Electrical ageing self-diagnosis of insulating materials and method for their production
By introducing organic small molecule indicators into electrical insulating materials and utilizing the chemical structural changes induced by free radicals during the electrical aging process, the visual detection of the electrical aging region is realized, which solves the problems of low detection efficiency and high cost in the existing technology and provides a fast and accurate method for monitoring electrical aging.
Patent Information
- Application Number
- CN202311344585.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-17
AI Technical Summary
Existing technologies for electrical aging testing of electrical insulation materials suffer from problems such as high labor costs, low testing efficiency, complex equipment, high operational difficulty, and limited applicability, making it difficult to achieve rapid and accurate electrical aging monitoring.
Design an electro-aging self-diagnostic insulating material comprising an organic small molecule indicator and a polymer dielectric matrix. By inducing changes in the chemical structure of the indicator through free radicals generated during the electro-aging process, a color change is caused, thereby enabling visualization of the aging region of the material.
It enables early warning of electrical equipment faults, quickly, accurately, and sensitively detects electrical aging areas, reduces detection costs and complexity, and has a wide range of applications.
Smart Images

Figure BDA0004498497070000121 
Figure BDA0004498497070000131 
Figure HDA0004498497100000011
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrical materials technology, and more specifically, to an electrical aging self-diagnostic insulating material and its preparation method. Background Technology
[0002] Polymers such as silicone rubber, epoxy resin, and polypropylene, and their composites, are widely used in the electrical insulation of power equipment and high-voltage electronic equipment. However, during long-term use, these organic insulating materials inevitably undergo electrical aging or damage under strong electromagnetic environments. This includes surface electrical degradation caused by corona discharge and flashover, and internal electrical damage caused by electrical treeing and partial discharge. If these local electrical degradations are not detected and remedied in time, they can lead to catastrophic breakdown of the equipment insulation, resulting in damage to power equipment or even line outages, causing extremely serious consequences. Currently, for the surface electrical aging and damage of external insulation materials, methods such as visual inspection, infrared thermography, ultraviolet imaging, acoustic wave measurement, and electric field measurement are commonly used for detection. For the internal electrical degradation of internal insulation materials, partial discharge testing or ultrasonic flaw detection is typically used. These methods are all external detection methods, which either require significant manpower or complex equipment or operating procedures, making it difficult to detect insulation material problems promptly and accurately. Furthermore, each of these methods is usually only applicable to specific operating conditions, environments, or insulation materials, resulting in a limited scope of application. If we design a universal self-diagnostic method that can visualize the electrical aging of insulating materials and is applicable to various insulating materials and forms of electrical aging, based on the functionality of the materials themselves, we can overcome a series of drawbacks of the aforementioned external detection methods. This would allow us to quickly, efficiently, and intuitively detect aging problems in insulating materials and effectively avoid the serious consequences caused by catastrophic breakdown of materials.
[0003] Specifically, the online monitoring of electrical aging of insulation materials in power equipment currently usually adopts external testing methods. These methods are only applicable under specific test conditions and each has certain limitations. Visual inspection methods for detecting electrical aging and damage in organic external insulation materials are generally only suitable for observing obvious visible damage, and are difficult to observe well-hidden defects and early-stage electrical degradation. Using electro-optical instruments (such as ultraviolet cameras) to observe corona discharge can detect anomalies in the electric field environment of the insulation material, but this method is easily affected by ambient temperature and humidity, and parameters such as ambient light and observation distance can also interfere with the measurement results. Infrared thermal imaging, a non-contact method for monitoring abnormal temperature rise in lines, is only suitable for insulation defects that can cause significant temperature increases; it is also easily affected by the environment and measurement parameters, and its efficiency is low, making it unsuitable for line surveys. Monitoring methods that measure audible noise caused by partial discharge are easily affected by background noise generated by operating transmission lines and power equipment, and it is difficult to accurately locate the specific location of the noise. Electric field measurement methods that directly connect to external circuits to measure the electric field distribution on the surface of the insulation material to detect defects at the interface require individual inspection of the equipment under test (such as line insulators), resulting in extremely high labor costs, high operational difficulty, and low detection efficiency, making them unsuitable for online real-time monitoring and large-scale line surveys. The partial discharge measurement or ultrasonic testing methods used to address the problems of electrical treeing and partial discharge aging in polymers require the construction of relatively complex testing systems and the analysis or waveform processing of the measured signals, making it difficult to draw accurate conclusions about the size and location of defects.
