A polycarbonate modified material, 3D printing filament for FDM and its preparation and application
Modified materials were prepared by adding aliphatic/aromatic copolyesters and polyether ether ketones or their derivative polymers to polycarbonate raw materials, followed by blending extrusion and continuous melt extrusion. This solved the problem of high warpage of polycarbonate 3D printing materials at high temperatures, achieving improved low-temperature printing and high-temperature resistance, making them suitable for industrial production.
Patent Information
- Application Number
- CN202210734727.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-27
AI Technical Summary
Existing polycarbonate 3D printing materials have high warpage at high temperatures, and the printing conditions are harsh, leading to energy waste and problems with high-temperature resistance.
By adding aliphatic/aromatic copolyesters and polyether ether ketones or their derivative polymers to polycarbonate raw materials, modified materials are prepared through blend extrusion and continuous melt extrusion, thereby reducing printing temperature and improving the high-temperature resistance of the materials.
It achieves reduced warpage at low temperatures, improves the high-temperature resistance of materials, reduces printing energy consumption, is suitable for low-temperature 3D printing, and has a simple process suitable for industrial production.
Smart Images

Figure CN117343520B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials, specifically relating to a polycarbonate modified material, 3D printing filament for FDM, its preparation method and application. Background Technology
[0002] 3D printing is an emerging rapid prototyping technology, hailed as a "manufacturing technology of industrial revolution significance." It meets ever-increasing demands for personalization, represents a breakthrough in traditional manufacturing technologies, and is considered a technological representative of the "Third Industrial Revolution." It is widely used in industrial production, civilian applications, aerospace, military, and medical fields. It is a technology that uses digital model files as a basis and prints the desired object layer by layer. Currently, the most mature and widely used technologies are five main processes: Stereolithography Apparatus (SLA), Laminated Object Manufacturing (LOM), Fused Deposition Modeling (FDM), Selective Laser Sintering (SLS), and Selective Laser Melting (SLM). Among these five technologies, Fused Deposition Modeling (FDM) is the most widely used in terms of materials, has the longest development history, and is also capable of miniaturization and everyday use.
[0003] Currently, commonly used thermoplastic printing plastics for FDM technology include acrylonitrile-butadiene-styrene copolymer (ABS), polylactic acid (PLA), nylon (PA), high-impact polystyrene (HIPS), and polycarbonate (PC). Compared to other printing materials, PC has good transparency, insulation, and excellent mechanical properties and thermal stability, making it a high-performance engineering material. However, in 3D printing, due to the printing mechanism of FDM itself and the high processing temperature of PC, high printhead and substrate temperatures are required to achieve printing, resulting in harsh printing conditions, significant energy waste, and poor high-temperature resistance. Summary of the Invention
[0004] To address the technical problems of excessively high nozzle and substrate temperatures in existing polycarbonate printing technologies, and the need to improve the high-temperature resistance of materials, this invention provides a modified polycarbonate material and 3D printing filament for FDM. By adding aliphatic / aromatic copolyesters and polyether ether ketones or their derivative polymers to the polycarbonate raw material, excessive warpage during polycarbonate 3D printing can be avoided, thereby improving the high-temperature resistance of the printing filament.
[0005] One objective of this invention is to provide a polycarbonate-modified material, which, by weight, comprises the following components:
[0006] (1) 70-90 parts polycarbonate, preferably 75-85 parts polycarbonate;
[0007] (2) 10 to 30 parts aliphatic / aromatic copolyester, preferably 15 to 25 parts aliphatic / aromatic copolyester;
[0008] (3) 0.1 to 5 parts of polyether ether ketone or its derivative polymers, preferably 0.5 to 3 parts of polyether ether ketone or its derivative polymers.
[0009] In a preferred embodiment of the present invention, the polycarbonate is a high molecular weight polymer containing carbonate groups in its molecular chain, selected from at least one of aliphatic polycarbonate, alicyclic polycarbonate, and aromatic polycarbonate, preferably an aromatic polycarbonate. In a more preferred embodiment of the present invention, the polycarbonate is selected from bisphenol A type polycarbonate.
