release evaluation test appearance are as follows Figure 1-4 As shown, Figure 1 The initial sustained-release composite material of Comparative Example 1 is shown to be a complete rod shape, while the initial sustained-release composite materials of Comparative Examples 2 and 3 have similar appearances to the initial sustained-release composite material of Comparative Example 1. Figure 1 All are intact rods; Figure 2 The slow-release composite material in Comparative Example 1 completely disintegrated and dissolved after 6 hours in the slow-release evaluation experiment. Figure 3 The slow-release composite material in Comparative Example 2 showed that it completely disintegrated and dissolved after 6 hours in the slow-release evaluation experiment. Figure 4 The slow-release composite material in Comparative Example 3 showed shrinkage and softening after 20 hours of slow-release evaluation, but a small amount remained. This indicates that PBAT maintains its properties for a longer period compared to PGA and PLA.
[0070] Comparative Examples 4-6
[0071] The method was carried out in accordance with Comparative Example 1, except that different biodegradable polymer resins were used: poly(3-hydroxybutyrate / 3-hydroxyvalerate) (PHBV) - Ningbo Tianan Company, polybutylene succinate (PBS) - PTT Chemical FZ71PB, Thailand, and polycaprolactone (PCL) - molecular weight 80,000.
[0072] The sustained-release evaluation experiment was the same as Comparative Example 1, and the dosage and dissolution time are shown in Table 2. It can be seen that the dissolution time of the composite materials prepared by PHBV, PBS, and PCL is shorter than that of PBAT: 20 hours.
[0073] Table 2.
[0074]
[0075]
[0076] Comparative Examples 7-9
[0077] The method was followed as in Comparative Example 1, except that a higher amount of surfactant (65%) was used, as shown in Table 3. It can be seen that the dissolution time of each composite material is significantly shorter compared to Comparative Examples 1-3, indicating that excessive surfactant content is detrimental to sustained-release performance.
[0078] Table 3
[0079] Composition\Number Comparative Example 7 Comparative Example 8 Comparative Example 9 PGA 35% PLA 35% PBAT 35% SDBS 65% 65% 65% Dissolution time (in hours) in 130℃ salt water <2 <2 10
[0080] Comparative Example 10 and Examples 1-3
[0081] The preparation method was the same as in Comparative Example 1, except that the raw materials used were the surfactant cocamidopropyl betaine (CAB, 97% solid content) and different contents of PBAT, and the inorganic particles were kaolin, CaCO3, and hydrophobic montmorillonite, respectively. The mixture was stirred at 155℃ (25 rpm) on a torque rheometer to form a uniform premix. The premix was then injection molded at 150℃ under hot melt conditions and cooled to form composite solid rods (4g each), resulting in a high-temperature resistant slow-release composite material. The composition and dissolution time of the high-temperature resistant slow-release composite material are shown in Table 4. It can be seen that, compared with Comparative Example 10, the addition of inorganic materials can increase the stability of the high-temperature resistant slow-release composite material and prolong the slow-release time.
[0082] Table 4
[0083]
[0084]
[0085] Examples 4-6
[0086] The method of Example 1 was followed, except that different amounts of surfactant and PBAT were used, and inorganic particles of nano-SiO2 (20-30 nm), 5-micron CaCO3, and nano-CaCO3 (10-100 nm) were used to composite the high-temperature resistant slow-release composite material. The composition and dissolution time of the high-temperature resistant slow-release composite material are shown in Table 5.
[0087] Table 5.
[0088] Composition\Sample Number Example 4 Example 5 Example 6 PBAT 75% 75% 75% <![CDATA[nano-SiO2]]> 10% <![CDATA[Micron CaCO3]]> 10% <![CDATA[Nano CaCO3]]> 10% CAB 15% 15% 15% Duration in 130℃ saline solution (hours) 48 72 96
[0089] Its typical appearance changes over time, such as Figure 5-8 As shown, Figure 5 The initial high-temperature resistant slow-release composite material of Example 4 is shown to be a complete rod shape. The initial high-temperature resistant slow-release composite materials of Examples 5 and 6 have similar appearances to the initial high-temperature resistant slow-release composite material of Example 4. Figure 5 All are intact rods; Figure 6 The high-temperature resistant slow-release composite material of Example 4 completely disintegrated after 48 hours in the slow-release evaluation experiment, forming an insoluble loose precipitate. Figure 7 The high-temperature resistant slow-release composite material of Example 5 showed that after 72 hours of slow-release evaluation experiment, it completely disintegrated and formed small dispersed precipitates. Figure 8 The high-temperature resistant slow-release composite material of Example 6 shrinks into a solid precipitate after 96 hours in the slow-release evaluation experiment. Table 5 shows that the high-temperature resistant slow-release composite materials prepared in Examples 4-6 can all maintain their release for more than 2 days, but the addition of inorganic particles, specifically micro / nano CaCO3 particles, yields better results.
[0090] Examples 4-6: Evaluation of surfactant release efficiency after release
[0091] For the released surfactants of Examples 4-6, their release efficiency was evaluated by testing their foaming volume and half-life performance.