[0004] Inspired by the biological perception of harmful external stimuli such as heat, pain, and injury, transforming the electrodegradation of insulating materials into visualized risk information is crucial for timely prevention of catastrophic failures of electrical equipment. Currently, in the field of mechanics, a large number of self-reporting materials for mechanical stress have been developed based on the force-induced mechanochemical transduction of mechanophores. Since the electroaging process does not involve mechanical stress overload, it cannot trigger the mechanochemical transduction process to cause color changes or fluorescence changes in the mechanophores. Therefore, these materials are typically used to monitor stress fatigue and mechanical history of materials, but are not suitable for visualizing electrodegradation. Summary of the Invention
[0005] To address the shortcomings of existing external testing methods in online monitoring of electrical aging of insulating materials, such as high labor costs, low testing efficiency, complex equipment, high operational difficulty, and limited applicability, this invention aims to provide an electrical aging self-diagnostic insulating material and its preparation method. This material enables self-diagnosis of electrical aging in general polymer materials. While meeting basic insulation performance requirements, this self-diagnostic insulating material also features the ability to visualize its own electrical aging. This allows for efficient inspection of the insulation aging of electrical equipment using only the naked eye or automated, intelligent optical monitoring equipment (such as drones) to determine the operating status of the insulating material. Furthermore, based on the spontaneous color change of the indicator introduced into the polymer matrix caused by free radicals generated during the electrical aging process, it can quickly, accurately, and sensitively indicate localized electrical aging. Moreover, it is to a certain extent independent of specific indicators, polymer matrices, or electrical aging forms, thus having a wider range of applications.
[0006] This invention provides an electrical aging self-diagnostic insulating material comprising an organic small molecule indicator and a polymer dielectric matrix.
[0007] Preferably, the organic small molecule indicator is selected from one or more of spiropyran or spiropyran derivatives, spiroxazine or spiroxazine derivatives, indole or indole derivatives, and o-phenylenediamine or o-phenylenediamine derivatives.
[0008] Preferably, the organic small molecule indicator is doped in the polymer dielectric matrix at a mass fraction of 0.05 wt.% to 0.5 wt.%.
[0009] Preferably, the polymer dielectric matrix is selected from one or more of silicone rubber, epoxy resin, polyethylene, cross-linked polyethylene, polypropylene, polyurethane, polystyrene, polymethyl methacrylate, polycarbonate, and polyetherimide.
[0010] Preferably, the electro-aging self-diagnostic insulating material further comprises:
[0011] Organic solvents required for synthesis.
[0012] Preferably, the organic solvent is selected from one or more of dichloromethane, trichloromethane, tetrahydrofuran, benzene, toluene, xylene, and acetone.
[0013] This invention also provides a method for preparing an electrical aging self-diagnostic insulating material, comprising the following steps:
[0014] a) Dissolve the small organic molecule indicator in an organic solvent to obtain the first organic solution;
[0015] b) Dissolve the polymer or the component used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution;
[0016] c) Mix the first organic solution and the second organic solution evenly, dry and remove the organic solvent, and directly restore the polymer matrix state or obtain the electro-aging self-diagnostic insulating material through a synthesis reaction.
[0017] Preferably, the drying and removal of organic solvents in step c) specifically involves:
[0018] The mixture was placed in a forced-air drying oven to initially dry the organic solvent, and then placed in a vacuum drying oven at the same temperature as the forced-air drying oven to completely remove the residual organic solvent.
[0019] Preferably, the temperature of the forced-air drying oven is set to 10°C to 30°C less than the boiling point of the organic solvent.
[0020] Preferably, the initial drying time in the blower drying oven is more than 4 hours; the time in the vacuum drying oven is more than 1 hour.
[0021] This invention relates to the field of electrical materials technology, and provides an electro-aging self-diagnostic insulating material and its preparation method. The electro-aging self-diagnostic insulating material comprises an organic small-molecule indicator and a polymer dielectric matrix. The preparation method includes the following steps: a) dissolving the organic small-molecule indicator in an organic solvent to obtain a first organic solution; b) dissolving the polymer or components used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution; c) mixing the first and second organic solutions evenly, drying to remove the organic solvent, and directly restoring the polymer matrix state or obtaining the electro-aging self-diagnostic insulating material through a synthetic reaction. Compared with the prior art, the electro-aging self-diagnostic insulating material provided by this invention spontaneously induces changes in the chemical structure of the organic small-molecule indicator in the matrix through the highly chemically active free radicals generated during the electro-aging process. This results in the appearance of new chromophores in the indicator structure, causing color changes in the aging area that are visible to the naked eye or optical monitoring equipment, thereby achieving early warning of electrical equipment failures.