[0010] In a preferred embodiment of the present invention, the aliphatic / aromatic copolyester is a copolyester with a molecular chain consisting of an aliphatic diacid or its derivative, an aromatic diacid or its derivative, and an aliphatic diol. The molecular chain segment of the aliphatic / aromatic copolyester contains: a) at least one aliphatic diol unit; b) at least one of an aliphatic diacid, an aliphatic diacid anhydride, an aliphatic diacyl halide, or an aliphatic diacyl ester unit; c) at least one of an aromatic diacid, an aromatic diacid anhydride, an aromatic diacyl halide, or an aromatic diacyl ester unit. In a more preferred embodiment of the present invention, the aliphatic / aromatic copolyester is selected from polyethylene terephthalate-co-oxalate, polyethylene terephthalate-co-malonate, polyethylene terephthalate-co-succinate, polyethylene terephthalate-co-glutarate, polyethylene terephthalate-co-adipate, polyethylene terephthalate-co-octanoate, and polyethylene terephthalate-co-oxalate. Poly(propylene glycol terephthalate), poly(propylene glycol terephthalate-co-malonate), poly(propylene glycol terephthalate-co-succinate), poly(propylene glycol terephthalate-co-glutarate), poly(propylene glycol terephthalate-co-adipate), poly(propylene glycol terephthalate-co-octanoate), poly(propylene glycol terephthalate-co-sebate), poly(butylene terephthalate-co-oxalate), poly(butylene terephthalate-co-malonate) Alcohol esters, polybutylene terephthalate-co-succinate, polybutylene terephthalate-co-glutarate, polybutylene terephthalate-co-adipate, polybutylene terephthalate-co-octanoate, polyhexylene terephthalate-co-oxalate, polyhexylene terephthalate-co-malonic acid, polyhexylene terephthalate-co-succinate, polyhexylene terephthalate-co-glutarate At least one of poly(hexyl terephthalate-co-hexyl terephthalate-co-octanoate), preferably selected from at least one of poly(butylene terephthalate-co-hexyl terephthalate-co-ethylene terephthalate-co-ethylene terephthalate-co-succinate, and more preferably poly(butylene terephthalate-co-hexyl terephthalate-co-butylene terephthalate).
[0011] In a preferred embodiment of the present invention, the polyetheretherketone or its derivative polymer is a polymer composed of repeating units containing one ketone bond and two ether bonds in its main chain structure, preferably a type of polyaryl ether / polyetheretherketone polymer obtained by condensation with an aromatic diphenol. The polyetheretherketone or its derivative polymer can be a commonly used commercially available product, such as 330PF, 550PF, or 770PF produced by Jilin Zhongyan, with a powder mesh size of 100–400 mesh, preferably 150–350 mesh.
[0012] The polycarbonate modified material provided by this invention exhibits a warpage of less than 0.5m in the sample under 3D printing conditions of a nozzle temperature of 220°C and a substrate temperature of 80°C. -1 The thermogravimetric loss curve of the polycarbonate modified material shows that 50% of the thermogravimetric loss occurs above 400℃, demonstrating excellent high-temperature resistance.
[0013] The second objective of this invention is to provide a method for preparing the above-mentioned polycarbonate modified material, comprising: co-extruding a component including the polycarbonate, aliphatic / aromatic copolyester, polyether ether ketone or its derivative polymer, to obtain the polycarbonate modified material.
[0014] The extrusion method in the above-mentioned polycarbonate modified material preparation method can adopt the extrusion process commonly used in the field of polymer material processing. The process conditions and equipment are also the usual conditions and equipment in the prior art. Preferably, the twin-screw extrusion method can be used.
[0015] In a specific embodiment of the present invention, the required amounts of polycarbonate, aliphatic / aromatic copolyester, polyetheretherketone or their derivative polymers are thoroughly mixed in a mixing device, and then co-extruded in a twin-screw extruder, granulated and dried to obtain the polycarbonate modified material for 3D printing.
