Thermochromic elastomers and methods for their preparation
Co-ION/PDMS composites were prepared by solvothermal reaction and freeze-drying, solving the problem of combining the mechanical properties of PDMS with thermochromic materials. This enabled the large-scale mass production of composite materials with improved mechanical properties and thermochromic properties, suitable for adaptive camouflage, temperature indicators and marine engineering.
Patent Information
- Application Number
- CN202311281021.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-27
AI Technical Summary
How to combine thermochromic materials with common commercial elastomers such as PDMS to improve their mechanical properties and achieve large-scale production, and solve the problems of difficult uniform dispersion of fillers and high equipment requirements in existing technologies.
Co-ION wet gel was synthesized by solvothermal reaction, and Co-ION aerogel was prepared by solvent exchange and freeze drying. Co-ION aerogel was then compounded with PDMS to form a Co-ION/PDMS composite. By utilizing the thermochromic properties of Co-ION aerogel and the mechanical properties of PDMS, a composite material with good mechanical and thermochromic properties was prepared.
The mechanical properties of the Co-ION/PDMS composite have been significantly improved, with the maximum compressive stress, maximum tensile strain, and maximum tensile stress being 1.44 times, 1.65 times, and 1.47 times that of pure PDMS, respectively. At the same time, it retains thermochromic properties, making it suitable for complex scenarios such as adaptive camouflage, temperature indicators, and marine engineering.
Smart Images

Figure CN117343542B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a thermochromic elastomer and its preparation method, belonging to the technical field of thermochromic materials. Background Technology
[0002] Thermochromic materials are special materials that change color with temperature. They exhibit different colors at different temperatures and have broad application potential. The color change of these materials is due to variations in their crystal structure, ligand structure, or molecular arrangement at different temperatures. Reversible thermochromic materials are the mainstream, as they can be recycled multiple times, leading to extensive research and applications in color indication, temperature measurement, sensors, and medical imaging. Currently, thermochromic materials also face some challenges. For large-scale production and commercial applications, the manufacturing cost of thermochromic materials is a key issue. If common commercial elastomers can be endowed with good mechanical properties and thermochromic properties, the cost problem can be solved while achieving thermochromic functionality.
[0003] One common method for reversibly changing the color of thermochromic materials is to utilize the reversible adsorption and desorption of coordinated water molecules within the material during heating and cooling to achieve reversible changes between crystal structures. This leverages the differences in light absorption at different wavelengths by different crystal structures to achieve reversible macroscopic color changes. Research has shown that Co... 2+ The ligand structure can achieve reversible transformation between coordination octahedra and coordination tetrahedra during the adsorption and desorption of water molecules, and exhibits differences in absorbance for different wavelengths of light. However, combining this thermochromic phenomenon with ordinary elastomers has always been a challenge.
[0004] Polydimethylsiloxane (PDMS), a commonly used elastomer, is renowned for its excellent flexibility, biocompatibility, and optical transparency, finding wide applications in biomedical engineering and flexible electronics. While PDMS offers numerous advantages as a commercial material, its use in thermochromic materials remains challenging, namely, how to improve its mechanical properties and impart thermochromic functionality. Previous studies have attempted to enhance the mechanical properties of PDMS through methods including adding reinforcing fillers, surface modification via plasma treatment or chemical functionalization, and advanced processing techniques such as soft lithography. Although these methods improve mechanical properties, they still suffer from limitations such as difficulty in uniformly dispersing fillers and the high demand for specialized equipment, restricting large-scale production.
[0005] Therefore, how to endow common commercial elastomers with good mechanical properties and thermochromic properties in a simple and effective way to achieve large-scale production has always been a concern. Summary of the Invention
[0006] This invention provides a thermochromic elastomer and its preparation method, which can effectively solve the above-mentioned problems. The invention is achieved as follows:
[0007] A method for preparing a thermochromic elastomer includes the following steps:
[0008] S1, after mixing cobalt acetylacetonate, benzoic acid and benzyl alcohol evenly, put them into a container and place them in a reaction vessel, heat and keep warm, and after cooling to room temperature, a wet gel is obtained.
[0009] S2, Immerse the wet gel in the soaking solution and change the soaking solution at intervals. The soaking solution contains cyclohexane or tert-butanol.
[0010] S3, freeze the wet gel into a solid state, and then freeze-dry it to obtain an aerogel;
[0011] S4, prepare polydimethylsiloxane dispersion;
[0012] S5. Immerse the aerogel in a polydimethylsiloxane dispersion and let it stand. After the aerogel has fully absorbed the dispersion, take it out and perform a curing treatment to obtain the thermochromic elastomer.
[0013] As a further improvement, in step S1, the molar concentration of cobalt acetylacetonate is 12-160 mM; the molar ratio of cobalt acetylacetonate to benzoic acid is (0.01-0.3):(0.05-1).