[0022] Meanwhile, the preparation method provided by this invention is simple, has mild and easy-to-control conditions, and uses readily available and low-cost raw materials, thus having broad application prospects. Attached Figure Description
[0023] Figure 1 The mechanism of action of the self-diagnostic electrical aging insulation material provided in the embodiments of the present invention;
[0024] Figure 2 This describes the color changes of pure samples and self-diagnostic samples before and after corona aging in this invention.
[0025] Figure 3This describes the color changes of pure samples and self-diagnostic samples before and after electrical resin aging in this invention. Detailed Implementation
[0026] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] This invention provides an electrical aging self-diagnostic insulating material comprising an organic small molecule indicator and a polymer dielectric matrix.
[0028] See Figure 1 As shown, Figure 1 The mechanism of action of the electro-aging self-diagnostic insulating material provided in the embodiments of the present invention (taking spiroxazine indicator as an example); wherein, (a) is the original electro-aging self-diagnostic insulating material, which includes an organic small molecule indicator and a polymer dielectric matrix; (b) is the process of the insulating material undergoing electro-degradation, generating free radicals and inducing structural changes in the indicator; (c) is the self-diagnostic insulating material after aging and discoloration, in which chromophores appear in the activated indicator.
[0029] In this invention, the design principle of the electro-aging self-diagnostic insulation material is to utilize the free radicals generated during the electro-degradation process of the insulation material itself to induce a chemical change in the organic small molecule indicator that has been pre-incorporated into the polymer dielectric matrix, thereby generating new chromophores in the chemical structure of the indicator and causing a color change in the aging area of the insulation material. Therefore, as long as the core color development mechanism remains unchanged, and only other organic small molecule indicators or polymer dielectric matrices are replaced, it should be considered an alternative to this solution.
[0030] In this invention, the organic small molecule indicator is preferably selected from one or more of spiropyran or spiropyran derivatives, spiroxazine or spiroxazine derivatives, indole or indole derivatives, and o-phenylenediamine or o-phenylenediamine derivatives, more preferably spiroxazine or spiroxazine derivatives. The organic small molecule indicator selected in this invention satisfies the following three conditions: (1) it can chemically react with free radicals or free radical initiators; (2) the reaction can cause a change in the chemical structure of the indicator molecule; and (3) the chemical structure of the reaction product contains a chromophore and has a strong absorption intensity in the visible light region. This invention does not impose any special restrictions on the source of the organic small molecule indicator; commercially available products well known to those skilled in the art can be used.
[0031] In this invention, the mass fraction of the organic small molecule indicator doped in the polymer dielectric matrix is preferably 0.05 wt.% to 0.5 wt.%, more preferably 0.08 wt.% to 0.12 wt.%, with a typical value of 0.1 wt.%. Too little indicator will result in poor visualization of electro-aging, i.e., poor color change in the aging area; too much indicator will cause uneven dispersion in the polymer, thereby adversely affecting the performance of the polymer matrix.
[0032] In this invention, the polymer dielectric matrix is preferably selected from one or more of silicone rubber, epoxy resin, polyethylene, cross-linked polyethylene, polypropylene, polyurethane, polystyrene, polymethyl methacrylate, polycarbonate, and polyetherimide, and more preferably silicone rubber, epoxy resin, or polypropylene. This invention does not impose any special restrictions on the source of the polymer dielectric matrix; commercially available or self-made polymer dielectric materials well-known to those skilled in the art can be used. This invention selects a suitable polymer matrix according to actual needs, and the electro-aging self-diagnostic insulating material provided by this invention will not cause significant harmful effects on the thermal, mechanical, or electrical properties of the polymer dielectric matrix.
[0033] In this invention, the electro-aging self-diagnostic insulating material, in addition to containing the above-mentioned organic small molecule indicator and polymer dielectric matrix as synthetic raw materials or components, preferably also contains:
[0034] Organic solvents required for synthesis.
[0035] In this invention, the organic solvent is preferably selected from one or more of dichloromethane, trichloromethane, tetrahydrofuran, benzene, toluene, xylene, and acetone, more preferably dichloromethane, xylene, or acetone. This invention does not impose any particular limitation on the source of the organic solvent; commercially available products well-known to those skilled in the art can be used. This invention uses an organic solvent with a low boiling point and weak polarity to uniformly disperse the indicator into the polymer matrix, and then thoroughly removes the added organic solvent by heating and depressurizing evaporation to restore the polymer's morphology and properties.
[0036] In this invention, the solvent used satisfies the following three conditions: (1) the selected small organic molecule indicator has high solubility in the solvent; (2) the selected polymer matrix or one of its components has high solubility in the solvent; (3) the solvent has a low boiling point (if multiple solvents meet the first two conditions, a solvent with a lower boiling point should be preferred) so that it can be efficiently and thoroughly removed in subsequent steps.