[0016] In the above preparation method, the blending extrusion conditions are: the blending extrusion temperature is 180-260℃, and the extruder speed is 60-200 rpm; preferably, the blending extrusion temperature is 200-250℃, and the extruder speed is 100-150 rpm; the drying conditions are: the drying temperature is 50-80℃, and the drying time is 4-8 h; preferably, the drying temperature is 55-70℃, and the drying time is 5-6 h.
[0017] The third objective of this invention is to provide a 3D printing filament for FDM, which is prepared from the above-mentioned polycarbonate modified material or the polycarbonate modified material obtained by the above-mentioned preparation method.
[0018] The FDM 3D printing filament provided by this invention allows the printhead temperature to be reduced to 220°C and the substrate temperature to 80°C while controlling the warpage curvature to within 0.5m. -1 Normal printing will not be affected.
[0019] The fourth objective of this invention is to provide a method for preparing the above-mentioned 3D printing filament for FDM, comprising continuously melting and extruding the polycarbonate modified material and then oriented and stretching it to obtain the 3D printing filament.
[0020] In a specific embodiment of the present invention, the polycarbonate modified material is melt-extruded in a screw extruder, cooled, and oriented to obtain the 3D printing filament for FDM by continuous melt extrusion; preferably, the polycarbonate modified material is melt-extruded in a single screw extruder, cooled and oriented at at least two different temperatures, and then wound to form the 3D printing filament.
[0021] In the above-mentioned method for preparing 3D printing filament, the melt extrusion conditions are: melt extrusion temperature of 205-240℃ and extruder speed of 10-15 rpm; preferably, the melt extrusion temperature is 210-225℃ and the extruder speed is 12-14 rpm; the traction frequency of the orientation stretching is 2.3-3.7, preferably 2.5-3.5.
[0022] In the above-mentioned method for preparing 3D printing filament, a cooling treatment is required after melt extrusion. This cooling treatment can employ common methods, such as water bath cooling. The cooling treatment includes at least two stages of cooling at different temperatures, with the temperature decreasing sequentially from the first stage to the last. The first stage temperature is no higher than 95°C, and the last stage is at room temperature. Preferably, the first stage cooling temperature is 65–95°C, and the last stage cooling temperature is 15–35°C; more preferably, the first stage cooling temperature is 75–90°C, and the last stage cooling temperature is 15–30°C. Utilizing two stages of water bath cooling effectively releases the internal stress of the material during cooling from the molten state, while simultaneously preventing material deformation during extrusion.
[0023] The fifth objective of this invention is to provide the above-mentioned 3D printing filament for FDM or the 3D printing filament for FDM obtained according to the above preparation method for use in low-temperature 3D printing.
[0024] In this invention, PC materials are modified by adding aliphatic / aromatic copolyesters and polyetheretherketone (PEEK) or their derivative polymers. This significantly improves the warpage of 3D printed PC materials and increases the thermal degradation temperature without affecting normal printing. Simultaneously, this invention uses PEEK or its derivatives to improve the low-temperature printing performance of PC copolyesters, effectively reducing the printing processing temperature of PC-containing 3D printing materials. This facilitates the release of internal stress in the material, reduces the difficulty of 3D printing, improves warpage of printed spline, and enhances the material's high-temperature resistance.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0026] 1. This invention reduces the excessive warpage of polycarbonate during 3D printing by adding aliphatic / aromatic copolyesters and polyether ether ketones or their derivative polymers to polycarbonate raw materials, while improving its high-temperature resistance.
[0027] 2. The 3D printing filament provided by this invention has significantly improved warping and can be used for low-temperature 3D printing;
[0028] 3. The preparation method provided by this invention is simple, suitable for industrial production, and has broad application prospects. Attached Figure Description
[0029] Figure 1 The DSC heating curves of the polycarbonate modified materials obtained in Examples 1-3 and Comparative Example 1 are shown below. Figure 1 As can be seen, compared with the polycarbonate modified material of Comparative Example 1, the glass transition temperature of the polycarbonate modified materials obtained in Examples 1-3 did not change significantly.