[0014] As a further improvement, in step S1, the heating and holding is to heat to 100-300°C at a heating rate of 2-10°C / min and hold for 5-24 hours.
[0015] As a further improvement, in step S2, the soaking time is 5 to 30 days, and the soaking solution is changed every 0.5 to 5 days.
[0016] As a further improvement, in step S3, the parameters for freeze drying are: freezing temperature -20 to -100°C, air pressure set to 30 to 100 Pa, and time set to 12 to 96 h.
[0017] As a further improvement, in step S4, the step of preparing the polydimethylsiloxane dispersion is as follows: mix polydimethylsiloxane and curing agent and stir evenly, then add n-hexane and continue stirring to obtain the polydimethylsiloxane dispersion.
[0018] As a further improvement, the mass ratio of the polydimethylsiloxane to the curing agent is 8 to 12:1.
[0019] As a further improvement, in step S5, the standing time is 6 to 48 hours; the curing temperature is 30 to 100°C, and the time is 2 to 12 hours.
[0020] As a further improvement, in step S5, the ratio of cobalt acetylacetonate to polydimethylsiloxane is 1.2–16 mmol: 5–8 g.
[0021] A thermochromic elastomer prepared by the above method.
[0022] The beneficial effects of this invention are:
[0023] This invention successfully synthesizes a cobalt-based inorganic-organic nanobelt (Co-ION) / PDMS elastic composite using a novel and simple method, resulting in significantly improved mechanical properties. The maximum compressive stress, maximum tensile strain, and maximum tensile stress are 1.44 times, 1.65 times, and 1.47 times that of pure PDMS, respectively. The improved mechanical properties also enhance the material's processability; this method enables the fabrication of one-dimensional, two-dimensional, and three-dimensional composites and allows for large-scale production.
[0024] The Co-ION / PDMS elastic composite prepared by this invention successfully retains the thermochromic properties derived from Co-ION aerogel, and its thermochromic properties are superior to those of Co-ION aerogel. The Co-ION / PDMS composite can achieve reversible thermochromic properties between 25℃ and 120℃, which can be achieved by controlling the Co content in the aerogel. 2+ The content of [specific ingredient] allows the prepared composite to exhibit different absorption intensities in the wavelength range of 350-800 nm, resulting in different shades of color, and the color changes are more significant than those of Co-ION aerogel. This invention successfully endows the common commercial elastomer PDMS with good mechanical properties and thermochromic properties in a simple and effective way, thereby enabling large-scale mass production and providing possibilities for applications in complex scenarios such as adaptive camouflage, temperature indicators, and marine engineering. Attached Figure Description
[0025] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.
[0026] Figure 1Photographs showing the preparation process of Co-ION aerogel. (a) Precursor solution of cobalt acetylacetonate and benzoic acid dissolved in benzyl alcohol; (b) Co-ION wet gel obtained after heating; (c) Photograph of the wet gel after being removed from the glass liner; (d) Co-ION aerogel obtained after solvent exchange and freeze-drying.
[0027] Figure 2 Photographs of the Co-ION / PDMS composite. (a) Co-ION aerogel; (b) PDMS; (c) Co-ION / PDMS composite.
[0028] Figure 3 Density diagrams of Co-ION aerogel, PDMS, and Co-ION / PDMS composites.
[0029] Figure 4 Photographs showing the Co-ION / PDMS composite cut into one-dimensional, two-dimensional, and three-dimensional structures.
[0030] Figure 5 Fourier transform infrared spectra of Co-ION aerogel and Co-ION / PDMS composite.
[0031] Figure 6 Scanning electron microscope images of the Co-ION / PDMS complex at different magnifications.
[0032] Figure 7 Photographs of the Co / P-75mM complex on hot stages at 25, 50, 60 and 120°C.
[0033] Figure 8 Thermochromic photographs of Co-ION / PDMS composites at different temperatures (around 25°C and around 60°C): (ab) photographs of the composites cut into triangular prisms and cuboids; (cd) photographs of large composite sheets laid flat and bent; (e) woven fabrics made from strips of Co-ION / PDMS composites.
[0034] Figure 9 The diagrams show the fading process of Co-ION aerogel, where (ac) represents the fading process of Co-ION aerogel suspended in air on a 60°C hot stage; and (df) represents the fading process of Co-ION aerogel in water at 60°C.
[0035] Figure 10 This image shows a comparison of the fading process of heated Co-ION aerogel and Co-ION / PDMS composite.
[0036] Figure 11 A faded photograph of the Co-ION / PDMS complex.
[0037] Figure 12 Photographs of Co / P-25mM and Co / P-75mM on hot surfaces at 25°C and 120°C.