[0037] This invention also provides a method for preparing an electrical aging self-diagnostic insulating material, comprising the following steps:
[0038] a) Dissolve the small organic molecule indicator in an organic solvent to obtain the first organic solution;
[0039] b) Dissolve the polymer or the component used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution;
[0040] c) Mix the first organic solution and the second organic solution evenly, dry and remove the organic solvent, and directly restore the polymer matrix state or obtain the electro-aging self-diagnostic insulating material through a synthesis reaction.
[0041] This invention first dissolves an organic small molecule indicator in an organic solvent to obtain a first organic solution; then, it dissolves a polymer or a component used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution. In this invention, the organic small molecule indicator and organic solvent are the same as those in the above-described technical solutions and will not be repeated here; the polymer or the component used to prepare the polymer is either a polymer capable of obtaining a polymer dielectric matrix or a source component for synthesizing a polymer dielectric matrix, and can be defined using the same limitations as described in the above-described technical solutions, and will not be repeated here.
[0042] This invention dissolves an organic small molecule indicator in an organic solvent, and prepares an organic solution by thorough stirring. The mass of the added indicator is calculated by multiplying the total mass of the planned polymer preparation by the expected mass fraction of the indicator. The total amount of organic solvent used must ensure that the indicator is completely dissolved; this invention does not have any special limitations in this regard.
[0043] In this invention, a polymer or a component used to prepare the polymer is dissolved in the same organic solvent as in step a). The total amount of organic solvent used should be sufficient to ensure that the polymer or polymer component is fully dissolved. For some polymer matrices (such as polyolefins), a period of heating and stirring is required to accelerate the process; however, this invention does not have any particular limitations in this regard.
[0044] Subsequently, the present invention mixes the first organic solution and the second organic solution evenly, dries and removes the organic solvent, and directly restores the polymer matrix state or obtains an electro-aging self-diagnostic insulating material through a synthesis reaction.
[0045] In this invention, the mixing process is preferably carried out in an open container, and the mixture is thoroughly stirred to ensure that the components are mixed evenly.
[0046] In this invention, the process of drying and removing the organic solvent is preferably specifically as follows:
[0047] The mixture was placed in a forced-air drying oven to initially dry the organic solvent, and then placed in a vacuum drying oven at the same temperature as the forced-air drying oven to completely remove the residual organic solvent.
[0048] In this invention, the temperature of the blower drying oven can be flexibly set according to the boiling point of the organic solvent, preferably set to 10°C to 30°C less than the boiling point of the organic solvent.
[0049] In this invention, the initial drying time in the blower drying oven is preferably 4 hours or more; the time in the vacuum drying oven is preferably 1 hour or more.
[0050] Finally, after thoroughly removing residual organic solvents, the present invention directly restores the polymer matrix state or obtains an electro-aging self-diagnostic insulating material through a synthesis reaction.
[0051] In this invention, the direct restoration of the polymer matrix state can completely restore the morphology and properties of the polymer matrix; the synthesis of the electro-aging self-diagnostic insulating material through a synthetic reaction, i.e., according to a certain synthesis method of pure polymer, should not destroy the activity of the indicator. In a preferred embodiment of this invention, the synthesis method of the provided electro-aging self-diagnostic material includes variations in the experimental temperature range and time; for example, the curing temperature of liquid vulcanized silicone rubber can be 20℃~120℃, and the curing time is usually 20min~48h; the curing temperature of epoxy resin can be 60℃~100℃, and the curing time is usually 4h~12h; this invention does not have any special limitations in this regard, and can be limited by technical solutions and corresponding conditions and parameters well known to those skilled in the art for synthesizing polymer matrices.
[0052] The preparation method provided by this invention is simple, with mild and easily controllable conditions, readily available raw materials, and low cost, and has broad application prospects.
[0053] Compared with the prior art, the beneficial effects of the electro-aging self-diagnostic insulating material and its preparation method provided by the present invention are as follows:
[0054] This invention provides a novel self-diagnostic insulating material for electrical aging, enabling online monitoring of the electrical aging of insulating materials. By generating highly chemically active free radicals during the electrical aging process, the free radicals spontaneously induce changes in the chemical structure of small organic molecules in the matrix, resulting in the appearance of new chromophores in the indicator structure. This causes color changes in the aging area that can be identified by the naked eye or optical monitoring equipment, thereby achieving early warning of electrical equipment failures.