[0030] Figure 2 The TG thermogravimetric curves of the polycarbonate modified materials obtained in Examples 1-3 and Comparative Example 1, and PEEK are shown. The horizontal axis represents temperature, and the vertical axis represents mass percentage. Figure 2 As can be seen, compared with the polycarbonate modified material of Comparative Example 1, the polycarbonate modified materials of Examples 1 to 3 have higher thermal decomposition temperatures, with a thermal decomposition temperature of 50% weight loss above 400°C.
[0031] Figure 3 The warpage of the polycarbonate-modified material is shown on the x-axis at a base plate temperature of 100℃ and different printhead temperatures, with printhead temperature on the x-axis and warpage on the y-axis. Figure 3 It can be seen that, compared with the polycarbonate modified material of Comparative Example 1, the polycarbonate modified materials of Examples 1 to 3 have a lower warpage at the same printhead temperature.
[0032] Figure 4 The warpage of the polycarbonate-modified material is shown at a nozzle temperature of 250℃ and different substrate temperatures. The horizontal axis represents substrate temperature, and the vertical axis represents warpage. Figure 4 It can be seen that, compared with the polycarbonate modified material of Comparative Example 1, the polycarbonate modified materials of Examples 1 to 3 have a lower warpage at the same base plate temperature. Detailed Implementation
[0033] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0034] The testing instruments and conditions used in this embodiment are as follows:
[0035] Melt flow index (MFR) determination method: According to ISO 1133 standard, the Instron CEAST MF20 melt flow indexer was used for determination. The barrel temperature was 250℃, the weight load was 5kg, the die diameter was 2.095mm and the length was 8mm, the preheating time was 4min, the sample was automatically cut at set time intervals, and 5 samples were taken and the average value was calculated. The result was expressed as grams per 10 minutes (g / 10min).
[0036] Thermal performance analysis (DSC): Tests were performed on a Discovery series differential scanning calorimeter (DSC) manufactured by TA Instruments, using TA Instruments Trios version 3.1.5 software. This DSC instrument is equipped with a TARefrigerated Cooling System 90 mechanical refrigeration accessory. The test atmosphere was nitrogen at a flow rate of 50 mL / min, and the required sample volume was 5–10 mg. The test procedure was as follows: the temperature was first stabilized at 40℃, then increased to 250℃ at a rate of 10℃ / min and held at that temperature for 1 min to remove thermal history. The temperature was then decreased to -50℃ at a rate of 10℃ / min, followed by a reheat to 250℃ at a rate of 10℃ / min. The cooling process and the second heating process were recorded to study the thermal properties of the sample. The glass transition (Tg) of the sample can be directly obtained from the DSC test software. g Melting temperature (T) m Information such as ""
[0037] Thermogravimetric analysis (TGA): The test was performed on a TGA2 instrument from METTLER. Approximately 10 mg of sample was weighed and added to a crucible. The temperature was increased from 30 °C to 600 °C at a rate of 10 °C / min to analyze the thermal degradation of the material.
[0038] Warp curvature: The warp curvature C can be calculated using the following formula:
[0039]
[0040] Where: C represents the curvature of the spline, in meters (m) -1 L represents the length of the spline, in meters; represents the warping height of the spline end from the bottom horizontal plane, in meters.
[0041]
Examples 1-3
[0042] The polycarbonate (PC) used in this invention is produced by SABIC under the brand name LEXAN. TM ResinHF1130-111 was dried in a vacuum oven at 120℃ for 5 hours to remove moisture. Polybutylene terephthalate (PBAT) was manufactured by BASF, Germany, under the brand name [brand name missing]. C1200 was dried in a vacuum oven at 60℃ for 5 hours to remove moisture. Polyetheretherketone (PEEK), produced by Jilin Zhongyan Company, grade 550PF, with a mesh size of 300, was dried in a vacuum oven at 120℃ for 5 hours to remove moisture. PC / PBAT was mixed in a mixer at a mass ratio of 80 / 20 for 20 minutes. Then, 0.3 parts, 1 part, and 3 parts of PEEK powder were added to the above blend, respectively, and mixed in a mixer for 10 minutes. Granulation was performed using a Eurolab 16 co-rotating twin-screw extruder (screw diameter 16 mm, L / D ratio L / D = 40) manufactured by Thermo Fisher Scientific, USA. The extruder consists of 11 sections from the feed inlet to the die, numbered 1-11. Section 1 only serves as the feeding section and does not provide heating. The temperatures of sections 2-11 are 220℃, 220℃, 220℃, 220℃, 230℃, 230℃, 230℃, 240℃, 240℃, and 240℃, respectively, with the screw speed set at 150 rpm. During stable operation, the torque is 60% of its maximum value. The extruder is equipped with a 3mm diameter circular die. After extrusion and air cooling, the sample is chopped into cylindrical particles with a set diameter of approximately 3mm using a pelletizer. The resulting particles are named Example 1, Example 2, and Example 3, respectively. They are then dried in a 60℃ vacuum drying oven for 4 hours and packaged for later use.