[0038] Figure 13 The images show the UV-Vis spectra of the complex at different temperatures, where (a) is the UV-Vis spectrum of the Co / P-75mM complex at different temperatures; and (b) is the UV-Vis spectrum of Co / P-25mM and Co / P-75mM at 120℃.
[0039] Figure 14 The absorption peaks of Co / P-25mM and Co / P-75mM at 635nm wavelength are shown as a function of temperature.
[0040] Figure 15 Geometry diagrams for (a) the cylindrical model and (b) the dumbbell model prepared as a tensile specimen.
[0041] Figure 16 The figures show the mechanical properties of the materials. Among them, (a) are the compressive stress-strain curves of PDMS and the composite; (b) are the tensile stress-strain curves of PDMS and the composite; and (c) are the mechanical properties of the Co-ION / PDMS composite compared with those of Co-ION aerogel and PDMS.
[0042] Figure 17 This is a schematic diagram illustrating the application of the Co-ION / PDMS complex in cup wall temperature indication.
[0043] Figure 18 This is a schematic diagram illustrating the application of Co-ION aerogel and Co-ION / PDMS composites in the field of adaptive camouflage.
[0044] Figure 19 This is a schematic diagram illustrating the application of the Co-ION / PDMS composite in leak detection. Detailed Implementation
[0045] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to represent selected embodiments of the invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0046] This invention provides a method for preparing a thermochromic elastomer, comprising the following steps:
[0047] S1, after mixing cobalt acetylacetonate, benzoic acid and benzyl alcohol evenly, put them into a container and place them in a reaction vessel, heat and keep warm, and after cooling to room temperature, wet gel is obtained; this method is an in-situ gelation method based on solvothermal reaction to synthesize Co-ION wet gel monomer with good mechanical properties.
[0048] S2, Immerse the wet gel in the soaking solution, and replace the soaking solution at intervals to complete the solvent exchange, thereby replacing benzyl alcohol in the wet gel; the soaking solution contains cyclohexane or tert-butanol; the difference between using tert-butanol and using cyclohexane for solvent exchange is that the tert-butanol solvent needs to be kept at a constant temperature of 30°C (the melting point of tert-butanol is 25.7°C), and the other steps are the same as the steps for solvent exchange using cyclohexane.
[0049] To prepare morphologically intact aerogels and ensure the integrity of the colloidal structure, the benzyl alcohol solvent in the wet gel needs to be replaced with a solvent with a higher melting point and saturated vapor pressure before freeze-drying. Although benzyl alcohol can be frozen at -15°C, its extremely low saturated vapor pressure (only 0.026 kPa at room temperature) means it can only sublimate under extremely high vacuum, which is difficult to achieve in commercial freeze dryers. Therefore, to facilitate the freeze-drying process, this method selects cyclohexane and tert-butanol, with melting points of 6.5°C and saturated vapor pressures of 12.46 kPa and 6.11 kPa at room temperature, respectively, as solvents for replacement.
[0050] S3. The wet gel was frozen into a solid state and then freeze-dried under vacuum to obtain an aerogel (Co-ION aerogel). This Co-ION aerogel is a cobalt inorganic-organic hybrid nanoribbon aerogel, which exhibits almost no volume shrinkage compared to the wet gel before freezing. The Co-ION aerogel displays excellent thermochromic properties. Vacuum freeze-drying can avoid significant volume shrinkage and structural collapse of the dried colloid. If an oven drying at atmospheric pressure is used, the presence of liquid surface tension or capillary forces during the drying process will destroy the three-dimensional network-like porous structure inside the aerogel, causing the aerogel to shrink and ultimately leading to the collapse of the overall structure.
[0051] S4, prepare polydimethylsiloxane dispersion.
[0052] S5. The aerogel is placed in a polydimethylsiloxane dispersion and allowed to stand. After the aerogel has fully absorbed the dispersion, it is removed and cured to obtain the thermochromic elastomer. Co-ION aerogel has a complete microscopic three-dimensional network pore structure but poor mechanical properties and is brittle. PDMS polymer monomers, on the other hand, have strong mechanical properties. In the Co-ION / PDMS composite, PDMS is uniformly filled in the three-dimensional network framework structure of the Co-ION aerogel. The combination of the two has a synergistic effect, resulting in a significant enhancement of the mechanical properties of the Co-ION / PDMS composite compared to pure PDMS.
[0053] This thermochromic flexible composite is composed of cobalt inorganic-organic hybrid nanoribbons (with the composition Co(OH)(C6H5COO)·nH2O, where n is 0.5–3, preferably 0.5) and polydimethylsiloxane. It exhibits thermochromic properties, appearing pink at room temperature and turning blue upon heating to 50°C (not exceeding 120°C), with the blue color deepening with increasing temperature. The cobalt inorganic-organic hybrid nanoribbons have a high aspect ratio, with a length of approximately 10–20 μm and a width of approximately 100–300 nm. The aerogel monomers formed by the self-entanglement of the nanoribbons possess high specific surface area and high porosity, and their shape is controllable.