[0055] The self-diagnostic material technology provided by this invention is not limited to a single organic small molecule indicator; different indicators have different chemical activities in reacting with free radicals. For example, spiroxazine is more reactive than indole. The sensitivity of the indicator's color change can be flexibly adjusted according to the actual needs of aging damage diagnosis, thereby achieving more accurate color indication of electrical aging; different indicators also present different colors after color change. For example, spiroxazine turns golden yellow after color change, while indole turns dark red after color change. The warning color can be flexibly adjusted according to the surrounding environment to achieve the best indication effect.
[0056] The self-diagnostic material technology provided by this invention is not limited to a certain polymer matrix; thermosetting epoxy resin, plexiglass, silicone rubber and other insulating polymers, as well as thermoplastic polyethylene, polypropylene, polystyrene and other organic dielectric materials can all achieve the self-diagnostic function of electrical aging damage after activation by an indicator. Therefore, a suitable polymer matrix can be flexibly selected according to the actual insulation requirements of electrical equipment.
[0057] The self-diagnostic material technology solution provided by this invention is not limited to identifying a certain form of electrical aging; surface electrical degradation caused by corona discharge, flashover discharge, etc., and internal electrical damage caused by electrical tree discharge, partial discharge, etc., can all produce color responses that are recognizable to the naked eye.
[0058] The self-diagnostic material technology solution provided by this invention can provide a rapid and accurate color response to localized electro-aging areas of insulating materials. This invention is based on free radical reactions for spontaneous color indication, so the material can quickly produce color changes after electro-aging (obvious color changes can be observed a few seconds after the free radicals react with the indicator, which is much faster than the time scale of material aging). There is a strong positive correlation between the degree of color change and the degree of material electro-aging, and the range of color change is also highly consistent with the range of electro-aging.
[0059] The self-diagnostic material technology solution provided by this invention has low equipment and labor costs, simple material preparation method, and accurate, intuitive and reliable aging self-diagnosis effect. It does not require complex and expensive external equipment, cumbersome operating procedures and maintenance processes, or post-data processing and analysis. It only requires the synthesis of corresponding self-diagnostic materials according to the actual scenario, and the color change can be observed with the naked eye or the color change signal can be identified autonomously using optical equipment, which is convenient to operate and use.
[0060] This invention relates to the field of electrical materials technology, and provides an electro-aging self-diagnostic insulating material and its preparation method. The electro-aging self-diagnostic insulating material comprises an organic small-molecule indicator and a polymer dielectric matrix. The preparation method includes the following steps: a) dissolving the organic small-molecule indicator in an organic solvent to obtain a first organic solution; b) dissolving the polymer or components used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution; c) mixing the first and second organic solutions evenly, drying to remove the organic solvent, and directly restoring the polymer matrix state or obtaining the electro-aging self-diagnostic insulating material through a synthetic reaction. Compared with the prior art, the electro-aging self-diagnostic insulating material provided by this invention spontaneously induces changes in the chemical structure of the organic small-molecule indicator in the matrix through the highly chemically active free radicals generated during the electro-aging process. This results in the appearance of new chromophores in the indicator structure, causing color changes in the aging area that are visible to the naked eye or optical monitoring equipment, thereby achieving early warning of electrical equipment failures.
[0061] Meanwhile, the preparation method provided by this invention is simple, has mild and easy-to-control conditions, and uses readily available and low-cost raw materials, thus having broad application prospects.
[0062] To further illustrate the present invention, the following embodiments will be described in detail.
[0063] Example 1: Spiroxazine-Silicone Rubber Electrical Aging Self-Diagnostic Insulating Material
[0064] (1) Dow Corning Sylgard 182 or Sylgard 184 silicone elastomers are selected as the matrix of the self-diagnostic insulating material for electrical aging. Sylgard 182 / 184 is a two-component addition curing system. Its curing principle is that the vinyl-terminated polydimethylsiloxane monomer undergoes a platinum-catalyzed hydrosilylation reaction with the hydrogen-silicon bond to form a network cross-linked structure. At room temperature, both the matrix (component A) and the curing agent (component B) are liquid. After mixing component A and component B at a mass ratio of 10:1 and degassing, the mixture is poured into a designated mold and heated in a 60°C forced-air oven for more than 4 hours to obtain a colorless and transparent silicone elastomer.