[0043] [Example 4] DSC test of polycarbonate modified material
[0044] The three types of polycarbonate modified material particles obtained in Examples 1-3 above, along with the raw materials PC, PBAT, and PEEK, were subjected to differential scanning calorimetry (DSC) tests according to the steps described above. The second heating curves are shown below. Figure 1 The crystallization temperature (T) can be obtained directly from it using software. c ), melting temperature (T) m ), glass transition (T) g Information such as ) is listed in Table 1.
[0045] Table 1. Thermal performance parameters of each particle obtained from DSC results
[0046] Sample Name <![CDATA[T m (℃)]]> <![CDATA[T g (℃)]]> PC - 144.4 Example 1 - 88.6 Example 2 - 92.5 Example 3 - 95.5 PEEK 345.2 140.5 PBAT 121.4 -29.3
[0047] The polycarbonate modified material is translucent yellow. As can be seen from Table 1, the polycarbonate modified materials after blending in Examples 1-3 have only one glass transition temperature, which is between the glass transition temperatures of PC and PBAT. This confirms that PEEK is uniformly distributed in the components PC and PBAT. Moreover, within the prepared content range, the glass transition temperature gradually increases with the increase of PEEK content. Specifically, the glass transition temperature of the modified materials with the addition of 0.3% PEEK and 2% PEEK increases from 88.6℃ to 95.5℃.
[0048] [Example 5] Melt Flow Index Test of Polycarbonate Modified Materials
[0049] The three polycarbonate modified material particles obtained in Examples 1-3, as well as the PC raw material, were subjected to melt index determination in an Instron CEASTMF20 melt indexer. The results are shown in Table 2.
[0050] Table 2. Melt index of each material at 250℃ and 5kg
[0051] Sample Name Melt index / g / 10min PC 15.6 Example 1 35.2 Example 2 30.8 Example 3 27.8
[0052] As can be seen from Table 2, under the conditions of 250℃ and 5kg, with the addition of PEEK, the flowability of the blend decreased slightly within the range of 0.2% to 5%, but the change was small.
[0053] [Example 6] Thermogravimetric analysis of polycarbonate modified materials
[0054] The three types of polycarbonate modified material particles obtained in Examples 1-3 were subjected to thermogravimetric analysis using a METTLER thermogravimetric instrument. The results are shown in Table 3.
[0055] Table 3. 50% thermogravimetric loss temperatures for Examples 1-3
[0056] Sample Name Temperature (°C) PEEK 698.4 Example 1 402.7 Example 2 415.2 Example 3 456.1
[0057] As can be seen from Table 3, with the increase of PEEK content, the thermogravimetric temperature of the polycarbonate modified material when the thermogravimetric loss is 50% can be increased from 402.7℃ to 456.1℃, and in Examples 1 to 3, it is increased to above 400℃.
[0058]
Example 7
[0059] 3D printing filaments were prepared using a 3D printing filament forming extrusion line (model SHG) manufactured by Songhu Machinery Manufacturing Plant in Dongguan, China. The line consists of a single-screw extruder, two water bath cooling structures (hot and cold water baths), and a winding component. The hot water bath temperature is 85℃, and the cold water bath temperature is 25℃. A die with a diameter of approximately 2mm was used. The polycarbonate modified material particles prepared in Examples 1-3 were added to the feeder in batches, approximately 1.5kg per batch. The feeder was maintained at 80℃ and dried using forced-air drying. The diameter of the filament was controlled by adjusting the single-screw speed and roller speed, and regulating the traction frequency. Specific parameters are shown in Table 4.