[0054] As a further improvement, in step S1, the molar concentration of cobalt acetylacetonate is 12-160 mM; the molar ratio of cobalt acetylacetonate to benzoic acid is (0.01-0.3):(0.05-1). While maintaining a constant molar ratio of cobalt acetylacetonate to benzoic acid, different molar concentrations of cobalt acetylacetonate can prepare Co-ION aerogels of different densities, thereby adjusting the specific surface area, porosity, and mechanical properties of the aerogel. Simultaneously, Co-ION aerogels of different densities allow the prepared Co-ION / PDMS composite to exhibit different absorption intensities in the wavelength range of 350-800 nm. This discoloration phenomenon is mainly due to the volatilization of coordinated water molecules during heating, causing the Co... 2+Coordination octahedral to Co 2+ Coordination tetrahedral transformation leads to significant differences in wavelength absorption by the complex at different temperatures. This is due to the influence of Co. 2+ The color-changing properties of the prepared composites varied significantly depending on the concentration of Co. 2+ As the concentration of the compound increases, the color of the compound gradually deepens. Without heating, the color of the compound gradually transitions from light pink to dark pink; when the heating temperature is 120℃, the color of the compound transitions from light blue to dark blue.
[0055] As a further improvement, in step S1, the heating and holding process involves heating to 100–300°C at a heating rate of 2–10°C / min and holding for 5–24 hours, more preferably at 150°C for 12 hours. The reaction temperature and time are crucial. At this temperature, if the reaction time is too short, the length of the formed inorganic-organic nanoribbons will be insufficient to achieve effective cross-linking and entanglement, resulting in a wet gel with low mechanical strength. If the reaction time is too long, it will increase the preparation time and cost, without significantly improving the mechanical properties of the resulting wet gel.
[0056] As a further improvement, in step S2, the soaking time is 5 to 30 days, with the soaking solution being changed every 0.5 to 5 days. More preferably, the soaking time is 10 days, with the soaking solution being changed every 1 day. These parameters are sufficient to completely displace the benzyl alcohol from the wet gel.
[0057] As a further improvement, in step S3, the parameters for vacuum freeze-drying are: freezing temperature -20 to -100°C, more preferably -50°C; gas pressure set to 30 to 100 Pa, more preferably 60 Pa; and time of 12 to 96 hours, more preferably 60 hours. These vacuum freeze-drying parameters can minimize significant volume shrinkage and structural collapse of the dried colloid.
[0058] As a further improvement, in step S4, the step of preparing the polydimethylsiloxane dispersion is as follows: The polydimethylsiloxane adhesive and the curing agent are mixed and stirred evenly, then n-hexane solution is added, and stirring is continued to obtain the polydimethylsiloxane dispersion. The mass ratio of the polydimethylsiloxane adhesive to the curing agent is 8–12:1, more preferably 10:1. The ratio of the total mass of the polydimethylsiloxane adhesive and the curing agent to n-hexane is 5–10 g: 5–40 mL. The polydimethylsiloxane adhesive and the curing agent are taken and stirred for 5–20 min, preferably 10 min; n-hexane is added, and stirring is continued for 5–20 min, preferably 10 min. Under these parameters, the polydimethylsiloxane can be fully dissolved in n-hexane, facilitating its composite with Co-ION aerogel.
[0059] As a further improvement, in step S5, the standing time is 6 to 48 hours, preferably 10 hours; the curing temperature is 30 to 100°C, preferably 60°C, and the time is 2 to 12 hours, preferably 6 hours.
[0060] As a further improvement, the ratio of cobalt acetylacetonate to polydimethylsiloxane is 1.2–16 mmol: 5–8 g. Within this ratio, PDMS can be uniformly filled into Co-ION aerogels of different densities. The three-dimensional framework structure inside the Co-ION aerogel provides strong support for the PDMS polymer, resulting in a synergistic effect between the Co-ION aerogel and PDMS in terms of mechanical properties. If this ratio is exceeded, the mechanical properties of the Co-ION / PDMS composite are greatly weakened.
[0061] A thermochromic elastomer prepared by the above method. This thermochromic elastomer has good mechanical properties and thermochromic properties, and can be applied in fields such as temperature sensing, pressure sensing, and color-changing camouflage.
[0062] Example 1
[0063] (1) Preparation of cobalt inorganic-organic hybrid nanobelt aerogel
[0064] Preparation of wet gel:
[0065] like Figure 1 As shown, cobalt acetylacetonate and solid benzoic acid were added to 10 mL of benzyl alcohol solution. The mixture was stirred for 30 minutes until homogeneous, then poured into a glass liner and placed in a 50 mL Teflon container. Finally, the container was placed in a stainless steel reactor, sealed, and placed in an oven. The reactor was heated to 150 °C (heating rate 5 °C / min) and held at that temperature for 12 h. After cooling in the oven, the Co-ION wet gel was obtained, exhibiting stable mechanical properties. In this system, the concentrations of cobalt acetylacetonate were 12.5, 25.0, 37.5, 50.0, 75.0, and 150 mM, and the molar ratio of cobalt acetylacetonate to benzoic acid needed to be controlled at 1:4. Changing the specific amounts of both could yield wet gels of different densities.