[0092] Take 40 mL of the released solution, dilute it with water to prepare a 200 mL standard solution, and then foam it by stirring. Use a stirrer to foam the solution at a speed of 16000 rpm for 30 seconds. Measure the foam volume and half-life (the time it takes for half of the liquid volume in the foam to be separated). The results are shown in Table 6.
[0093] Table 6.
[0094]
[0095] As can be seen from Table 6, all of Examples 4-6 can maintain surfactant release for more than 48 hours, but the composite material containing micro-nano CaCO3 inorganic particles has better foam retention performance after surfactant release, indicating that its slow-release performance is better.
[0096] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0097] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A high-temperature resistant slow-release composite material comprising a biodegradable heat-resistant polymer, a surfactant, and inorganic particles; wherein the biodegradable heat-resistant polymer is polybutylene adipate terephthalate; the surfactant is at least one of anionic surfactants and amphoteric surfactants; the anionic surfactant is at least one of sodium alkyl sulfate, sodium alkyl sulfonate, sodium alkylbenzene sulfonate, and sodium alkyl taurate; the amphoteric surfactant is at least one of alkylamine oxide and alkyl betaine; the high-temperature resistant slow-release composite material is obtained by injection molding after melt blending of components including the biodegradable heat-resistant polymer, surfactant, and inorganic particles; based on 100% of the total weight of the high-temperature resistant slow-release composite material, the biodegradable heat-resistant polymer is 30-80%; the surfactant is 1-60%; and the inorganic particles are 1-50%; wherein the inorganic particles are at least one of hydrophobic montmorillonite, organobentonite, SiO2, kaolin, and CaCO3.
2. The high-temperature resistant slow-release composite material as described in claim 1, characterized in that: Based on a total weight of 100% for high-temperature resistant slow-release composite materials, The biodegradable and heat-resistant polymer content is 50-75%. Surfactant content is 5-35%; Inorganic particles account for 1-40%.
3. The high-temperature resistant slow-release composite material as described in any one of claims 1-2, characterized in that: The amphoteric surfactant is at least one of alkylamidopropylamine oxide, alkylamidopropyl betaine, and alkyl hydroxypropyl sulfobetaine.
4. The high-temperature resistant slow-release composite material as described in claim 3, characterized in that: The surfactant has an alkyl chain length of 8 to 16.
5. The high-temperature resistant slow-release composite material as described in claim 1, characterized in that: The surfactant is at least one of sodium dodecylbenzenesulfonate, sodium dodecyl sulfonate, cocamidopropyl betaine, and cocamidopropyl hydroxysulfonate.
6. The high-temperature resistant slow-release composite material as described in claim 3, characterized in that: The surfactants also include nonionic surfactants as auxiliaries.
7. The high-temperature resistant slow-release composite material as described in claim 6, characterized in that: The nonionic surfactant is an alkyl polyoxyethylene and / or an alkyl glycoside.
8. The high-temperature resistant slow-release composite material as described in claim 7, characterized in that: The alkyl polyoxyethylene is at least one of alkyl polyoxyethylene ether, alkylamine polyoxyethylene ether, and castor oil polyoxyethylene ether; and / or The alkyl glycoside has a carbon chain of C15. 8-14 Alkyl glycosides or alkyl polysaccharides.
9. The high-temperature resistant slow-release composite material as described in claim 7, characterized in that: The degree of polymerization of the alkyl polyoxyethylene is 4 to 10.
10. The high-temperature resistant slow-release composite material as described in any one of claims 1-2, characterized in that: The inorganic particles are at least one of hydrophobic montmorillonite, kaolin, and CaCO3.
11. The high-temperature resistant slow-release composite material as described in claim 1, characterized in that: The inorganic particles have a particle size of 30 nm to 5 μm.
12. The high-temperature resistant slow-release composite material as described in claim 11, characterized in that: The inorganic particles have a particle size of 30nm to 200nm.
13. A method for preparing a high-temperature resistant slow-release composite material as described in any one of claims 1-12, comprising melting and blending components including a degradable heat-resistant polymer, a surfactant, and inorganic particles, followed by injection molding to obtain the high-temperature resistant slow-release composite material.
14. The preparation method according to claim 13, characterized in that: The melt blending temperature is 140~250℃.
15. The preparation method according to claim 14, characterized in that: The melt blending temperature is 150~250℃.
16. The use of a high-temperature resistant slow-release composite material as described in any one of claims 1-12 or a high-temperature resistant slow-release composite material prepared by any one of claims 13-15 as a foaming agent.
Citation Information
Patent Citations
Environment-friendly slow-release polymer scale inhibitor and preparation method thereof
CN107304078A
Slow release type liquid-carrying and sand-carrying foam drainage agent and preparation method thereof
CN110003875A
Preparation method of controllable long-acting slow-release scale inhibitor capsule
CN110157401A
Temperature-sensitive plugging colloid for oil and gas fields, preparation method and use method thereof
CN110564388A
Composites for controlled release of well treatment agents
US20120273197A1