[0060] Table 4. Processing conditions for 3D printing filaments
[0061] Sample Name Extrusion temperature (°C) Screw speed (rpm) Traction frequency Wire diameter (mm) PC 270 13.1 3.1 1.67-1.73 Example 1 225 11.9 2.7 1.68-1.74 Example 2 225 12.0 2.9 1.65-1.73 Example 3 225 13.7 2.8 1.66-1.75
[0062] Samples with different compositions exhibit varying glass transition temperatures and flowability. Therefore, adjustments to processing temperature, screw speed, and roller speed are necessary to control the filament diameter to approximately 1.73 mm for FDM 3D printing. The PBAT-containing polycarbonate-modified materials in Examples 1-3 can be extruded at lower temperatures, saving energy.
[0063]
Example 8
[0064] The 3D printing filament prepared in Example 7 was used for spline 3D printing on a MakerBot Replicator 2X 3D printer. The spline parameters and printing parameters are as follows: the spline dimensions were a cuboid of 150.0mm × 15.0mm × 4.0mm; the printing parameters were: standard resolution, nozzle extrusion speed of 90mm / s, moving speed of 90mm / s, spline infill rate of 100%, layer height of 200μm, nozzle temperatures set to 250℃, 240℃, 230℃, and 220℃, and substrate temperature of 100℃; alternatively, the nozzle temperature was controlled at 250℃, and the substrate temperature was set to 70℃, 80℃, 90℃, and 100℃. Under these conditions, pure PC filaments could not be printed normally, and the splines exhibited significant warping. Under the same conditions, in Examples 1, 2, and 3, when the printhead temperature was above 220°C and the substrate temperature was above 70°C, the warpage was significantly improved, and all three examples could print normally. This indicates that adding a small amount of PEEK can effectively reduce the nozzle and substrate temperatures during printing. Treating the spline as part of a circular arc, the warpage rate was calculated using the curvature calculation method, resulting in a line graph of the spline warpage rate. Figure 3 When the printed strip is placed on a flat surface, it can be observed that the warping of the strip is greatly improved as the amount of PEEK used increases.
[0065] Examples 1, 2, and 3 all exhibited excellent printing performance, with a spline curvature as low as 0.15m at a printhead temperature of 220°C and a substrate temperature of 100°C. -1 With a nozzle temperature of 250℃ and a substrate temperature of 80℃, the curvature of the sample strip was as low as 0.24m. -1 .
[0066] Comparative Example 1
[0067] The polycarbonate (PC) used in this invention is produced by SABIC under the brand name LEXAN. TM ResinHF1130-111. Polybutylene terephthalate (PBAT) is manufactured by BASF AG, Germany, and its brand name is [not specified]. C1200. The two types of particles were first dried in vacuum ovens at 120℃ and 60℃ respectively for 4 hours to remove moisture. They were then mixed in a mixer at a matrix resin mass ratio of 80 / 20 (PC / PBAT) for 20 minutes. Granulation was performed using a Eurolab16 co-rotating twin-screw extruder (screw diameter 16mm, L / D ratio L / D = 40) manufactured by Thermo Fisher Scientific, Inc. This extruder has 11 sections from the feed port to the die, numbered 1-11. Section 1 only serves as the feeding section and does not provide heating. The temperatures of sections 2-11 of the extruder are 210℃, 220℃, 230℃, 230℃, 230℃, 240℃, 240℃, 240℃, 240℃, and 240℃ respectively, with the screw speed set at 100 rpm. During stable operation, the torque is 60% of its maximum value. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample is extruded from the die and cooled by air, it is cut into cylindrical particles with a set diameter of about 3 mm by a pelletizer. The above particles are named Comparative Example 1. After granulation, they are dried in a vacuum drying oven at 60°C for 4 hours and then packaged for later use.