[0066] Preparation of large-size samples:
[0067] Prepare 30 mL and 90 mL solutions of 25.0 mM cobalt acetylacetonate, respectively, and transfer them to 250 mL and 500 mL Teflon containers. Place these containers in a stainless steel reactor and then transfer them to an oven for heating. The heating conditions are the same as in the previous section, which will yield large-sized Co-ION wet gels.
[0068] Converting wet gels into aerogels:
[0069] The wet gel was immersed in cyclohexane for 10 days, with the cyclohexane replaced every other day to perform solvent exchange and displace benzyl alcohol from the wet gel. After solvent exchange, the wet gel was frozen into a solid state using liquid nitrogen, and then freeze-dried using a vacuum freeze dryer at -50°C, 80 Pa, and for 48 hours. The resulting Co-ION aerogel (e.g., ...) was then obtained. Figure 1 d).
[0070] Preparation of PDMS solution:
[0071] Mix 60g of Dow Corning Sylgard 184 PDMS base adhesive (PDMS) and 6g of curing agent together and stir for 10 minutes to ensure thorough mixing. Pour in 200mL of n-hexane and stir for 10 minutes to ensure that the PDMS and n-hexane solution are fully miscible. The PDMS solution is now ready.
[0072] Preparation of Co-ION / PDMS complex:
[0073] The prepared Co-ION aerogel was placed in a PDMS solution and then placed in a fume hood for 24 hours. During this process, n-hexane gradually evaporated. After evaporation was complete, a solid Co-ION / PDMS composite was obtained. Next, the composite was placed in an oven and cured at 60°C for 6 hours. The Co-ION aerogel and the Co-ION / PDMS composite were named Co-x and Co / Px, respectively, where x represents the concentration of cobalt acetylacetonate precursor used in the synthesis of the Co-ION aerogel (if the concentration of cobalt acetylacetonate used in this system is 75.0 mM, the corresponding aerogel is named Co-75 mM, and the corresponding composite is named Co / P-75 mM). Unless otherwise specified, the aerogel and composite mentioned below are referred to as Co-75 mM and Co / P-75 mM, respectively.
[0074] Preparation of large-size thin films of Co-ION / PDMS composite:
[0075] First, large-size aerogels need to be prepared. The preparation process is the same as above, except that after the wet gel is prepared, it is cut into 3mm thick slices and solvent exchange is performed to obtain aerogel slices of the corresponding size. Next, these slices are processed repeatedly according to the preparation process of the flexible thermochromic elastomer described above to obtain Co-ION / PDMS composite slices.
[0076] Preparation of tensile specimens of Co-ION / PDMS composite:
[0077] like Figure 15As shown, the tensile specimens were prepared according to the national standard GB / T-528IV, dumbbell shape. First, the prepared large-sized Co-ION aerogel sheets were placed in a 20 cm diameter glass petri dish, which was then filled with PDMS solution. Next, the above process for preparing the Co-ION / PDMS composite was repeated. This yielded some large-sized Co-ION / PDMS composite sheets, as well as some pure PDMS sheets. Finally, the large-sized Co-ION / PDMS composite sheets were cut into the shapes shown in the diagram using a mold. For comparison, pure PDMS sheets were also cut into the same shapes during the preparation process.
[0078] Example 2
[0079] In Example 2, tert-butanol was chosen as the organic solvent for solvent exchange instead of cyclohexane. The main difference between solvent exchange using tert-butanol and using cyclohexane lies in temperature control. The tert-butanol must be placed on a hot plate and the solvent temperature must be maintained at 30°C (the melting point of tert-butanol is 25.7°C). Apart from this, the remaining steps are the same as those for solvent exchange using cyclohexane. Other operations are the same as in Example 1.
[0080] Test case
[0081] The following tests were performed on the sample from Example 1:
[0082] (1) Thermochromic performance test
[0083] Thermochromic properties of Co-ION aerogel: The aerogel prepared with 25.0 mM cobalt acetylacetone was placed on a Shimadzu UV3600 for testing. The testing equipment is equipped with an integrating sphere and an in-situ heating device. The absorption spectrum in the wavelength range of 350-800 nm was measured at room temperature, and then the visible spectrum of the aerogel was measured by in-situ heating to 150 °C.