[0065] A specific example method for preparing electrically aging self-diagnostic insulating materials is as follows:
[0066] First, dissolve 11 mg (0.1 wt.%) of spiroxazine indicator (CAS: 27333-47-7) in 1 mL of dichloromethane. The typical ratio of solvent to matrix material is 1 mL: 10 g. Then add 10 g of matrix (component A) and stir until homogeneous. Place the above solution in a 60°C forced-air oven for more than 4 hours to preliminarily evaporate the solvent, and then place it in a 60°C vacuum drying oven for more than 1 hour to completely remove the dichloromethane solvent from the mixture. Then add 1 g of curing agent (component B) to the above mixture and stir thoroughly. After vacuum degassing at room temperature, pour the mixture into a designated mold. Place the mold in a 60°C forced-air oven for more than 4 hours to obtain the spiroxazine-silicone rubber electro-aging self-diagnostic insulating material.
[0067] After sample preparation, the electrical and mechanical properties of the pure sample and the self-diagnostic sample were measured to verify that the synthesis process of the self-diagnostic sample did not affect the material properties.
[0068] Electrical breakdown field strength tests were performed at room temperature according to IEC 60243-2:2001. The specimen and the double-sphere electrode were immersed in silicone oil to prevent surface flashover. A sinusoidal AC voltage was applied to the specimen, and the sample thickness and breakdown voltage were recorded to calculate the electric field strength. Each group of samples was measured 20 times, and the characteristic breakdown field strength was calculated using Weibull methods.
[0069] The relative permittivity and breakdown voltage at power frequency were measured and calculated using a broadband dielectric spectrometer (Concept 80, Novocontrol, Germany) with an applied voltage of 1V and ambient temperature and pressure during measurement.
[0070] The volume resistivity was measured using the three-electrode method recommended in GB / T 1410-2006, where the applied electric field was 10 kV / mm and the diameter of the protected electrode was 20 mm.
[0071] Tensile strength and elongation at break were measured using a tensile testing machine in accordance with GB / T 528-2008 standard.
[0072] The mechanical and insulating properties of this spiroxazine-silicone rubber electro-aging self-diagnostic insulating material were tested and are shown in Table 1. The material can achieve rapid and accurate visualization of the electro-aging region (see Table 1). Figures 2-3 ).
[0073] (2) The Gelest addition polymerization silicone system was selected as the matrix of the self-diagnostic insulating material for electrical aging. Gelest silicone rubber is also an addition curing system, with the same curing mechanism as Sylgard 184. Vinyl-terminated DMS-V31 (CAS:68083-19-2) was selected as the matrix reagent, HMS-301 (CAS:68037-59-2) containing hydrogen-silicon bonds was selected as the crosslinking agent, and SIP6830.3 (CAS:68478-92-2) containing platinum was selected as the catalyst. 200 ppm of SIP6830.3 was added to 30 parts by weight of DMS-V31, and then 1 part by weight of HMS-301 was added. After mixing evenly, the mixture was degassed and cured at 60°C for more than 4 hours to obtain a colorless and transparent pure silicone elastomer.
[0074] A specific example method for preparing electrically aging self-diagnostic insulating materials is as follows:
[0075] First, dissolve 31 mg (0.1 wt.%) of spiroxazine in 3 mL of dichloromethane, then add 30 g of DMS-V31 and stir until homogeneous. Place the above solution in a 60°C forced-air oven for more than 4 hours to preliminarily evaporate the solvent, and then place it in a 60°C vacuum drying oven for more than 1 hour to completely remove the dichloromethane solvent from the mixture. Then add 1 g of HMS-301 crosslinking agent to the above mixture, stir thoroughly, and let the mixture stand to room temperature. Then add 10 μL of LSP6830.3 catalyst and stir until homogeneous. After vacuum degassing at room temperature, pour the mixture into a designated mold. Place the mold in a 60°C forced-air oven and heat for more than 4 hours to obtain the spiroxazine-silicone rubber electro-aging self-diagnostic insulating material.
[0076] The mechanical and insulating properties of the spiroxazine-silicone rubber electro-aging self-diagnostic insulating material were tested and are shown in Table 1; the material can achieve rapid and accurate visualization of the electro-aging area.
[0077] (3) The Gelest condensation polymerization organosilicon system was selected as the matrix of the self-diagnostic insulating material for electrical aging. This Gelest silicone rubber is a condensation curing silanol system. Its curing mechanism is that the polydimethylsiloxane monomer with silanol end caps undergoes a tin-catalyzed condensation reaction with the alkoxy crosslinking agent to form a crosslinked network structure. The silanol end cap DMS-S35 (CAS:70131-67-8) can be used as the matrix, the alkoxy functional group-containing PSI-021 (CAS:68412-37-3) can be used as the crosslinking agent, and the tin-containing SND3260 (CAS:77-58-7) can be used as the catalyst. 10 parts by weight of DMS-S35 and 1 part by weight of PSI-021 are mixed, and then 0.2 wt.% of SND3260 is added. After stirring evenly, the mixture is degassed and cured at 60°C for more than 4 hours to obtain a colorless and transparent pure silicone elastomer.