[0068] The above-mentioned sample (Comparative Example 1) was prepared using a 3D printing filament extrusion line (model SHG) manufactured by Songhu Machinery Manufacturing Plant in Dongguan, China. Approximately 1.5 kg of sample was added, and the feeder was maintained at 80°C with forced-air drying. The single screw speed was adjusted to 12.5 rpm and the roller speed was adjusted, and the traction frequency was adjusted to 3.0 to control the filament diameter. The final filament diameter was 1.68–1.76 mm.
[0069] Spline 3D printing was performed on a MakerBot Replicator 2X 3D printer. The spline and printing parameters are as follows: the spline size is a cuboid of 150.0mm × 15.0mm × 4.0mm, the printing parameters are as follows: standard resolution, nozzle extrusion speed of 90mm / s, moving speed of 90mm / s, spline infill rate of 100%, height of each layer of 200μm, nozzle temperature set to 250℃, 240℃, 230℃, and 220℃, and base plate temperature of 100℃; simultaneously, the nozzle temperature is controlled at 250℃, and the base plate temperature is set to 80℃, 90℃, and 100℃. Under these conditions, PC-20%PBAT (Comparative Example 1) can control the curvature to below 1 when the printhead temperature is 240-250°C. When the printhead temperature drops to 220-230°C, the curvature increases significantly, to more than two to three times that of the polycarbonate modified materials obtained in Examples 1-3, making normal printing impossible. When the substrate temperature drops to 90°C, normal printing is also impossible.
[0070] Comparative Example 2
[0071] The polycarbonate (PC) used in this invention is produced by SABIC under the brand name LEXAN. TM ResinHF1130-111 was dried in a vacuum oven at 120℃ for 5 hours to remove moisture. Polybutylene terephthalate (PBAT) was manufactured by BASF, Germany, under the brand name [brand name missing]. C1200. Drying was performed in a 60℃ vacuum oven for 5 hours to remove moisture. Polyetheretherketone (PEEK) was produced by Jilin Zhongyan Company, grade 550PF, with a mesh size of 300. It was dried in a 120℃ vacuum oven for 5 hours to remove moisture. PC / PBAT was mixed in a mixer at a mass ratio of 80 / 20 for 20 minutes; subsequently, 10 parts of PEEK powder were added to the PC blend and mixed in a mixer for 10 minutes. Granulation was performed using a Eurolab 16 co-rotating twin-screw extruder (screw diameter 16mm, L / D ratio L / D = 40) manufactured by Thermo Fisher Scientific, USA. This extruder has 11 sections from the feed port to the die, numbered 1-11, where section 1 only serves as the feeding section and does not provide heating. The temperatures of extruder sections 2-11 were 230℃, 240℃, 240℃, 240℃, 250℃, 250℃, 250℃, 260℃, 260℃, and 260℃, respectively, with the screw speed set at 100 rpm. During stable operation, the torque was 60% of its maximum value. The extruder was equipped with a 3mm diameter circular die. After extrusion and air cooling, the sample was granulated into cylindrical particles with a set diameter of approximately 3mm using a pelletizer. These particles were named Comparative Example 2. After granulation, they were dried in a 60℃ vacuum drying oven for 4 hours and then packaged for later use.
[0072] Comparative Example 2 of the above sample was tested for melt flow index in an Instron CEAST MF20 melt flow indexer. The result was 18.5 g / 10 min, which does not meet the conditions for 3D printing filament preparation. The fluidity is insufficient and it cannot be used for 3D printing.
Claims
1. A polycarbonate-modified material, comprising the following components by weight: (1) 70-90 parts polycarbonate; (2) 10-30 parts of aliphatic / aromatic copolyester, wherein the aliphatic / aromatic copolyester is selected from polyethylene terephthalate-co-oxalate, polyethylene terephthalate-co-malonate, polyethylene terephthalate-co-succinate, polyethylene terephthalate-co-glutarate, polyethylene terephthalate-co-adipate, polyethylene terephthalate-co-octanoate, polyethylene terephthalate-co-oxalate, polyethylene terephthalate-co-malonate, polyethylene terephthalate-co-succinate, polyethylene terephthalate-co-glutarate, polyethylene terephthalate-co-adipate, and polyethylene terephthalate-co-octanoate. At least one of the following: propylene glycol ester, poly(propylene sebate) terephthalate, poly(butylene terephthalate) terephthalate, poly(butylene terephthalate) terephthalate, poly(butylene terephthalate) terephthalate, poly(butylene terephthalate) terephthalate, poly(butylene terephthalate) terephthalate, poly(hexylene terephthalate) terephthalate, poly(hexylene terephthalate) terephthalate, poly(hexylene terephthalate) terephthalate, poly(hexylene terephthalate) terephthalate, and poly(hexylene terephthalate) terephthalate. (3) 0.1 to 5 parts of polyether ether ketone, wherein the polyether ether ketone is a polyarylether / polyether ether ketone polymer obtained by condensation with aromatic diphenols.