[0084] The Co-ION / PDMS composite was cut into 1.5 mm thick slices. The slices were then heated to the target temperature on a hot plate and held for 3 min. The slices were then quickly transferred to a UV-Vis spectrophotometer (with an integrating sphere). The UV-Vis spectrum was measured after heating in the wavelength range of 350-800 nm. The changes in the absorption spectral intensity at different temperatures were observed. The scan rate was 5 nm / s.
[0085] (2) Thermogravimetric analysis test
[0086] The prepared Co-ION / PDMS composite block was placed in the thermogravimetric analyzer, and the air flow rate was set to 120 mL / min and the heating rate to 20 °C / min.
[0087] (3) Mechanical performance testing
[0088] Uniaxial compression tests were conducted on pure PDMS, Co-ION aerogel, and Co-ION / PDMS composite samples at a compression rate of 4 mm / min, compressing the aerogel to 90% of its original height. The resulting FS data were converted into stress-strain curves.
[0089]
[0090] Where σ is the compressive stress, F is the pressure applied to the aerogel by the testing machine, and R is the radius of the compressed sample perpendicular to the compression direction.
[0091] Uniaxial tensile tests were performed on the Co-ION / PDMS composite. Before testing, the thickness of the thinnest point in the middle of the dumbbell-shaped sample was measured to determine the tensile stress. The tensile rate was set to 20 mm / min, and the sample length was entered as 12 mm and the width as 2 mm before each measurement. The experimental results are as follows: Figures 3 to 19 As shown.
[0092] The experimental results are analyzed as follows:
[0093] The average densities of Co-ION aerogel and PDMS monomer are approximately 0.02 g / cm³. 3 and 1.05g / cm 3 The average density of the complex is approximately 0.91 g / cm³. 3 ( Figure 3 This indicates that the majority of the porous structure inside the aerogel is filled with PDMS. The Co-ION / PDMS composite can be cut into one-dimensional, two-dimensional, and three-dimensional shapes. The composite exhibits flexibility and stretchability, allowing for large-angle twisting and bending. Figure 4 Fourier transform infrared spectroscopy (FTIR) clearly demonstrated the structure of the composite containing both nanoribbons and PDMS. Figure 5 ), of which, located at 2961cm -1 The sharp peak belongs to the stretching vibration of the -CH3 group; it is located at 1257 cm⁻¹. -1 and 788cm -1 The absorption peak represents the stretching vibration of the Si-CH3 bond; it is located at 10¹⁵ cm⁻¹. -1 and 1062cm -1 The absorption band at 1410 cm⁻¹ is a typical stretching vibration of the Si-O-Si bond; while at 1410 cm⁻¹... -1 Up to 1603cm -1 And 661cm -1 Up to 754cm -1The absorption band originates from the aromatic ring of Co-ION. Notably, due to the dominant content of PDMS in the complex, the Fourier transform infrared peak belonging to the aerogel in the shown FTIR spectrum is significantly weakened, while the PDMS signal remains prominent. The perfect integration of Co-ION and PDMS can be clearly observed in the scanning electron microscope (SEM) images. Figure 6 The black area circled by the dashed line represents the PDMS polymer, while the linear curves represent Co-ION. These high aspect ratio nanowires are approximately 20-100 μm long and 30-50 nm wide. The nanowires intertwine to form a three-dimensional network porous structure, allowing PDMS to fill the pores and achieving a perfect combination. As can be seen, compared to Co-ION aerogel, the three-dimensional network structure of the Co-ION composite filled with PDMS remains unchanged, preserving the original aerogel's skeletal structure, thus demonstrating the effectiveness of the method.
[0094] The Co-ION / PDMS composite exhibits controllable thermochromic properties. Unless otherwise stated, all composite slices mentioned below are 1.5 mm thick. The prepared sheet-like composites are light pink at room temperature. Figure 7 When heated to 50°C on a hot plate, the composite material initially changes color to light blue, continuing until the temperature reaches 60°C, at which point the transformation is complete. Upon further heating to 120°C, the blue color gradually deepens. Similar thermochromic effects were observed in other shapes of composite materials when heated on a hot plate at 60°C. Figure 8 Based on our previous research, we believe that the thermochromic behavior may be due to the reversible adsorption of weakly coordinated water molecules present in the original Co-ION aerogel. Since the porous structure of the aerogel is highly conducive to the adsorption and desorption of water molecules, its color change rate also depends on the ambient humidity. Experiments show that after heating the Co-ION aerogel to 60°C on a hot plate, the aerogel turns blue. It only begins to fade after the aerogel is suspended in the air for approximately 10 seconds. Figure 9 (ac), while under the same conditions, if the aerogel is placed directly into water at a temperature of 60°C, the aerogel will quickly fade in just 2 seconds. Figure 9 This demonstrates that humidity affects the rate of color change in aerogels. Similarly, compared to aerogels, the PDMS-composite material exhibits a much slower color transition because the internal pores are filled with PDMS, blocking the adsorption and desorption channels for water molecules. Experiments show that preheating the aerogel and composite to 60°C to turn them blue, and then quickly immersing them in 60°C water, easily reveals that the aerogel still fades rapidly within 2 seconds, while the composite remains blue. Figure 10This further demonstrates that PDMS in the composite prevents water molecules from being adsorbed and desorbed from the porous structure of the aerogel. Due to the limited channels for water molecule adsorption and desorption, the composite requires immersion for up to 2 minutes in 60°C water to completely decolorize. Figure 11 Interestingly, as the concentration of Co-ION aerogel used decreased, the blue color exhibited by Co / P-25mM was lighter than that of Co / P-75mM. Figure 12 Furthermore, ultraviolet-visible spectroscopy also confirmed these phenomena. These results indicate that the complex exhibits thermochromic behavior characterized by water molecule-induced fading.