[0078] A specific example method for preparing electrically aging self-diagnostic insulating materials is as follows:
[0079] First, dissolve 11 mg (0.1 wt.%) of spiroxazine indicator in 1 mL of dichloromethane, then add 10 g of DMS-S35 and stir until homogeneous. Place the above solution in a 60°C forced-air oven for more than 4 hours to preliminarily evaporate the solvent, and then place it in a 60°C vacuum drying oven for more than 1 hour to completely remove the dichloromethane solvent from the mixture. Then add 1 g of PSI-021 crosslinking agent to the above mixture, stir thoroughly, and let the mixture stand to room temperature. Then add 20 μL of SND3260 catalyst and stir until homogeneous. After vacuum degassing at room temperature, pour the mixture into a designated mold. Place the mold in a 60°C forced-air oven and heat for more than 4 hours to obtain the spiroxazine-silicone rubber electro-aging self-diagnostic insulating material.
[0080] The mechanical and insulating properties of the spiroxazine-silicone rubber electro-aging self-diagnostic insulating material were tested and are shown in Table 1; the material can achieve rapid and accurate visualization of the electro-aging area.
[0081] Example 2: Spiroxazine-Epoxy Resin Electrical Aging Self-Diagnostic Insulating Material
[0082] Bisphenol A liquid epoxy resin EPON was selected. TM Resin 828 (EP828) was used as the matrix reagent to prepare solid epoxy resin polymers. Diethylenetriamine, accounting for 12 wt.% of the matrix reagent, was used as a curing agent to crosslink EP828, thereby forming a network structure with good mechanical and insulating properties. After the matrix and curing agent were thoroughly mixed, they were degassed at room temperature, and then the mixture was poured into a designated mold to prepare pure epoxy resin samples for testing. It should be noted that the curing reaction is highly exothermic, so the temperature of the mixture must be strictly controlled during operation to prevent premature curing or burns.
[0083] A specific example method for preparing electrically aging self-diagnostic insulating materials is as follows:
[0084] First, dissolve 11 mg (0.1 wt.%) of spiroxazine in 1 mL of acetone, with a typical solvent-to-matrix material ratio of 1 mL:10 g. Then, add 10 g of EP828 matrix reagent, stir thoroughly, and place in a 60°C forced-air oven for at least 6 hours to initially remove the acetone solvent. Then, place in a 60°C vacuum drying oven for at least 1 hour to completely remove residual solvent. After removing the mixture and cooling it to room temperature, add 1.2 g of diethylenetriamine and stir thoroughly to degas. Then, quickly pour the mixture into a designated mold, paying close attention to the temperature of the mixture during this process and taking precautions against burns. Place the mold in a 60°C forced-air oven and heat for at least 4 hours to obtain the spiroxazine-epoxy resin electro-aging self-diagnostic insulating material.
[0085] After sample preparation, the electrical and mechanical properties of the pure sample and the self-diagnostic sample were measured to verify that the synthesis process of the self-diagnostic sample did not affect the material properties. The electrical properties were tested using the same method as in Example 1, and the mechanical properties were measured according to the GB13022-1991 standard.
[0086] The mechanical and insulating properties of the spiroxazine-epoxy resin electro-aging self-diagnostic insulating material were tested and are shown in Table 1; the material can achieve rapid and accurate visualization of the electro-aging area.
[0087] Example 3: Spiroxazine-polypropylene electro-aging self-diagnostic insulation material
[0088] Macklin polypropylene (PP) granules (MW: 42.08, melt index: 0.5 g / 10 min) were selected as the matrix for the electro-aging self-diagnostic insulation material; pure PP samples were prepared by hot pressing the granules in a designated mold at 200°C.
[0089] A specific example method for preparing electrically aging self-diagnostic insulating materials is as follows:
[0090] First, add 10g of PP granules to 200mL Stir thoroughly in hot xylene at 120℃ until PP is completely dissolved (the ratio of PP to xylene is usually 1g:20mL); then take another 1mL of xylene and add 10mg (0.1wt.%) of spiroxazine to prepare a solution, and then add it to the above hot PP-xylene solution. Stir continuously at 120℃ for 10 minutes to mix evenly; then pour the above solution into a large petri dish while it is still hot, and quickly put it into a 100℃ forced-air oven to dry for more than 12 hours to initially remove the organic solvent. Then put the sample into a 100℃ vacuum drying oven for more than 1 hour to completely remove the residual xylene solvent. The PP-based composite material obtained can be used to make various PP-based self-diagnostic samples according to the hot pressing method of pure PP; that is, first put a sufficient amount of the above PP-based composite material into a mold, preheat it to 200℃ until it melts, then hot press it at 10MPa pressure and 200℃ temperature for 5min, and then cold press it at 5MPa pressure and 20℃ temperature for 5min to form the self-diagnostic sample in the mold.