2. The polycarbonate-modified material according to claim 1, characterized in that, The polycarbonate modified material, by weight, comprises the following components: (1) 75-85 parts polycarbonate; (2) 15-25 parts aliphatic / aromatic copolyester; (3) 0.5 to 3 parts of polyether ether ketone.
3. The polycarbonate-modified material according to claim 1, characterized in that, The polycarbonate is selected from at least one of aliphatic polycarbonate, alicyclic polycarbonate, and aromatic polycarbonate.
4. The polycarbonate-modified material according to claim 3, characterized in that, The polycarbonate mentioned is an aromatic polycarbonate.
5. The polycarbonate-modified material according to claim 4, characterized in that, The polycarbonate mentioned is selected from bisphenol A type polycarbonate.
6. The polycarbonate-modified material according to any one of claims 1 to 5, characterized in that, The warpage of the polycarbonate-modified material specimen is less than 0.5m under the conditions of a 3D printing nozzle temperature of 220℃ and a substrate temperature of 80℃. -1 .
7. A method for preparing the polycarbonate modified material according to any one of claims 1 to 6, comprising: The polycarbonate-modified material is obtained by co-extruding the components including the polycarbonate, aliphatic / aromatic copolyester, and polyether ether ketone.
8. The preparation method according to claim 7, characterized in that, The conditions for the blending extrusion are: blending extrusion temperature 180~260℃, extruder speed 60~200 rpm.
9. The preparation method according to claim 8, characterized in that, The conditions for the blending extrusion are: blending extrusion temperature 200~250℃, extruder speed 100~150 rpm.
10. A 3D printing filament for FDM, prepared from the polycarbonate modified material according to any one of claims 1 to 6 or the polycarbonate modified material obtained by the preparation method according to any one of claims 7 to 8.
11. A method for preparing the 3D printing filament for FDM as described in claim 10, comprising continuously melt-extruding the polycarbonate modified material and then oriented drawing to obtain the 3D printing filament for FDM.
12. The preparation method according to claim 11, characterized in that, The conditions for the melt extrusion are: melt extrusion temperature 205~240℃, extruder speed 10~15 rpm; and / or, The traction frequency of the orientation stretching is 2.3~3.7; and / or, The melt extrusion process requires further cooling.
13. The preparation method according to claim 12, characterized in that, The conditions for the melt extrusion are: melt extrusion temperature 210~225℃, extruder speed 12~14 rpm; and / or, The traction frequency of the orientation stretching is 2.5~3.
5.
14. The preparation method according to claim 12, characterized in that, The cooling process includes at least two stages of cooling at different temperatures, with the temperature decreasing sequentially from the first stage to the last.
15. The preparation method according to claim 14, characterized in that, In the cooling process, the first stage of cooling has a temperature of 65~95℃, and the last stage of cooling has a temperature of 10~35℃.
16. The preparation method according to claim 15, characterized in that, In the cooling process, the first cooling stage has a temperature of 75~90℃, and the last cooling stage has a temperature of 15~30℃.
17. A 3D printing filament for FDM as described in claim 10, or a 3D printing filament for FDM obtained by the preparation method described in any one of claims 11 to 16, for use in low-temperature 3D printing.
Citation Information
Patent Citations
Combined resin 3d printing wire and preparation method thereof
CN109280992A
Low-printing-temperature polycarbonate modified material for 3D printing as well as preparation method and printing wire thereof