[0095] UV-Vis spectrum of the complex at room temperature Figure 13 a) Shows three absorption bands at 500, 530, and 624 nm, corresponding to 4TT. 1g (F)→4T 1g (P), 4T 1g (F)→4A 2g (P) and 4T 1g (F)→4A 2g The electronic transition of (F) is the Co transition in octahedral coordination geometry. 2+ The characteristics of the complex are as follows: Absorption bands are clearly observed at 540, 586, and 635 nm as the temperature of the complex increases to 120 °C. Figure 13 a) Corresponding to Co in tetrahedral geometry 2+ 4A 2g (F)→4T1(P) transition (ν3 band). The higher the temperature of the complex, the higher the absorption peak intensity, and... Figure 7 The varying shades of blue in the Co / P-25mM complex correspond to this phenomenon. Furthermore, at 120°C, the absorption peak of the Co / P-25mM complex in the 550nm-650nm range is lower than that of the Co / P-75mM complex. Figure 13 b), which is related to Figure 12 The depths of the complexes are consistent. Correspondingly, from... Figure 14 As can be seen, the Co / P-75mM complex (23.9au) exhibits a wider fluorescence intensity absorption range compared to the Co / P-25mM complex (19.1au). This may be due to the increased concentration of Co-ION aerogel, which leads to a greater concentration of Co in the Co-ION / PDMS complex. 2+ The concentration of Co is constantly increasing, leading to more Co. 2+ The ligands participate in the dynamic transition between octahedral and tetrahedral coordination during heating and cooling.
[0096] Figure 8 The images shown are of the Co-ION / PDMS composite at 25°C (powder) and 120°C (blue). Figure 8As shown in ab, the Co-ION / PDMS composite, when cut into triangular prisms and cuboids, retains its thermochromic properties. At 120℃, the composite turns deep blue, as... Figure 8 As shown in CD, large-sized aerogel sheets retain good thermochromic properties when laid flat and bent. Figure 8 As shown in Figure e, the Co-ION / PDMS composite, cut into strips and fabricated into a woven structure, still exhibits good thermochromic properties. This demonstrates that the Co-ION / PDMS composite possesses excellent flexibility, allowing it to be cut into arbitrary shapes while maintaining good thermochromic performance.
[0097] To further verify the flexibility and bendability of the Co-ION / PDMS composite, we conducted uniaxial compression and tensile tests on the Co-ION / PDMS composite, Co-ION aerogel, and pure PDMS, respectively. Cylindrical and dumbbell tensile models were typically used as standard samples for the compression and tensile tests, respectively. Figure 15 At a compressive strain of 50%, the compressive stresses of aerogel and PDMS are only 3.6 kPa and 1851.8 kPa, respectively, and the maximum tensile strains of aerogel and PDMS are 8.5% and 128.6%, respectively. Their maximum tensile stresses are 0.1 MPa and 1.7 MPa, respectively. Figure 16 The compressive and tensile properties of the Co-ION / PDMS composite were significantly improved after the aerogel was combined with PDMS. The compressive stress of the Co / P-75mM composite was 2664.1 kPa, which is more than 740 times that of the aerogel and 1.44 times that of pure PDMS. Figure 16 (a and 16c). Furthermore, the maximum tensile strain of the composite was 189.4%, which is 22 times that of the aerogel and 1.47 times that of pure PDMS, respectively. The maximum tensile stress of the composite was 2.8 MPa, which is 28 times that of the aerogel and approximately 1.65 times that of pure PDMS. Figure 16 (b and 16c). The improved compressive and tensile properties of the Co-ION / PDMS composite may be due to the synergistic effect of the high specific surface area, unique three-dimensional interconnected network, and porous structure of the aerogel combined with the PDMS polymer matrix. The cross-linked nanoribbons inside the aerogel form a large number of contact points with PDMS, resulting in entanglement between the nanoribbons and PDMS, increasing friction and improving the compressive and tensile strength of the composite. It may also be related to the abundant functional groups on the surfaces of PDMS and Co-ION. The strong bonding force between the functional groups makes the aerogel and PDMS more firmly bonded, thereby enhancing the overall strength and greatly improving the mechanical integrity.