[0091] After sample preparation, the electrical and mechanical properties of the pure sample and the self-diagnostic sample were measured to verify that the synthesis process of the self-diagnostic sample did not affect the material properties. The testing method for electrical properties was the same as in Example 2.
[0092] The mechanical and insulation properties of the spiroxazine-polypropylene electro-aging self-diagnostic insulation material were tested and are shown in Table 1; the material can achieve rapid and accurate visualization of the electro-aging area.
[0093] Table 1. Test results of electrical and mechanical properties of various dielectric materials synthesized in Examples 1-3.
[0094]
[0095]
[0096] In summary, this invention synthesizes an electro-aging self-diagnostic insulating material. It utilizes the free radicals generated during the electro-aging of the matrix itself to induce color changes in an organic small-molecule indicator, thereby visualizing the electro-aging regions of the insulating material. The self-diagnostic scheme provided by this invention can flexibly change the types of indicator and polymer insulating material according to actual application needs, and can provide color indication for various aging forms such as electrical treeing and corona aging. Moreover, the introduction of the organic small-molecule indicator does not adversely affect the basic properties of the polymer material. Compared with aging methods for insulating materials, the self-diagnostic technology for insulating materials has the advantages of low equipment and labor costs, simple material preparation methods, and accurate, intuitive, and reliable self-diagnostic results. The feasibility of this invention has been demonstrated through the above experiments and tests, achieving rapid and accurate visualization of the electro-aging regions of the material without affecting the mechanical and insulating properties of the matrix itself.
[0097] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A self-diagnostic insulating material for electrical aging, characterized in that, It contains organic small molecule indicators and a polymer dielectric matrix; The electro-aging self-diagnostic insulating material spontaneously induces changes in the chemical structure of organic small molecule indicators in the matrix by free radicals generated during the electrical aging process, resulting in the appearance of new chromophores in the indicator structure and causing color changes in the aging area that can be identified by the naked eye or optical monitoring equipment. The organic small molecule indicator is selected from one or more of spiropyran or spiropyran derivatives, spiroxazine or spiroxazine derivatives, indole or indole derivatives, and o-phenylenediamine or o-phenylenediamine derivatives. The organic small molecule indicator is doped in the polymer dielectric matrix at a mass fraction of 0.05 wt.% to 0.5 wt.%.
2. The self-diagnostic insulating material for electrical aging according to claim 1, characterized in that, The polymer dielectric matrix is selected from one or more of silicone rubber, epoxy resin, polyethylene, polypropylene, polyurethane, polystyrene, polymethyl methacrylate, polycarbonate, and polyetherimide.
3. The self-diagnostic electrical aging insulating material according to claim 1 or 2, characterized in that, The electro-aging self-diagnostic insulating material also includes: Organic solvents required for synthesis.
4. The self-diagnostic insulating material for electrical aging according to claim 3, characterized in that, The organic solvent is selected from one or more of dichloromethane, trichloromethane, tetrahydrofuran, benzene, toluene, xylene, and acetone.
5. A method for preparing the electro-aging self-diagnostic insulating material according to claim 1, characterized in that, Includes the following steps: a) Dissolve the small organic molecule indicator in an organic solvent to obtain the first organic solution; b) Dissolve the polymer or the component used to prepare the polymer in the same organic solvent as in step a) to obtain a second organic solution; c) Mix the first organic solution and the second organic solution evenly, dry and remove the organic solvent, and directly restore the polymer matrix state or obtain the electro-aging self-diagnostic insulating material through a synthesis reaction.
6. The preparation method according to claim 5, characterized in that, The process of drying and removing organic solvents described in step c) is specifically as follows: The mixture was placed in a forced-air drying oven to initially dry the organic solvent, and then placed in a vacuum drying oven at the same temperature as the forced-air drying oven to completely remove the residual organic solvent.
7. The preparation method according to claim 6, characterized in that, The temperature of the blower drying oven is set to 10°C to 30°C less than the boiling point of the organic solvent.
8. The preparation method according to claim 6, characterized in that, The initial drying time in the blower drying oven is more than 4 hours; the time in the vacuum drying oven is more than 1 hour.
Citation Information
Patent Citations
Method for indicating aging degree of room temperature vulcanized silicone rubber
CN115524280A