[0098] like Figure 17As shown, the inventors also demonstrated the application of the Co / P-75mM Co-ION / PDMS composite in temperature-based colorimetric analysis. The inventors adhered a Co-ION / PDMS composite sheet to the surface of a beaker as a wall coating, and placed a thermometer inside the beaker. From... Figure 15 As can be seen, the Co / P-75mM exhibits a significant color change with temperature. At 90℃, the Co-ION / PDMS complex is dark blue. As the water temperature decreases, the Co-ION / PDMS complex gradually changes from blue to pink. When the water temperature reaches 60℃, the complex appears light blue, and when the water temperature drops to 30℃, it turns pink. In this application scenario, when the complex is blue, it serves as a warning to avoid touching it to prevent burns.
[0099] Due to the thermochromic effect of aerogels and composites, and their near-sky and ocean blue hues, Co-ION aerogels and Co-ION / PDMS composites can serve as functional coating materials for camouflage of aircraft in the sky and warships in the sea. Figure 18 It has excellent camouflage capabilities.
[0100] Furthermore, due to the excellent mechanical properties and hydrophobicity of this composite, and its ability to fade even at relatively high temperatures in aquatic environments, we have successfully demonstrated a model for detecting leaks in certain scenarios in marine engineering and warm-water aquaculture. Figure 19 We used plastic petri dishes as simulations of high-temperature water pipes or hot water tanks for our experiments, placing the composite material beneath the dishes as a color indicator. When the water in the petri dishes was at room temperature, the composite material remained pink. However, when the water in the petri dishes was heated to 60°C or higher, the composite material turned blue, indicating that the water temperature had increased. When an external force caused a leak in the petri dishes, water seeped out and came into contact with the composite material, causing it to fade back to its original pink color, thus providing a warning signal for personnel to repair the leak.
[0101] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the invention by those skilled in the art. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the invention should be included within the scope of protection of the invention.
Claims
1. A method for preparing a thermochromic elastomer, characterized in that, Includes the following steps: S1, after mixing cobalt acetylacetonate, benzoic acid and benzyl alcohol evenly, put them into a container and place them in a reaction vessel, heat and keep warm, and after cooling to room temperature, a wet gel is obtained. S2, Immerse the wet gel in the soaking solution and change the soaking solution at intervals. The soaking solution contains cyclohexane or tert-butanol. S3, by freezing the wet gel into a solid state and then freeze-drying it, a cobalt-based inorganic gel with a three-dimensional network porous structure was obtained. Organic hybrid nanobelt aerogel; S4, prepare polydimethylsiloxane dispersion; S5, the aerogel is immersed in a polydimethylsiloxane dispersion and allowed to stand until the polydimethylsiloxane dispersion fills the three-dimensional network porous structure of the aerogel. Then, it is removed and cured. The ratio of cobalt acetylacetone to polydimethylsiloxane is 1.2–16 mmol: 5–8 g, thus obtaining the cobalt-based inorganic... The thermochromic elastomer is a three-dimensional framework of organic hybrid nanoribbon aerogel, with polydimethylsiloxane filling the pores of the framework.
2. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S1, the molar concentration of cobalt acetylacetone is 12. 160mM; the molar ratio of cobalt acetylacetone to benzoic acid is (0.01~0.3):(0.05~1).
3. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S1, the heating and holding process involves heating to 100-300°C at a heating rate of 2-10°C / min and holding for 5-24 hours.
4. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S2, the soaking time is 5 to 30 days, and the soaking solution is changed every 0.5 to 5 days.
5. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S3, the parameters for freeze-drying are: freezing temperature. 20~ 100℃, air pressure set to 30~100Pa, time 12~96h.
6. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S4, the step of preparing the polydimethylsiloxane dispersion is as follows: the polydimethylsiloxane adhesive and the curing agent are mixed and stirred evenly, then n-hexane is added and stirring is continued to obtain the polydimethylsiloxane dispersion.
7. The method for preparing the thermochromic elastomer according to claim 6, characterized in that, The mass ratio of the polydimethylsiloxane adhesive to the curing agent is 8 to 12:
1.
8. The method for preparing the thermochromic elastomer according to claim 1, characterized in that, In step S5, the settling time is 6 to 48 hours; the curing temperature is 30 to 100°C, and the time is 2 to 12 hours.
9. A thermochromic elastomer prepared by the method of any one of claims 1 to 8, characterized in that, The thermochromic elastomer is cobalt-based inorganic The organic hybrid nanoribbon aerogel forms a three-dimensional framework, with polydimethylsiloxane filling the pores of the three-dimensional framework.